Strain sensor preparation method based on conductive ink and strain sensor
Through the strain sensor preparation method based on conductive ink, the interwoven network structure of carbon nanotubes and graphene is used to solve the problems of long response time and narrow frequency band of traditional metal strain gauge, effectively monitoring of high-frequency signals is achieved, and sensors are improved sensitivity and stability.
Patent Information
- Application Number
- CN202411205271.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
AI Technical Summary
The response time of traditional metal strain gauge is long, which is difficult to meet the rapidly changing strain monitoring needs, and the monitoring frequency band is narrow, making it impossible to effectively capture high-frequency dynamic strain signals.
Using the strain sensor preparation method based on conductive ink, by fine grinding carbon nanotubes and graphene with resin and solvent, a uniformly dispersed conductive ink is formed, and a conductive structure is formed on the substrate surface through screen printing technology, combined with the packaging material. Package, build interleaved network structures to improve sensor sensitivity and stability.
It has achieved the improvement of strain monitoring capabilities for ultra-high frequency signals, increased the sensitivity of the sensor and reliability and stability in complex stress environments, and met the requirements of high-precision, high-speed response and extensive frequency band monitoring in the field of structural health monitoring. .
Smart Images

Figure CN119081477A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of sensor technology, and in particular to a method for preparing a strain sensor based on conductive ink and a strain sensor. Background Art
[0002] Strain sensors are key tools for detecting deformation of materials or structures and are widely used in aerospace, civil engineering, machinery manufacturing and other fields. In these fields, structural health monitoring and damage detection are crucial, and strain sensors have become indispensable equipment because of their ability to detect tiny deformations in real time. Traditional strain sensors mainly use metal strain gauges, which are usually made of highly sensitive metal materials such as platinum, nickel-chromium alloys, etc. The basic working principle of metal strain gauges is based on the resistance strain effect of metals: when the strain gauge is stretched or compressed, its resistance will change, and the strain can be calculated by measuring the change in resistance.
[0003] Metal strain gauges are widely used due to their excellent resistance strain effect, good linearity and temperature stability. Applications include aerospace composite structure monitoring, bridge stress monitoring, building health monitoring, and mechanical equipment status monitoring. These strain gauges show good long-term stability and repeatability in strain detection. They have a simple structure, a clear working principle, and can maintain reliable operation in harsh environments.
[0004] However, despite the many advantages of metal strain gauges, due to material and design limitations, metal strain gauges have a long response time and are difficult to meet the needs of rapidly changing strain monitoring. In addition, the monitoring frequency band of traditional metal strain gauges is narrow and cannot effectively capture high-frequency dynamic strain signals. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a strain sensor based on conductive ink and a strain sensor, so as to improve the strain monitoring capability of the sensor for ultra-high frequency signals, increase the sensitivity of the sensor, and increase the reliability and stability in complex stress environments.
[0006] In order to achieve the above object, the embodiment of the present invention discloses the following technical solution:
[0007] On the one hand, a method for preparing a strain sensor based on conductive ink is provided, comprising the following steps:
[0008] Grinding the designed amount of carbon nanotubes, graphene mixture, resin and solvent to obtain uniformly dispersed conductive ink;
[0009] The conductive ink is screen-printed onto the surface of the substrate according to a preset pattern, and heated and cured at a temperature of 120° C. to 130° C. for 3 min to 5 min to form a conductive structure;
[0010] The strain sensor is manufactured by packaging the substrate and the conductive structure on the substrate after curing using a packaging material;
[0011] The step of grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain uniformly dispersed conductive ink includes, in sequence, an initial mixing stage, a rough grinding stage, a fine grinding stage and a precise grinding stage.
[0012] In addition to or as an alternative to one or more of the features disclosed above, the primary mixing stage comprises the following steps:
[0013] Mixing carbon nanotubes and graphene with resin and solvent according to designed amounts;
[0014] Preliminary dispersion by magnetic stirring or ultrasonic oscillation ensures that the carbon nanotubes and graphene are evenly distributed in the solvent;
[0015] The gap between the rollers of the three-roll mill was set to 100-120 μm to ensure that there would be no excessive loss of material or clogging during grinding.
[0016] In addition to or as an alternative to one or more of the features disclosed above, the rough grinding stage comprises the following steps:
[0017] Start the grinder, maintain a low roller speed of 30-50r / min, and begin grinding. During the grinding process, continue to observe the state of the material to ensure that the material is evenly distributed;
[0018] The gap between the rollers is gradually reduced to 70-80 μm, ensuring that the material can adapt to the new gap after each adjustment;
[0019] The adjustment distance of each spacing is 10 to 20 μm, and the grinding time after each spacing adjustment is 5 to 10 minutes.
[0020] In addition to or as an alternative to one or more of the features disclosed above, the grinding stage comprises the following steps:
[0021] After the material is initially dispersed evenly, the distance between the rollers is gradually reduced to 50-60 μm, and the roller speed is maintained at 30-50 r / min to prevent the high shear force from causing damage to the carbon nanotubes or graphene sheets;
[0022] The adjustment distance of each spacing is 20 to 30 μm, and the grinding time after each spacing adjustment is 10 to 20 minutes, ensuring that the material can be further dispersed under the new spacing conditions.
[0023] In addition to or as an alternative to one or more of the features disclosed above, the lapping stage comprises the following steps:
[0024] Gradually reduce the gap between the rollers to 15-20μm, keep the roller speed at 20-30r / min, and adjust the gap by 20-30μm each time to avoid excessive grinding and changes in material properties;
[0025] Grind for 20-30 minutes to ensure that the carbon nanotubes and graphene are evenly dispersed in the resin and solvent.
[0026] In addition to or as an alternative to one or more of the features disclosed above, the step of screen printing the conductive ink onto the substrate surface in a predetermined pattern comprises:
[0027] Fixing the screen printing template on the screen printing workbench, and keeping the electrode position on the substrate coincident with the electrode position on the screen printing template;
[0028] The conductive ink is evenly coated on the screen printing template, and a scraper is used to apply uniform pressure to print the ink through the mesh of the screen onto the substrate.
[0029] In addition to or as an alternative to one or more of the features disclosed above, the preset pattern is one or more of a straight line, a bent shape, an S shape, a circuitous shape, and a bow shape; and the substrate is one or more of polyimide, glass, and ceramic.
[0030] In addition to or as an alternative to one or more of the features disclosed above, the packaging material is one or more of imide film, epoxy resin and silicone.
[0031] In addition to or as an alternative to one or more of the features disclosed above, the conductive ink is composed of the following materials by mass percentage:
[0032]
[0033] In addition to one or more of the features disclosed above, or as an alternative, the resin is one or more of a saturated polyester resin, an acrylic resin, and an epoxy resin; the solvent is one or more of DBE, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol ethyl ether acetate, dimethyl adipate, diethyl adipate and N-methylpyrrolidone.
[0034] On the other hand, a strain sensor is further disclosed, which is prepared by the strain sensor preparation method as described in any of the above items. In addition to or instead of one or more of the features disclosed above, the strain sensor includes: a flexible printed circuit substrate, an ink sensing layer and a packaging layer, the flexible printed circuit substrate is provided with a substrate electrode connected on both sides, the ink sensing layer is screen-printed on the flexible printed circuit substrate, and the packaging layer covers the ink sensing layer to encapsulate the ink sensing layer.
[0035] In addition to or instead of one or more of the features disclosed above, the thickness of the flexible printed circuit substrate is 50 μm to 250 μm; the material of the substrate electrode is at least one of silver, aluminum, and copper; the thickness of the substrate electrode is 0.01 mm to 0.04 mm; the substrate electrode is aligned with the electrode position on the screen printing template; one side of the substrate electrode is printed with conductive ink, and the other side is welded with a wire to prepare the positive and negative electrodes of the sensor.
[0036] Compared with the prior art, the present invention has the following beneficial technical effects: in the manufacturing process of the sensor, fine three-roll grinding ensures the uniform dispersion and reasonable arrangement of carbon nanotubes and graphene in the ink, thereby effectively controlling the tunneling distance, which not only stabilizes the tunneling resistance of the sensor, but also improves its strain monitoring capability for ultra-high frequency signals, and the shear force formed during the fine grinding process prompts the carbon nanotubes and graphene to construct an interwoven network structure, which is similar to a bone sponge structure with a high porosity and complex conductive paths, which not only increases the sensitivity of the sensor, but also further enhances its reliability and stability in complex stress environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The technical solutions and other beneficial effects of the present invention will be made apparent by describing in detail the specific embodiments of the present invention in conjunction with the accompanying drawings.
[0038] Figure 1 is an exploded diagram of a strain sensor based on conductive ink provided according to an embodiment of the present invention;
[0039] Figure 2 is a strain-resistance change rate response curve of a strain sensor based on conductive ink provided according to an embodiment of the present invention, wherein the X-axis is strain and the Y-axis is resistance change rate;
[0040] Figure 3 is a time-resistance change rate response curve of a strain sensor based on conductive ink provided according to an embodiment of the present invention, wherein the X-axis is time and the Y-axis is the resistance change rate;
[0041] Figure 4 is a frequency response curve of a strain sensor based on conductive ink provided according to an embodiment of the present invention, wherein the X-axis is the frequency and the Y-axis is the amplitude;
[0042] Figure 5 is a scanning electron microscope image of a strain sensor based on conductive ink provided according to an embodiment of the present invention;
[0043] Figure 63 is a tensile strain-resistance change rate response curve of a strain sensor based on conductive ink provided according to an embodiment of the present invention, wherein the X-axis is strain and the Y-axis is resistance change rate. DETAILED DESCRIPTION
[0044] The technical scheme in the embodiment of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiment of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0045] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the term "and / or" herein is merely a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " herein, unless otherwise specified, generally indicates that the associated objects before and after are in an "or" relationship.
[0046] For descriptive purposes, spatially relative terms such as "below," "beneath," "below," "above," "on," etc. may be used herein to describe the relationship of one element or feature illustrated in the accompanying drawings to another element or feature. Spatially relative terms are intended to cover different orientations of the device when in use, in operation, and / or in manufacture other than the orientation depicted in the accompanying drawings. For example, if the device in the accompanying drawings is turned over, elements described as being "below" or "below" other elements or features will be "above" the other elements or features. Therefore, the exemplary term "below" may include both above and below orientations. Moreover, the device may be oriented in other directions (e.g., rotated 90 degrees or in other orientations), and the spatially relative descriptors used herein are therefore interpreted accordingly.
[0047] In one embodiment of the present invention, a method for preparing a strain sensor based on conductive ink is disclosed, comprising the following steps:
[0048] Step S1, grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain a uniformly dispersed conductive ink;
[0049] Step S2, screen printing the conductive ink onto the surface of the substrate according to a preset pattern, and heating and curing at a temperature of 120° C. to 130° C. for 3 min to 5 min to form a conductive structure;
[0050] Step S3, using a packaging material to package the substrate and the conductive structure that has been cured on the substrate, so as to obtain the strain sensor;
[0051] The step of grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain uniformly dispersed conductive ink includes, in sequence, an initial mixing stage, a rough grinding stage, a fine grinding stage and a precise grinding stage.
[0052] In an embodiment of the present invention, the carbon-based conductive filler in the conductive ink forms a conductive path in the flexible resin through microscopic mutual contact. When the material is subjected to tension / pressure, the distance between adjacent conductive particles inside the material changes, resulting in changes in the conductive path formed by the contact of the conductive particles, causing the resistance of the conductive ink to change on a macroscopic level, so that the conductive ink has a stress-resistance effect.
[0053] The dispersion state of carbon nanotubes (CNT) and graphene (GN) in the ink can be effectively controlled by three-roll grinding. During the fine grinding process, CNT and GN are gradually evenly distributed under the action of shear force and form an interwoven network in the ink, such as Figure 5 shown.
[0054] According to Simons theory, tunneling distance is the direct factor affecting tunneling resistance, and in the manufacturing process of nanosensors, fine three-roll grinding ensures the uniform dispersion of carbon nanotubes (CNT) and graphene (GN) in the ink, thereby effectively controlling the tunneling distance. This not only stabilizes the tunneling resistance of the sensor, but also improves its ability to monitor ultra-high frequency signals. In addition, the shear force formed during the fine grinding process prompts CNT and GN to build an interwoven network structure, which is similar to a bone sponge structure with a high porosity and complex conductive paths, which not only increases the sensitivity of the sensor, but also further enhances its reliability and stability in complex stress environments.
[0055] Furthermore, the initial mixing stage comprises the following steps:
[0056] Step T1, mixing carbon nanotubes and graphene with resin and solvent according to designed amounts;
[0057] Step T2, preliminarily dispersing by magnetic stirring or ultrasonic oscillation to ensure that the carbon nanotubes and graphene are evenly distributed in the solvent;
[0058] Step T3, setting the roller spacing of the three-roll mill to 100-120 μm to ensure that there is no excessive material loss or clogging during grinding. The above steps help to evenly distribute the filler during grinding and improve grinding efficiency.
[0059] Furthermore, the rough grinding stage comprises the following steps:
[0060] Step P1, start the grinder, maintain a relatively low roller speed of 30-50 r / min, start grinding, and continuously observe the material state during the grinding process to ensure that the material is evenly distributed;
[0061] Step P2, gradually reducing the gap between the rollers to 70-80 μm, ensuring that the material can adapt to the new gap after each adjustment;
[0062] The adjustment distance of each spacing is 10 to 20 μm, and the grinding time after each spacing adjustment is 5 to 10 minutes. Through the above steps, it is possible to avoid excessive shear force damaging carbon nanotubes and graphene, and each small adjustment provides time for gradually forming uniform dispersion.
[0063] Furthermore, the fine grinding stage comprises the following steps:
[0064] After the material is initially dispersed evenly, the distance between the rollers is gradually reduced to 50-60 μm, and the roller speed is maintained at 30-50 r / min to prevent the high shear force from causing damage to the carbon nanotubes or graphene sheets;
[0065] The adjustment distance of each spacing is 20 to 30 μm, and the grinding time after each spacing adjustment is 10 to 20 minutes to ensure that the material can be further dispersed under the new spacing conditions. Through the above steps, the material can be further dispersed while avoiding the damage to the carbon nanotubes or graphene sheets due to high shear force. The grinding conditions at this stage help the nanomaterials to be more evenly distributed in the matrix and improve the performance of the sensing material.
[0066] Furthermore, the lapping stage comprises the following steps:
[0067] Gradually reduce the gap between the rollers to 15-20μm, keep the roller speed at 20-30r / min, and adjust the gap by 20-30μm each time to avoid excessive grinding and changes in material properties;
[0068] Grind for 20-30 minutes to ensure that the carbon nanotubes and graphene are evenly dispersed in the resin and solvent. Through the above steps, the ultra-fine and uniform dispersion of carbon nanotubes and graphene can be achieved, ensuring that the conductivity and sensitivity of the sensor material are in the best state. Through this stage of fine grinding, the nanomaterials can be more closely distributed in the matrix to form an ideal microstructure.
[0069] Furthermore, the step of screen printing the conductive ink onto the surface of the substrate according to a preset pattern comprises:
[0070] Step R1, fixing the screen printing template on the screen printing workbench, and keeping the electrode position on the substrate coincident with the electrode position on the screen printing template;
[0071] Step R2, evenly coating the conductive ink on the screen printing template, using a scraper to apply uniform pressure, and printing the ink through the mesh of the screen onto the substrate.
[0072] Furthermore, the preset pattern is one or more of a straight line, a bend, an S-shape, a circuitous shape, and a bow shape; and the substrate is one or more of polyimide, glass, and ceramic. Figure 1 In the illustrated embodiment, the preset pattern is a bow-shaped structure, so that the prepared ink sensing layer 12 also has a bow-shaped structure.
[0073] Furthermore, the packaging material is one or more of imide film, epoxy resin and silica gel.
[0074] Furthermore, the conductive ink is composed of the following materials in percentage by mass:
[0075]
[0076] The sensitive conductive ink provided by the embodiment of the present invention has good flexibility and resilience, and can produce a high mechanical deformation; at the same time, the resistance of the sensitive conductive ink provided by the present invention continuously rises / falls with the increase of the tensile / compressive deformation under the action of tension / pressure, showing a positive / negative resistance-strain effect; in addition, the sensitive conductive ink provided by the present invention has good signal sensitivity and stability, and is particularly suitable as a stress-strain sensing material for a flexible film pressure sensor. In addition, the sensitive conductive ink provided by the present invention has good printability and adhesion.
[0077] In the embodiment of the present invention, carbon nanotubes and graphene are used as conductive fillers, which not only have a good stress-resistance effect, but also can be evenly dispersed in the resin to improve the conductive stability of the sensitive conductive ink; in addition, the preferred conductive fillers are beneficial for the sensitive conductive ink to maintain the flexibility and resilience of the flexible resin.
[0078] Furthermore, the resin is one or more of saturated polyester resin, acrylic resin, and epoxy resin; the solvent is one or more of dibasic acid ester (DBE), diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol ethyl ether acetate, dimethyl adipate, diethyl adipate, and N-methylpyrrolidone. Figure 1 In the embodiment shown, the resin is epoxy resin. In the embodiment of the present invention, the selected resin has excellent flexibility and resilience, which gives the sensitive conductive ink excellent flexibility and resilience, as well as a large range of mechanical quantity changes.
[0079] Reference Figure 1The present invention also discloses a strain sensor, which is prepared by the strain sensor preparation method as described in any one of the above items, and the strain sensor includes: a flexible printed circuit substrate 13, an ink sensing layer 12 and a packaging layer 11, the flexible printed circuit substrate 13 is provided with a first substrate electrode 131 and a second substrate electrode 132 connected on both sides, the ink sensing layer 12 is screen-printed on the flexible printed circuit substrate 13, and the packaging layer 11 covers the ink sensing layer 12 to encapsulate the ink sensing layer 12. In one embodiment of the present invention, an epoxy film is used for packaging, and the resin interface formed after curing can not only stably bond to the surface of the composite material structure, but also play a role of insulation protection. When the sensitive conductive ink is used as a stress and strain sensing material of a flexible thin film strain sensor, the consistency of the distribution of the resistance value of the flexible thin film strain sensor can be achieved, especially the sensitivity, stability, hysteresis and other properties of the resistance signal under the action of external force. Figure 1 In the illustrated embodiment, a first conductive ring 121 and a second conductive ring 122 are formed at the head and the end of the ink sensing layer 12 , respectively. The first conductive ring 121 and the second conductive ring 122 are aligned with the first substrate electrode 131 and the second substrate electrode 132 , respectively.
[0080] Furthermore, the thickness of the flexible printed circuit substrate 13 is 50μm to 250μm; the material of the substrate electrodes 131 and 132 is at least one of silver, aluminum, and copper; the thickness of the substrate electrodes 131 and 132 is 0.01mm to 0.04mm; the substrate electrode is aligned with the electrode position on the screen printing template; one side of the substrate electrode is printed with conductive ink, and the other side is welded with a wire to prepare the positive and negative electrodes of the sensor.
[0081] The ink sensing layer 12 of the embodiment of the present invention makes a synchronous response under the positive strain cycle. As the deformation increases, the resistance value of the ink sensing layer 12 increases, showing a positive strain-resistance effect. The black line is the strain response curve, and the red line is the resistance change rate response curve. Figure 6 Therefore, in the flexible film strain sensor of the present invention, which uses the ink sensing layer 12 as the sensitive film layer, the sensor generates a change in resistance value when subjected to external pressure.
[0082] Static stress monitoring focuses on the percolation mechanism, that is, the conductive path formed by the direct contact between the conductive fillers, while guided wave signal monitoring relies on the tunneling effect, that is, the quantum tunneling transition of electrons in the conductive fillers. The combination of these two sensing mechanisms enables the ink strain sensor to be flexibly applied to different monitoring and detection needs, from static stress monitoring to dynamic guided wave signal analysis, providing accurate and reliable data support.
[0083] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0084] Example 1
[0085] In embodiment 1 of the present invention, a method for preparing a strain sensor based on conductive ink is disclosed, comprising the following steps:
[0086] Step S1, grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain a uniformly dispersed conductive ink;
[0087] Step S2, screen printing the conductive ink onto the surface of the substrate according to a preset pattern, and heating and curing at a temperature of 120° C. for 5 minutes to form a conductive structure;
[0088] Step S3, using a packaging material to package the substrate and the conductive structure that has been cured on the substrate, so as to obtain the strain sensor;
[0089] The step of grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain uniformly dispersed conductive ink includes, in sequence, an initial mixing stage, a rough grinding stage, a fine grinding stage and a precise grinding stage.
[0090] Furthermore, the initial mixing stage comprises the following steps:
[0091] Step T1, mixing carbon nanotubes and graphene with resin and solvent according to designed amounts;
[0092] Step T2, preliminarily dispersing by magnetic stirring or ultrasonic oscillation to ensure that the carbon nanotubes and graphene are evenly distributed in the solvent;
[0093] Step T3, setting the gap between the rollers of the three-roll mill to 100 μm to ensure that there is no excessive loss of material or clogging during grinding.
[0094] Furthermore, the rough grinding stage comprises the following steps:
[0095] Step P1, start the grinder, maintain a relatively low roller speed of 30 r / min, start grinding, and continuously observe the material state during the grinding process to ensure that the material is evenly distributed;
[0096] Step P2, gradually reduce the gap between the rollers to 80 μm, ensuring that the material can adapt to the new gap after each adjustment;
[0097] The adjustment distance of each spacing is 20 μm, and the grinding time after each spacing adjustment is 10 minutes.
[0098] Furthermore, the fine grinding stage comprises the following steps:
[0099] After the material is initially dispersed evenly, the gap between the rollers is gradually reduced to 50 μm, and the roller speed is maintained at 30 r / min to prevent high shear forces from causing damage to the carbon nanotubes or graphene sheets;
[0100] The adjustment distance of each spacing is 30 μm, and the grinding time after each spacing adjustment is 20 minutes, ensuring that the material can be further dispersed under the new spacing conditions.
[0101] Furthermore, the lapping stage comprises the following steps:
[0102] Gradually reduce the gap between the rollers to 20μm, keep the roller speed at 30r / min, and adjust the gap by 30μm each time to avoid excessive grinding and change of material properties;
[0103] Grind for 30 minutes to ensure that the carbon nanotubes and graphene are evenly dispersed in the resin and solvent.
[0104] Furthermore, the step of screen printing the conductive ink onto the surface of the substrate according to a preset pattern comprises:
[0105] Step R1, fixing the screen printing template on the screen printing workbench, and keeping the electrode position on the substrate coincident with the electrode position on the screen printing template;
[0106] Step R2, evenly coating the conductive ink on the screen printing template, using a scraper to apply uniform pressure, and printing the ink through the mesh of the screen onto the substrate.
[0107] In Example 1, the preset pattern is a bow-shaped structure, so that the prepared ink sensing layer 12 also has a bow-shaped structure.
[0108] Furthermore, the packaging material is one or more of imide film, epoxy resin and silica gel.
[0109] Furthermore, the conductive ink is composed of the following materials in percentage by mass:
[0110]
[0111] In Example 1, the resin is a saturated polyester resin. In the embodiment of the present invention, the selected resin has excellent flexibility and resilience, which gives the sensitive conductive ink excellent flexibility and resilience, as well as a large range of mechanical quantity changes.
[0112] Reference Figure 1The present invention also discloses a strain sensor, which is prepared by the strain sensor preparation method as described in any one of the above items, and the strain sensor includes: a flexible printed circuit substrate 13, an ink sensing layer 12 and a packaging layer 11, the flexible printed circuit substrate 13 is provided with a first substrate electrode 131 and a second substrate electrode 132 connected on both sides, the ink sensing layer 12 is screen-printed on the flexible printed circuit substrate 13, and the packaging layer 11 covers the ink sensing layer 12 to encapsulate the ink sensing layer 12. In one embodiment of the present invention, an epoxy film is used for packaging, and the resin interface formed after curing can not only stably bond to the surface of the composite material structure, but also play a role of insulation protection. When the sensitive conductive ink is used as a stress and strain sensing material of a flexible thin film strain sensor, the consistency of the distribution of the resistance value of the flexible thin film strain sensor can be achieved, especially the sensitivity, stability, hysteresis and other properties of the resistance signal under the action of external force. Figure 1 In the illustrated embodiment, a first conductive ring 121 and a second conductive ring 122 are formed at the head and the end of the ink sensing layer 12 , respectively. The first conductive ring 121 and the second conductive ring 122 are aligned with the first substrate electrode 131 and the second substrate electrode 132 , respectively.
[0113] Furthermore, the thickness of the flexible printed circuit substrate 13 is 250 μm; the material of the substrate electrodes 131 and 132 is copper; the thickness of the substrate electrodes 131 and 132 is 0.03 mm; the substrate electrodes are aligned with the electrode positions on the screen printing template; one side of the substrate electrode is printed with conductive ink, and the other side is welded with a wire to prepare the positive and negative electrodes of the sensor.
[0114] Performance test: The strain sensor prepared in Example 1 was subjected to static and dynamic tests, and the response curve is as follows: Figure 2-4 As shown. Figure 2-4 The analysis shows that: Figure 2-4 The analysis shows that the sensor's high sensitivity (GF=27.48), ultrafast response time (0.04-0.05 microseconds), and wide-band monitoring capability (up to 10MHz) effectively meet the requirements of high-precision, high-speed response, and wide-band monitoring in the field of structural health monitoring. Combined with a sophisticated three-roll grinding process, the microstructure of the sensor material can be ensured to be in an optimal state. The uniform CNT and GN distribution, stable tunneling distance, and bone sponge-like structure work together to make the sensor perform well in sensitivity, response speed, and band monitoring capability. The optimization of the grinding process is the key to achieving superior performance of the sensor. This process ensures that the sensor meets the application requirements of high-precision, high-speed response, and wide-band monitoring, providing strong technical support for structural health monitoring.
[0115] Example 2
[0116] In embodiment 2 of the present invention, a method for preparing a strain sensor based on conductive ink is disclosed, comprising the following steps:
[0117] Step S1, grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain a uniformly dispersed conductive ink;
[0118] Step S2, screen printing the conductive ink onto the surface of the substrate according to a preset pattern, and heating and curing at a temperature of 130° C. for 3 minutes to form a conductive structure;
[0119] Step S3, using a packaging material to package the substrate and the conductive structure that has been cured on the substrate, so as to obtain the strain sensor;
[0120] The step of grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain uniformly dispersed conductive ink includes, in sequence, an initial mixing stage, a rough grinding stage, a fine grinding stage and a precise grinding stage.
[0121] Furthermore, the initial mixing stage comprises the following steps:
[0122] Step T1, mixing carbon nanotubes and graphene with resin and solvent according to designed amounts;
[0123] Step T2, preliminarily dispersing by magnetic stirring or ultrasonic oscillation to ensure that the carbon nanotubes and graphene are evenly distributed in the solvent;
[0124] Step T3, the gap between the rollers of the three-roll mill is set to 120 μm to ensure that there is no excessive loss of material or clogging during grinding.
[0125] Furthermore, the rough grinding stage comprises the following steps:
[0126] Step P1, start the grinder, maintain a relatively low roller speed of 50 r / min, start grinding, and continuously observe the material state during the grinding process to ensure that the material is evenly distributed;
[0127] Step P2, gradually reduce the gap between the rollers to 70 μm, ensuring that the material can adapt to the new gap after each adjustment;
[0128] The adjustment distance of each spacing is 10 μm, and the grinding time after each spacing adjustment is 10 minutes.
[0129] Furthermore, the fine grinding stage comprises the following steps:
[0130] After the material is initially dispersed evenly, the gap between the rollers is gradually reduced to 60 μm, and the roller speed is maintained at 50 r / min to prevent high shear forces from causing damage to the carbon nanotubes or graphene sheets;
[0131] The adjustment distance of each spacing is 20 μm, and the grinding time after each spacing adjustment is 10 minutes, ensuring that the material can be further dispersed under the new spacing conditions.
[0132] Furthermore, the lapping stage comprises the following steps:
[0133] Gradually reduce the gap between the rollers to 15μm, keep the roller speed at 20r / min, and adjust the gap by 20μm each time to avoid excessive grinding and change of material properties;
[0134] Grind for 30 minutes to ensure that the carbon nanotubes and graphene are evenly dispersed in the resin and solvent.
[0135] Furthermore, the step of screen printing the conductive ink onto the surface of the substrate according to a preset pattern comprises:
[0136] Step R1, fixing the screen printing template on the screen printing workbench, and keeping the electrode position on the substrate coincident with the electrode position on the screen printing template;
[0137] Step R2, evenly coating the conductive ink on the screen printing template, using a scraper to apply uniform pressure, and printing the ink through the mesh of the screen onto the substrate.
[0138] In Example 1, the preset pattern is a bow-shaped structure, so that the prepared ink sensing layer 12 also has a bow-shaped structure.
[0139] Furthermore, the packaging material is one or more of imide film, epoxy resin and silica gel.
[0140] Furthermore, the conductive ink is composed of the following materials in percentage by mass:
[0141]
[0142] In Example 1, the resin is a saturated polyester resin. In the embodiment of the present invention, the selected resin has excellent flexibility and resilience, which gives the sensitive conductive ink excellent flexibility and resilience, as well as a large range of mechanical quantity changes.
[0143] Reference Figure 1The present invention also discloses a strain sensor, which is prepared by the strain sensor preparation method as described in any one of the above items, and the strain sensor includes: a flexible printed circuit substrate 13, an ink sensing layer 12 and a packaging layer 11, the flexible printed circuit substrate 13 is provided with a first substrate electrode 131 and a second substrate electrode 132 connected on both sides, the ink sensing layer 12 is screen-printed on the flexible printed circuit substrate 13, and the packaging layer 11 covers the ink sensing layer 12 to encapsulate the ink sensing layer 12. In one embodiment of the present invention, an epoxy film is used for packaging, and the resin interface formed after curing can not only stably bond to the surface of the composite material structure, but also play a role of insulation protection. When the sensitive conductive ink is used as a stress and strain sensing material of a flexible thin film strain sensor, the consistency of the distribution of the resistance value of the flexible thin film strain sensor can be achieved, especially the sensitivity, stability, hysteresis and other properties of the resistance signal under the action of external force. Figure 1 In the illustrated embodiment, a first conductive ring 121 and a second conductive ring 122 are formed at the head and the end of the ink sensing layer 12 , respectively. The first conductive ring 121 and the second conductive ring 122 are aligned with the first substrate electrode 131 and the second substrate electrode 132 , respectively.
[0144] Furthermore, the thickness of the flexible printed circuit substrate 13 is 50 μm; the material of the substrate electrodes 131 and 132 is copper; the thickness of the substrate electrodes 131 and 132 is 0.04 mm; the substrate electrodes are aligned with the electrode positions on the screen printing template; one side of the substrate electrode is printed with conductive ink, and the other side is welded with a wire to prepare the positive and negative electrodes of the sensor.
[0145] Example 3
[0146] In embodiment 3 of the present invention, a method for preparing a strain sensor based on conductive ink is disclosed, comprising the following steps:
[0147] Step S1, grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain a uniformly dispersed conductive ink;
[0148] Step S2, screen printing the conductive ink onto the surface of the substrate according to a preset pattern, and heating and curing at a temperature of 125° C. for 4 minutes to form a conductive structure;
[0149] Step S3, using a packaging material to package the substrate and the conductive structure that has been cured on the substrate, so as to obtain the strain sensor;
[0150] The step of grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain uniformly dispersed conductive ink includes, in sequence, an initial mixing stage, a rough grinding stage, a fine grinding stage and a precise grinding stage.
[0151] Furthermore, the initial mixing stage comprises the following steps:
[0152] Step T1, mixing carbon nanotubes and graphene with resin and solvent according to designed amounts;
[0153] Step T2, preliminarily dispersing by magnetic stirring or ultrasonic oscillation to ensure that the carbon nanotubes and graphene are evenly distributed in the solvent;
[0154] Step T3, the gap between the rollers of the three-roll mill is set to 115 μm to ensure that there is no excessive loss of material or clogging during grinding.
[0155] Furthermore, the rough grinding stage comprises the following steps:
[0156] Step P1, start the grinder, maintain a relatively low roller speed of 40 r / min, start grinding, and continuously observe the material state during the grinding process to ensure that the material is evenly distributed;
[0157] Step P2, gradually reduce the gap between the rollers to 75 μm, ensuring that the material can adapt to the new gap after each adjustment;
[0158] The adjustment distance of each spacing is 15 μm, and the grinding time after each spacing adjustment is 5 minutes.
[0159] Furthermore, the fine grinding stage comprises the following steps:
[0160] After the material is initially dispersed evenly, the gap between the rollers is gradually reduced to 55 μm, and the roller speed is maintained at 40 r / min to prevent high shear forces from causing damage to the carbon nanotubes or graphene sheets;
[0161] The adjustment distance of each spacing is 25 μm, and the grinding time after each spacing adjustment is 15 minutes, ensuring that the material can be further dispersed under the new spacing conditions.
[0162] Furthermore, the lapping stage comprises the following steps:
[0163] Gradually reduce the gap between the rollers to 18μm, keep the roller speed at 25r / min, and adjust the gap by 25μm each time to avoid excessive grinding and changes in material properties;
[0164] Grind for 25 minutes to ensure that the carbon nanotubes and graphene are evenly dispersed in the resin and solvent.
[0165] Furthermore, the step of screen printing the conductive ink onto the surface of the substrate according to a preset pattern comprises:
[0166] Step R1, fixing the screen printing template on the screen printing workbench, and keeping the electrode position on the substrate coincident with the electrode position on the screen printing template;
[0167] Step R2, evenly coating the conductive ink on the screen printing template, using a scraper to apply uniform pressure, and printing the ink through the mesh of the screen onto the substrate.
[0168] In Example 1, the preset pattern is a bow-shaped structure, so that the prepared ink sensing layer 12 also has a bow-shaped structure.
[0169] Furthermore, the packaging material is one or more of imide film, epoxy resin and silica gel.
[0170] Furthermore, the conductive ink is composed of the following materials in percentage by mass:
[0171]
[0172] In Example 1, the resin is a saturated polyester resin. In the embodiment of the present invention, the selected resin has excellent flexibility and resilience, which gives the sensitive conductive ink excellent flexibility and resilience, as well as a large range of mechanical quantity changes.
[0173] Reference Figure 1 The present invention also discloses a strain sensor, which is prepared by the strain sensor preparation method as described in any one of the above items, and the strain sensor includes: a flexible printed circuit substrate 13, an ink sensing layer 12 and a packaging layer 11, the flexible printed circuit substrate 13 is provided with a first substrate electrode 131 and a second substrate electrode 132 connected on both sides, the ink sensing layer 12 is screen-printed on the flexible printed circuit substrate 13, and the packaging layer 11 covers the ink sensing layer 12 to encapsulate the ink sensing layer 12. In one embodiment of the present invention, an epoxy film is used for packaging, and the resin interface formed after curing can not only stably bond to the surface of the composite material structure, but also play a role of insulation protection. When the sensitive conductive ink is used as a stress and strain sensing material of a flexible thin film strain sensor, the consistency of the distribution of the resistance value of the flexible thin film strain sensor can be achieved, especially the sensitivity, stability, hysteresis and other properties of the resistance signal under the action of external force. Figure 1 In the illustrated embodiment, a first conductive ring 121 and a second conductive ring 122 are formed at the head and the end of the ink sensing layer 12 , respectively. The first conductive ring 121 and the second conductive ring 122 are aligned with the first substrate electrode 131 and the second substrate electrode 132 , respectively.
[0174] Furthermore, the thickness of the flexible printed circuit substrate 13 is 100 μm; the material of the substrate electrodes 131 and 132 is copper; the thickness of the substrate electrodes 131 and 132 is 0.01 mm; the substrate electrodes are aligned with the electrode positions on the screen printing template; one side of the substrate electrode is printed with conductive ink, and the other side is welded with a wire to prepare the positive and negative electrodes of the sensor.
[0175] The above description is only a partial implementation of the embodiments of the present invention and does not impose any form of limitation on the application. The protection scope of the embodiments of the present invention is not limited to this. Any simple modifications, equivalent changes and modifications that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the embodiments of the present invention should be covered within the protection scope of the embodiments of the present invention.
Claims
1. A method for preparing a strain sensor based on conductive ink, characterized in that: The following steps are involved: Grinding the designed amount of carbon nanotubes, graphene mixture, resin and solvent to obtain uniformly dispersed conductive ink; The conductive ink is screen-printed onto the surface of the substrate according to a preset pattern, and heated and cured at a temperature of 120° C. to 130° C. for 3 min to 5 min to form a conductive structure; The strain sensor is manufactured by packaging the substrate and the conductive structure on the substrate after curing using a packaging material; The step of grinding the designed amount of carbon nanotubes, graphene, resin and solvent to obtain uniformly dispersed conductive ink includes, in sequence, an initial mixing stage, a rough grinding stage, a fine grinding stage and a precise grinding stage.
2. The method for preparing a strain sensor according to claim 1, characterized in that: The initial mixing stage comprises the following steps: Mixing carbon nanotubes and graphene with resin and solvent according to designed amounts; Preliminary dispersion by magnetic stirring or ultrasonic oscillation ensures that the carbon nanotubes and graphene are evenly distributed in the solvent; The gap between the rollers of the three-roll mill was set to 100-120 μm to ensure that there would be no excessive loss of material or clogging during grinding.
3. The method for preparing a strain sensor according to claim 1, characterized in that: The rough grinding stage includes the following steps: Start the grinder, maintain a low roller speed of 30-50r / min, and begin grinding. During the grinding process, continue to observe the state of the material to ensure that the material is evenly distributed; The gap between the rollers is gradually reduced to 70-80 μm, ensuring that the material can adapt to the new gap after each adjustment; The adjustment distance of each spacing is 10 to 20 μm, and the grinding time after each spacing adjustment is 5 to 10 minutes.
4. The method for preparing a strain sensor according to claim 1, characterized in that: The grinding stage includes the following steps: After the material is initially dispersed evenly, the distance between the rollers is gradually reduced to 50-60 μm, and the roller speed is maintained at 30-50 r / min to prevent the high shear force from causing damage to the carbon nanotubes or graphene sheets; The adjustment distance of each spacing is 20 to 30 μm, and the grinding time after each spacing adjustment is 10 to 20 minutes, ensuring that the material can be further dispersed under the new spacing conditions.
5. The method for preparing a strain sensor according to claim 1, characterized in that: The lapping stage comprises the following steps: Gradually reduce the gap between the rollers to 15-20μm, keep the roller speed at 20-30r / min, and adjust the gap by 20-30μm each time to avoid excessive grinding and changes in material properties; Grind for 20-30 minutes to ensure that the carbon nanotubes and graphene are evenly dispersed in the resin and solvent.
6. The method for preparing a strain sensor according to claim 1, characterized in that: The step of screen printing the conductive ink onto the surface of the substrate according to a preset pattern comprises: Fixing the screen printing template on the screen printing workbench, and keeping the electrode position on the substrate coincident with the electrode position on the screen printing template; The conductive ink is evenly coated on the screen printing template, and a scraper is used to apply uniform pressure to print the ink through the mesh of the screen onto the substrate.
7. The method for preparing a strain sensor according to claim 1 or 6, characterized in that: The preset pattern is one or more of a straight line, a bent shape, an S shape, a circuitous shape, and a bow shape; and the substrate is one or more of polyimide, glass, and ceramic.
8. The method for preparing a strain sensor according to claim 1, characterized in that: The packaging material is one or more of imide film, epoxy resin and silica gel.
9. The method for preparing a strain sensor according to claim 1, characterized in that: In terms of mass percentage, the conductive ink is composed of the following materials:
10. The method for preparing a strain sensor according to claim 9, characterized in that: The resin is one or more of saturated polyester resin, acrylic resin, and epoxy resin; the solvent is one or more of DBE, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol ethyl ether acetate, dimethyl adipate, diethyl adipate, and N-methylpyrrolidone.
11. A strain sensor, characterized in that: The strain sensor is prepared by the strain sensor preparation method according to any one of claims 1 to 10, comprising: a flexible printed circuit substrate, an ink sensing layer and a packaging layer, the flexible printed circuit substrate is provided with a substrate electrode connected on both sides, the ink sensing layer is screen-printed on the flexible printed circuit substrate, and the packaging layer covers the ink sensing layer to encapsulate the ink sensing layer.
12. The strain sensor according to claim 11, characterized in that: The thickness of the flexible printed circuit substrate is 50μm to 250μm; the material of the substrate electrode is at least one of silver, aluminum, and copper; the thickness of the substrate electrode is 0.01mm to 0.04mm; the substrate electrode is aligned with the electrode position on the screen printing template; one side of the substrate electrode is printed with conductive ink, and the other side is welded with a wire to prepare the positive and negative electrodes of the sensor.