Elastic functional coating with high infrared emissivity and preparation method thereof
By using a combination formula of elastic hydroxy resin and polyisocyanate elastic curing agent in high emissivity infrared coatings, the problems of insufficient tensile strength and easy cracking of existing coatings are solved, and high infrared emissivity and excellent on the surface of deformed substrates are achieved. Mechanical properties, coating preparation adapted to high-frequency vibration, and has good media and environmental resistance.
Patent Information
- Application Number
- CN202411386268.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
The tensile strength of existing high-emissivity infrared coatings is insufficient, which is difficult to meet the needs of aircraft long-term service applications, and the coating cracking and falling off is prone to occur under substrate deformation and high-frequency vibration conditions.
The combination of component A and component B, including elastic hydroxy resin, polyisocyanate elastic curing agent, filler, anti-deposition agent, dispersant, drying agent and mixed solvent, is used to form a fineness less than that of pre-dispersion and sanding treatment. 40μm component A is mixed uniformly with polyisocyanate elastic curing agent and mixed solvent to form component B, and finally mix it in a 1:1 ratio to prepare the coating to ensure that the coating has high infrared emissivity and excellent Mechanical properties.
The high infrared emissivity characteristic on the surface of the deformed substrate is achieved. The coating has good adaptability to deformation and vibration. The infrared emissivity is greater than 0.8, and has excellent mechanical properties. It has good media and environmental resistance to penetration and damage to corrosive media.
Smart Images

Figure BDA0005071042350000011 
Figure BDA0005071042350000021 
Figure BDA0005071042350000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and in particular relates to an elastic high infrared emissivity functional coating and a preparation method thereof. Background Art
[0002] As a new type of heat-resistant protective coating with infrared radiation ability, high emissivity coating mainly plays the role of energy saving and consumption reduction. It has a series of advantages such as simple construction, saving investment, and wide application range. It has been widely used in metallurgy, petrochemical, ceramics, medicine and other industries in my country.
[0003] "Preparation and Performance Research of High-Emissivity Infrared Radiation Coatings for Spacecraft" (Liu Leichun et al., Coatings Industry, 2023, 53(8): 8-13) introduces the preparation and performance research of high-emissivity infrared radiation coatings. The high-emissivity infrared radiation powder is obtained by compounding alkali metal hydroxides and their oxides with SiC, and then mixed with silicone rubber to obtain high-emissivity infrared coatings. The developed high-emissivity infrared coatings have an infrared emissivity of up to 0.93, a tensile strength of 2.89MPa, and an elongation at break of 114%. Although the high-emissivity infrared coating studied in this paper is also an elastic coating, its tensile strength is limited by the intrinsic mechanical properties of silicone rubber and is only less than 3MPa, which is difficult to meet the long-term service application requirements of aircraft. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide an elastic high infrared emissivity functional coating and a preparation method thereof, which can adapt to the deformation of various types of flexible substrates and application environments under various high-frequency vibration conditions without the problem of coating cracking and falling off. It has good adaptability to the deformation and vibration of the substrate and can achieve high infrared emissivity characteristics on the surface of the deformed substrate in dynamic work.
[0005] The present invention provides an elastic high infrared emissivity functional coating, comprising component A and component B;
[0006] The component A comprises an elastic hydroxyl resin, a high-emissivity filler, an anti-settling agent, a dispersant, a leveling agent, a drying agent and a mixed solvent; the elastic hydroxyl resin comprises hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12):(20-40):(4-10):(20-30):(20-30);
[0007] The second component comprises a polyisocyanate elastic curing agent and a mixed solvent.
[0008] Preferably, in terms of mass fraction, the formula of component A is:
[0009]
[0010]
[0011] Preferably, the total hydroxyl value of the elastic hydroxyl resin is 2.0 to 4.0 mg KOH / g.
[0012] Preferably, the filler is selected from two or more of titanium dioxide, aluminum oxide, zinc oxide, zirconium dioxide and chromium oxide.
[0013] Preferably, the mixed solvent is selected from two or more of xylene, butyl acetate, cyclohexanone, butanone, ethyl acetate and ethylene glycol ethyl ether acetate.
[0014] Preferably, the polyisocyanate elastic curing agent comprises HMDI (dicyclohexylmethane diisocyanate)-polyolefin prepolymer;
[0015] It also includes one or more of HDI (hexamethylene diisocyanate) trimer, IPDI (isophordione diisocyanate) and HMDI (dicyclohexylmethane diisocyanate).
[0016] Preferably, the mass ratio of the polyisocyanate elastic curing agent to the mixed solvent in the second component is (40-60): (40-60).
[0017] The present invention provides a method for preparing the elastic high infrared emissivity functional coating described in the above technical solution, comprising the following steps:
[0018] The mixed solvent, elastic hydroxyl resin, filler, anti-settling agent, drying agent, dispersant and leveling agent are mixed, and after pre-dispersion, sand-grinded until the coating fineness is less than 40 μm to obtain component A;
[0019] The polyisocyanate elastic curing agent and the mixed solvent are mixed evenly to obtain component B.
[0020] The present invention provides an elastic high infrared emissivity functional coating, comprising component A and component B; the component A comprises an elastic hydroxy resin, a filler, an anti-settling agent, a dispersant, a leveling agent, a drying agent and a mixed solvent; the elastic hydroxy resin comprises hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12):(20-40):(4-10):(20-30):(20-30); the component B comprises a polyisocyanate elastic curing agent and a mixed solvent. The coating has good interlayer adhesion with a substrate, forms a coating after curing on the surface of the substrate, has excellent mechanical properties, good elasticity, high strength, good adaptability to deformation of a deformed substrate, and can realize dynamic protection for the substrate; the cured coating has good medium tolerance, has good protection effect on salt spray and hot and humid environments, and can effectively prevent the penetration and damage of the corrosive medium to the substrate. DETAILED DESCRIPTION
[0021] The present invention provides an elastic high infrared emissivity functional coating, comprising component A and component B;
[0022] The component A comprises an elastic hydroxyl resin, a filler, an anti-settling agent, a dispersant, a leveling agent, a drying agent and a mixed solvent; the elastic hydroxyl resin comprises hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12):(20-40):(4-10):(20-30):(20-30);
[0023] The second component comprises a polyisocyanate elastic curing agent and a mixed solvent.
[0024] The coating can adapt to the deformation of various types of flexible substrates and application environments under various high-frequency vibration conditions without cracking or falling off. It has good adaptability to the deformation and vibration of the substrate and can achieve high infrared emissivity characteristics on the surface of the deformed substrate in dynamic work. The infrared emissivity is greater than 0.8. The coating itself also has excellent resistance to various media and environmental performance.
[0025] In terms of mass percentage, the formula of component A in the present invention is:
[0026]
[0027] The present invention can precisely regulate the mechanical properties of the coating by controlling the above-mentioned formula to meet the high infrared function requirements of the surface of the flexible deformable substrate in different application scenarios.
[0028] In the present invention, component A includes an elastic hydroxyl resin, and the elastic hydroxyl resin includes hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12): (20-40): (4-10): (20-30): (20-30). In a specific embodiment, the elastic hydroxyl resin is a mixture of hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of 10:20:10:30:30, and the hydroxyl value is 3.5 mg KOH / g; or a mixture of hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of 8:36:6:25:25, and the hydroxyl value is 3.2 mg KOH / g. The present invention selects the elastic hydroxyl resin prepared by the above-mentioned specific components as the resin material of the coating to meet the high infrared function requirements of the surface of the flexible deformable substrate in different application scenarios.
[0029] The total hydroxyl value of the elastic hydroxyl resin is 2.0-4.0 mg KOH / g, preferably 3.0-4.0 mg KOH / g; in a specific embodiment, the total hydroxyl value of the elastic hydroxyl resin is 3.2 mg KOH / g or 3.5 mg KOH / g. The elastic hydroxyl resin in the above total hydroxyl value range enables the functional coating to have more excellent mechanical properties, such as impact resistance, flexibility, adhesion, moisture and heat resistance, and neutral salt spray resistance.
[0030] The filler in the present invention is selected from two or more of titanium dioxide, aluminum oxide, zinc oxide, zirconium dioxide and chromium oxide. In a specific embodiment, the filler is selected from a mixture of titanium dioxide, zinc oxide and talc in a mass ratio of 3:30:4; or a mixture of aluminum oxide, zinc oxide and zirconium dioxide in a mass ratio of 5:25:5; or a mixture of aluminum oxide, zinc oxide and chromium oxide in a mass ratio of 2:30:8. The above-mentioned types of fillers make the coating have excellent infrared emissivity.
[0031] The mixed solvent in the present invention is selected from two or more of xylene, butyl acetate, cyclohexanone, butanone, ethyl acetate or ethylene glycol ethyl ether acetate solvents. In a specific embodiment, the mixed solvent is selected from a mixed solvent of xylene, butyl acetate and cyclohexanone in a mass ratio of 4:3:3; or a mixed solvent of xylene, butyl acetate and ethyl acetate in a mass ratio of 3:3:4; or a mixed solvent of xylene, butyl acetate and butanone in a mass ratio of 4:4:2.
[0032] The anti-settling agent of the present invention is Aerosil R972; the drying agent is preferably organic tin DY12, the dispersant is preferably Digo 670 and the leveling agent is preferably BYK331.
[0033] The elastic high infrared emissivity functional coating provided by the present invention comprises a component B, wherein the component B comprises a polyisocyanate elastic curing agent and a mixed solvent. The polyisocyanate elastic curing agent comprises HMDI-polyolefin prepolymer; the polyisocyanate elastic curing agent further comprises one or more of HDI (hexamethylene diisocyanate) trimer, IPDI (isophordione diisocyanate) or HMDI (dicyclohexylmethane diisocyanate); the mass ratio of the HMDI-polyolefin prepolymer to other types of polyisocyanate elastic curing agents is 2-10:40-60. In a specific embodiment, the polyisocyanate elastic curing agent includes a mixture of HDI trimer (product brand N3390) and HMDI-polyolefin prepolymer in a mass ratio of 5:45; or a mixture of HDI trimer (product brand N3390), IPDI and HMDI-polyolefin prepolymer in a mass ratio of 3:5:52; or a mixture of HDI trimer (product brand N3390), HMDI and HMDI-polyolefin prepolymer in a mass ratio of 2:4:44.
[0034] The mixed solvent in component B is selected from two or more of xylene, butyl acetate, cyclohexanone, butanone, ethyl acetate and ethylene glycol ethyl acetate. The type and composition of the mixed solvent in component A and the mixed solvent in component B may be consistent or inconsistent. In a specific embodiment, the mixed solvent in component B is selected from a mixed solvent of xylene, butyl acetate and cyclohexanone in a mass ratio of 4:3:3; or a mixed solvent of xylene, butyl acetate and ethyl acetate in a mass ratio of 3:3:4.
[0035] The mass ratio of the polyisocyanate elastic curing agent to the mixed solvent in the component B of the present invention is (40-60): (40-60); in a specific embodiment, the mass ratio of the polyisocyanate elastic curing agent to the mixed solvent is 60:40; or 50:50.
[0036] The mass ratio of component A to component B in the present invention is 1:1.
[0037] The present invention provides a method for preparing the elastic high infrared emissivity functional coating described in the above technical solution, comprising the following steps:
[0038] The mixed solvent, elastic hydroxyl resin, filler, anti-settling agent, drying agent, dispersant and leveling agent are mixed, and the mixture is pre-dispersed and sand-ground to a coating fineness of less than 40 μm to obtain component A; the elastic hydroxyl resin comprises hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12):(20-40):(4-10):(20-30):(20-30);
[0039] The polyisocyanate elastic curing agent and the mixed solvent are mixed evenly to obtain component B.
[0040] When ready to use, component A and component B are mixed together; the mass ratio of component A to component B is 1:1.
[0041] The above preparation method is simple and easy to realize industrialization. The present invention preferably adds a mixed solvent, an elastic hydroxyl resin, a filler, an anti-settling agent, a drying agent, a dispersant and a leveling agent in order, stirs and pre-disperses the materials, and then grinds and disperses them with a sand mill, a high-speed oscillating disperser or other grinding equipment until the coating fineness is less than 40 μm, and obtains the coating component A after filtering.
[0042] In order to further illustrate the present invention, an elastic high infrared emissivity functional coating and a preparation method thereof provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] Example 1
[0044] (1) Preparation of component A of elastic high infrared emissivity functional coating: 25 kg of mixed solvent (xylene: butyl acetate: cyclohexanone = 4:3:3), 35 kg of elastic hydroxyl resin (hydroxy polybutadiene acrylonitrile resin: hydroxy acrylate: polyaspartic acid ester: butyl acetate: xylene = 10:20:10:30:30, hydroxyl value 3.5 mg KOH / g), 37 kg of filler (3 kg of titanium dioxide, 30 kg of zinc oxide, 4 kg of aluminum oxide), 2 kg of anti-settling agent Aerosil R972, 0.10 kg of drying agent organotin DY12, 0.5 kg of dispersant Digo 670 and 0.5 kg of leveling agent BYK331 were added into a stirring barrel in sequence under high-speed stirring. After preliminary stirring and pre-dispersion, the mixture was ground and dispersed with a sand mill for 3 times until the coating fineness was less than 40 μm. After filtering, the mixture was canned to obtain component A of the coating.
[0045] (2) Preparation of component B of elastic high infrared emissivity functional coating: Add 50 kg of mixed solvent (xylene: butyl acetate: cyclohexanone = 4:3:3), 5 kg of HDI trimer (product brand N3390) and 45 kg of hydrogenated MDI-polyolefin prepolymer into a stirring barrel under high-speed stirring conditions, stir evenly, fill and seal, and obtain component B of the coating.
[0046] Example 2
[0047] (1) Preparation of component A of elastic high infrared emissivity functional coating: 20.5 kg of mixed solvent (xylene: butyl acetate: ethyl acetate = 3:3:4), 40 kg of elastic hydroxy resin (hydroxy polybutadiene acrylonitrile resin: hydroxy acrylate: polyaspartic acid ester: butyl acetate: xylene = 8:36:6:25:25, hydroxy value 3.2 mg KOH / g), 35 kg of filler (5 kg of aluminum oxide, 25 kg of zinc oxide, 5 kg of zirconium dioxide), 3 kg of anti-settling agent Aerosil R972, 0.10 kg of drying agent organic tin DY12, 0.6 kg of dispersant Digo 670 and 0.6 kg of leveling agent BYK331 were added into a stirring barrel in sequence under high-speed stirring. After preliminary stirring and pre-dispersion, the mixture was ground and dispersed with a sand mill for 3 times until the coating fineness was less than 40 μm. After filtering, the mixture was canned to obtain component A of the coating.
[0048] (2) Preparation of component B of elastic high infrared emissivity functional coating: 40 kg of mixed solvent (xylene: butyl acetate: ethyl acetate = 3:3:4), 3 kg of HDI trimer (product brand N3390), 5 kg of IPDI and 52 kg of hydrogenated MDI-polyolefin prepolymer are added into a stirring barrel under high-speed stirring conditions, and the mixture is stirred evenly, filled and sealed to obtain component B of the coating.
[0049] Example 3
[0050] (1) Preparation of component A of elastic high infrared emissivity functional coating: 25 kg of mixed solvent (xylene: butyl acetate: butanone = 4:4:2), 32 kg of elastic hydroxy resin (hydroxy polybutadiene acrylonitrile resin: hydroxy acrylate: polyaspartic acid ester: butyl acetate: xylene = 8:36:6:25:25, hydroxy value 3.2 mg KOH / g), 40 kg of filler (2 kg of aluminum oxide, 30 kg of zinc oxide, 8 kg of chromium oxide), 2 kg of anti-settling agent Aerosil R972, 0.10 kg of drying agent organotin DY12, 0.5 kg of dispersant Digo 670 and 0.5 kg of leveling agent BYK331 were added into a stirring barrel in sequence under high-speed stirring. After preliminary stirring and pre-dispersion, the mixture was ground and dispersed with a sand mill for 3 times until the coating fineness was less than 40 μm. After filtering, the mixture was canned to obtain component A of the coating.
[0051] (2) Preparation of component B of elastic high infrared emissivity functional coating: 50 kg of mixed solvent (xylene: butyl acetate: ethyl acetate = 3:3:4), 2 kg of HDI trimer (product brand N3390), 4 kg of HMDI and 44 kg of HMDI-polyolefin prepolymer are added into a stirring barrel under high-speed stirring conditions, and the mixture is stirred evenly, filled and sealed to obtain component B of the coating.
[0052] The present invention mixes the products of the elastic high infrared emissivity functional coatings of Examples 1 to 3 evenly in a mass ratio of 1:1 between component A and component B, prepares test samples according to the corresponding test standard requirements, and tests the main properties after curing at 80° C. for 12 hours. The test results are shown in Table 1:
[0053] Table 1
[0054]
[0055] It can be seen from the above embodiments that the present invention provides an elastic high infrared emissivity functional coating, including component A and component B; the component A includes an elastic hydroxy resin, a filler, an anti-settling agent, a dispersant, a leveling agent, a drying agent and a mixed solvent; the elastic hydroxy resin includes hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12): (20-40): (4-10): (20-30): (20-30); the component B includes a polyisocyanate elastic curing agent and a mixed solvent. The coating has good interlayer adhesion with the substrate, forms a coating after curing on the surface of the substrate, has excellent mechanical properties, good elasticity, high strength, good adaptability to the deformation of the deformed substrate, and can realize dynamic protection for the substrate; the cured coating has good medium tolerance, has good protection effect on salt spray and hot and humid environments, and can effectively prevent the penetration and damage of the corrosive medium to the substrate. The experimental results show that the infrared incidence rate (8μm~14μm) of the coating is 0.87~0.93; the elongation at break is 200~257%; the adhesion is 9.1~10.9MPa; and the tensile strength is 8.2~11.7MPa.
[0056] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. An elastic high infrared emissivity functional coating, comprising component A and component B; The component A comprises an elastic hydroxyl resin, a filler, an anti-settling agent, a dispersant, a leveling agent, a drying agent and a mixed solvent; the elastic hydroxyl resin comprises hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12):(20-40):(4-10):(20-30):(20-30); The second component comprises a polyisocyanate elastic curing agent and a mixed solvent.
2. The elastic high infrared emissivity functional coating according to claim 1, characterized in that: In terms of mass percentage, the formula of component A is:
3. The elastic high infrared emissivity functional coating according to claim 2, characterized in that: The total hydroxyl value of the elastic hydroxyl resin is 2.0 to 4.0 mg KOH / g.
4. The elastic high infrared emissivity functional coating according to claim 2, characterized in that: The filler is selected from two or more of titanium dioxide, aluminum oxide, zinc oxide, zirconium dioxide and chromium oxide.
5. The elastic high infrared emissivity functional coating according to claim 1, characterized in that: The mixed solvent is selected from two or more of xylene, butyl acetate, cyclohexanone, butanone, ethyl acetate and ethylene glycol ethyl ether acetate.
6. The elastic high infrared emissivity functional coating according to claim 1, characterized in that: The polyisocyanate elastic curing agent includes dicyclohexylmethane diisocyanate-polyolefin prepolymer; It also includes one or more of hexamethylene diisocyanate trimer, isophordione diisocyanate and dicyclohexylmethane diisocyanate.
7. The elastic high infrared emissivity functional coating according to claim 1, characterized in that: The mass ratio of the polyisocyanate elastic curing agent to the mixed solvent in the second component is (40-60): (40-60).
8. A method for preparing the elastic high infrared emissivity functional coating according to claim 1, comprising the following steps: The mixed solvent, elastic hydroxyl resin, filler, anti-settling agent, drying agent, dispersant and leveling agent are mixed, and the mixture is pre-dispersed and sand-ground to a coating fineness of less than 40 μm to obtain component A; the elastic hydroxyl resin comprises hydroxy polybutadiene acrylonitrile resin, hydroxy acrylate, polyaspartic acid ester, butyl acetate and xylene in a mass ratio of (6-12):(20-40):(4-10):(20-30):(20-30); The polyisocyanate elastic curing agent and the mixed solvent are mixed evenly to obtain component B.
Citation Information
Patent Citations
Multicolor infrared low-emissivity environmental protection coating
CN104403440A
Preparation and application method of dark-colored heat-reflective ship deck coating
CN104910755A
Radome antistatic coating and preparation method thereof
CN109575777A
Elastic protective coating for flexible base material and preparation method of elastic protective coating
CN115286988A
Polyurea coating for fiberboard surface
CN115403995A