Concrete interface agent, preparation method and application

Through the in-situ emulsion polymerization of lithium acrylate-silica sol precursor and olefin monomer, an organic-inorganic hybrid structure is formed, which solves the brittleness and water resistance of concrete interface agents, and improves the adhesion and curing layer of the surfaces of new and old concretes. density.

CN119081493AInactive Publication Date: 2024-12-06SHANGHAI KEXIN NEW MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411447215.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-16
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing concrete interface agents have problems such as brittleness, low curing strength, poor water resistance, and insufficient adhesion on the surface of old concrete.

Method used

In situ emulsion polymerization with lithium acrylate-silica sol precursor and other olefin monomers is used to form an organic-inorganic hybrid structure. Through the reaction between lithium acrylate-silica sol precursor and concrete surface layer, the toughness of the cured layer of the interface agent is improved. and water resistance, and improve adhesion through the permeability of lithium ions.

Benefits of technology

It significantly improves the adhesion and water resistance of concrete interface agents, and is suitable for new and old concrete surfaces, ensuring high adhesion and dense cured layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of building materials, and particularly relates to a concrete interface agent, a preparation method and application, the concrete interface agent comprises the following components by weight: 5-10% of a lithium acrylate-silica sol precursor, 0.5-2% of an emulsifier, 0.1-0.5% of an initiator, 10-20% of a vinyl monomer, and 67.5-80% of water; the lithium acrylate-silica sol precursor is prepared from the following components in percentage by weight: 15 to 25 percent of acrylic monomer, 0.005 to 0.01 percent of polymerization inhibitor, 5 to 15 percent of lithium hydroxide, 35 to 45 percent of silica sol and 30 to 40 percent of water; the water resistance and the adhesive force are improved, and the adhesive force on new concrete and old concrete can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to a concrete interface agent, a preparation method and application thereof. Background Art

[0002] Concrete interface agents usually use alkali metal silicates as the main component, such as potassium silicate and sodium silicate aqueous solutions, which can solidify the concrete surface to form an interface layer, play a role in waterproofing and bonding, and provide adhesion for organic materials. However, pure silicate interface agents have the disadvantages of being brittle, low in curing strength, poor in permeability, and poor in water resistance.

[0003] Using organic polymer modification to improve the performance of the interface agent is a common method. CN115820053A discloses a method of using an acrylic copolymer emulsion with a particle size of less than 100nm, and a wetting agent to reduce the surface tension of the concrete interface agent. By introducing the epoxy end of the cross-linking agent into the carboxyl group in the acrylic polymer emulsion for ring-opening grafting, the inorganic concrete base and the acrylic copolymer ester bond form an effective bridge, thereby improving the reinforcement performance and surface hardness of the concrete base, and the reinforcement is greater than 0.85MPa, and can reach up to 1.02Mpa. CN109553717A discloses a method for preparing a concrete interface agent by adding a silane coupling agent, nano zinc oxide, a dispersant, a wetting agent, a pH regulator, a defoamer and a thickener to a hydrophobic acrylic polymer emulsion. The bonding strength on the concrete surface can reach up to 1.4MPa, but it is only suitable for new concrete surfaces. It is not known whether it is effective for loose old concrete surfaces.

[0004] Although the bonding strength of the interface agent can be increased by physical cold bonding with inorganic materials, organic-inorganic materials still have problems such as poor compatibility, short storage period and poor permeability. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a concrete interface agent, a preparation method and an application thereof, so as to improve water resistance and adhesion, and can improve adhesion on new concrete and old concrete.

[0006] The embodiment of the present invention provides a concrete interface agent, comprising the following components in percentage by weight: Lithium acrylate-silica sol precursor 5-10%, Emulsifier 0.5-2%, Initiator 0.1-0.5%, Olefin monomer 10-20%, Water 67.5-80%; The lithium acrylate-silica sol precursor comprises the following components in percentage by weight: Acrylic monomer 15-25%, Inhibitor 0.005-0.01%, Lithium hydroxide 5-15%, Silica sol 35-45%, Water 30-40%.

[0007] Preferably, the concrete interface agent includes the following components in percentage by weight: Lithium acrylate-silica sol precursor 6-9%, Emulsifier 0.8-1.8%, Initiator 0.2-0.4%, Olefin monomer 12-18%, Water 70-79%; The lithium acrylate-silica sol precursor comprises the following components in percentage by weight: Acrylic monomer 18-22%, Inhibitor 0.008-0.01%, Lithium hydroxide 8-12%, Silica sol 32-36%, Water 32-36%.

[0008] Optionally, the acrylic monomer is one or more of acrylic acid, methacrylic acid, crotonic acid, maleic acid, and itaconic acid; the inhibitor is one or more of hydroquinone, p-hydroxyanisole, p-benzoquinone, methylhydroquinone, 2-tert-butylhydroquinone, and 2,5-di-tert-butylhydroquinone.

[0009] Optionally, the emulsifier is an anionic surfactant or a nonionic surfactant; The initiator is one or more of ammonium persulfate, sodium persulfate, and potassium persulfate; The vinyl monomer is one or more of styrene, butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, glycidyl (meth)acrylate, acrylamide, diacetone acrylamide, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dibutyl maleate, vinyl triethoxysilane, and vinyl trimethoxysilane.

[0010] Butyl (meth)acrylate is butyl acrylate or butyl methacrylate, methyl (meth)acrylate is methyl acrylate or methyl methacrylate, ethyl (meth)acrylate is ethyl acrylate or ethyl methacrylate, hydroxyethyl (meth)acrylate is hydroxyethyl acrylate or hydroxyethyl methacrylate, glycidyl (meth)acrylate is glycidyl acrylate or glycidyl methacrylate, cyclohexyl (meth)acrylate is cyclohexyl acrylate or cyclohexyl methacrylate, and isobornyl (meth)acrylate is isobornyl acrylate or isobornyl methacrylate.

[0011] Optionally, the anionic surfactant is one or more of ammonium dodecyl sulfate, sodium dodecylbenzene sulfonate, alkylphenol polyoxyethylene ether sulfate, and fatty alcohol polyether sulfate, and the nonionic surfactant is one or more of OP (octylphenol polyoxyethylene ether) and NP (nonylphenol polyoxyethylene ether).

[0012] The silica sol described in the present application is prepared by at least one of a silica powder method, an ion exchange method, a direct acid neutralization method, an electrolytic dialysis method, and a sol-gel method.

[0013] Optionally, the preparation method of the lithium acrylate-silica sol precursor is to add a lithium hydroxide aqueous solution to a mixture of acrylic monomers, inhibitors and silica sol, the reaction temperature is 50-70° C., heat preservation, and cooling to obtain the lithium acrylate-silica sol precursor.

[0014] Optionally, the reaction temperature is 60° C., the adding method is dropwise addition, and the dropwise addition time is 1-3 h (preferably 2 h).

[0015] The preparation method of the mixture of acrylic monomer, inhibitor and silica sol is to stir the acrylic monomer, inhibitor and silica sol at a stirring speed of 40-100 rpm. The lithium hydroxide aqueous solution is obtained by stirring lithium hydroxide and water at a stirring speed of 40-100 rpm.

[0016] The embodiment of the present invention provides a method for preparing the concrete interface agent, wherein a pre-emulsifier and an initiator aqueous solution are simultaneously added to an emulsifier aqueous solution, the reaction temperature is 80-85°C, the mixture is kept warm, and the concrete interface agent is obtained by cooling; the pre-emulsifier is a mixture of a lithium acrylate-silica sol precursor, an emulsifier, an olefin monomer and water, and is preferably obtained by high-speed dispersion (300-800 r / min, time is 30 min).

[0017] Preferably, the reaction temperature is 82° C., the adding method is dropwise addition, and the dropwise addition time is 3-5 h.

[0018] An embodiment of the present invention provides an application of the concrete interface agent, wherein the concrete interface agent is used for repairing concrete.

[0019] The beneficial effect of the present invention is that the present invention uses acrylic monomers, silica sol and lithium hydroxide to prepolymerize to form lithium acrylate-silica sol prepolymer. Since the acidity of acrylic monomers is stronger than that of silica sol, lithium hydroxide reacts with acrylic monomers to form lithium acrylate monomers first, and silica sol can be more evenly distributed in latex particles during polymerization to form an organic-inorganic hybrid structure. An in-situ emulsion polymerization reaction is carried out using lithium acrylate-silica sol precursors and other olefin monomers to obtain a polyacrylate emulsion with an organic-inorganic structure. Since the ionic radius of lithium ions is small, they can penetrate deep into the surface layer of concrete to react with dicalcium silicate and free calcium oxide to solidify and form a dense solidified layer. The introduction of organic polyacrylate can greatly improve the toughness, density and water resistance of the solidified layer. DETAILED DESCRIPTION

[0020] Example 1 Lithium acrylate-silica sol precursor, the formula is shown in Table 1: Table 1 Components and ratios of Example 1

[0021] The preparation process is: 1. Add the formulated amount of acrylic acid, hydroquinone and silica sol into the reactor and start stirring at a speed of 50 rpm.

[0022] 2. Add deionized water to the high-level tank, then add lithium hydroxide, start stirring at a speed of 40 rpm until all the solids are dissolved to obtain a lithium hydroxide aqueous solution.

[0023] 3. Heat the reactor to 60°C and add the lithium hydroxide aqueous solution in the high-level tank dropwise for 2 hours. After the addition is complete, keep the reactor warm for 2 hours.

[0024] After the heat preservation is completed, the temperature is lowered to room temperature to obtain the lithium acrylate-silica sol precursor.

[0025] The preparation method of the concrete interface agent comprises the following steps: Pre-emulsification: 1) Add 29 parts of deionized water and 0.5 parts of emulsifier sodium dodecylbenzene sulfonate into the pre-emulsification kettle in sequence, start stirring and dissolve evenly; add 5 parts of styrene, 8 parts of butyl acrylate, 2 parts of acrylamide and 8 parts of lithium acrylate-silica sol precursor in turn, disperse at high speed for 30 minutes, fully emulsify, and rotate at 500r / min.

[0026] 2) Initiator dissolution: Add 1.8 parts of deionized water and 0.2 parts of ammonium persulfate into the header tank, stir and dissolve evenly; 3) Aggregation: Add 45 parts of deionized water and 0.5 parts of emulsifier sodium dodecylbenzene sulfonate into the reaction kettle, raise the temperature to 82±2°C, then start to drop the liquid in the pre-emulsification kettle and the high-level tank simultaneously, add it in 3 hours, then keep it warm for 3 hours, and finally cool it to room temperature to obtain the concrete interface agent.

[0027] Example 2 Lithium acrylate-silica sol precursor, the formula is shown in Table 2: Table 2 Components and ratios of Example 2

[0028] The preparation process is: 1. Add the formulated amount of methacrylic acid, p-hydroxyanisole and silica sol into the reaction kettle and start stirring at a speed of 75 rpm.

[0029] 2. Add deionized water to the high-level tank, then add lithium hydroxide, start stirring at a speed of 50 rpm until all the solids are dissolved to obtain a lithium hydroxide aqueous solution.

[0030] 3. Heat the reactor to 60°C and add the lithium hydroxide aqueous solution in the high-level tank dropwise for 2 hours. After the addition is complete, keep the reactor warm for 2 hours.

[0031] After the heat preservation is completed, the temperature is lowered to room temperature to obtain the lithium acrylate-silica sol precursor.

[0032] A method for preparing a concrete interface agent, comprising the following steps; Pre-emulsification: 1) Add 17 parts of deionized water, 1.3 parts of emulsifier ammonium dodecyl sulfate and 0.2 parts of OP-10 nonionic emulsifier into the pre-emulsification kettle in sequence, start stirring and dissolve evenly; add 2.5 parts of methyl methacrylate, 10.5 parts of butyl methacrylate, 3 parts of glycidyl methacrylate, 3 parts of diacetone acrylamide and 12 parts of lithium acrylate-silica sol precursor in turn, disperse at high speed for 30 minutes, fully emulsify, and rotate at 500r / min.

[0033] 2) Initiator dissolution: Add 2.8 parts of deionized water and 0.3 parts of ammonium persulfate into the header tank, stir and dissolve evenly; 3) Aggregation: 47 parts of deionized water and 0.5 parts of emulsifier ammonium dodecyl sulfate were added to the reaction kettle, and the temperature was raised to 82±2°C, and then the liquid in the pre-emulsification kettle and the high-level tank were added dropwise synchronously, and the addition was completed in 3.5 hours, and then the temperature was kept for 3 hours. Finally, the temperature was lowered to room temperature to obtain the concrete interface agent.

[0034] Example 3 Lithium acrylate-silica sol precursor, the formula is shown in Table 3: Table 3 Components and ratios of Example 3

[0035] The preparation process is: 1. Add the formulated amount of methacrylic acid, crotonic acid, p-hydroxyanisole and silica sol into the reaction kettle and start stirring at a speed of 80 rpm.

[0036] 2. Add deionized water to the high-level tank, then add lithium hydroxide, and start stirring at a speed of 50 rpm until all the solids are dissolved.

[0037] 3. Heat the reactor to 60°C and add the lithium hydroxide aqueous solution in the high-level tank dropwise for 2 hours. After the addition is complete, keep the reactor warm for 2 hours.

[0038] After the heat preservation is completed, the temperature is lowered to room temperature to obtain the lithium acrylate-silica sol precursor.

[0039] The preparation method of the concrete interface agent comprises the following steps: Pre-emulsification: 1) Add 20 parts of deionized water, 1.2 parts of emulsifier nonylphenol polyether ammonium sulfate and 0.3 parts of NP-15 nonionic emulsifier into the pre-emulsification kettle in turn, start stirring and dissolve evenly; add 7 parts of methyl methacrylate, 7 parts of isooctyl acrylate, 1 part of vinyl triethoxysilane, 1 part of N-hydroxymethyl acrylamide and 5 parts of lithium acrylate-silica sol precursor in turn, disperse at high speed for 30 minutes, fully emulsify, and rotate at 500r / min.

[0040] 2) Initiator dissolution: Add 1 part of deionized water and 0.1 part of ammonium persulfate into the header tank, stir and dissolve evenly; 3) Aggregation: Add 57.1 parts of deionized water and 0.3 parts of emulsifier ammonium nonylphenol polyether sulfate into the reaction kettle, heat it to 82±2°C, then start to drop the liquid in the pre-emulsification kettle and the high-level tank simultaneously, add it in 4 hours, then keep it warm for 3 hours, and finally cool it to room temperature to obtain the concrete interface agent.

[0041] Comparative Example 1 Compared with Example 1, the difference is that the lithium acrylate-silica sol precursor is replaced by acrylic acid, and the rest is the same as Example 1.

[0042] Comparative Example 2 Compared with Example 1, the difference is that the content of lithium hydroxide is 2% and the content of deionized water is 41.992%, and the rest is the same as Example 1.

[0043] Comparative Example 3 Compared with Example 1, the lithium acrylate-silica sol precursor is replaced by the following lithium silicate solution. The components and proportions of the lithium silicate are shown in Table 4.

[0044] Table 4 Components and ratios of Comparative Example 3

[0045] The preparation method is: 1. Add the formulated amount of silica sol into the reactor and start stirring at a speed of 50 rpm.

[0046] 2. Add deionized water to the high-level tank, then add lithium hydroxide, start stirring at a speed of 40 rpm until all the solids are dissolved to obtain a lithium hydroxide aqueous solution.

[0047] 3. Heat the reactor to 60°C and add the lithium hydroxide aqueous solution in the high-level tank dropwise for 2 hours. After the addition is complete, keep the reactor warm for 2 hours.

[0048] After the heat preservation is completed, the temperature is lowered to room temperature to obtain the lithium silicate solution.

[0049] The other steps are the same as in Example 1.

[0050] Comparative Example 4 The interface agent is prepared by physically mixing the commercially available emulsion Acronal ECO 7536 and a lithium silicate solution (the lithium silicate solution is the lithium silicate solution of Comparative Example 3) in a ratio of 2:1.

[0051] Comparative Example 5 The preparation method of the concrete interface agent comprises the following steps: Pre-emulsification: 1) Add 29 parts of deionized water and 0.5 parts of emulsifier sodium dodecylbenzene sulfonate into the pre-emulsification kettle in sequence, start stirring and dissolve evenly; add 5 parts of styrene, 8 parts of butyl acrylate, 2 parts of acrylamide and 8 parts of acrylic acid-silica sol mixture in turn, disperse at high speed for 30 minutes, fully emulsify, and rotate at 500r / min.

[0052] The acrylic acid-silica sol mixture is obtained by directly mixing the components and proportions shown in Table 1 of Example 1.

[0053] The other steps are the same as in Example 1.

[0054] The performance of the concrete interface agent of each embodiment and comparative example was tested to obtain a performance comparison table as shown in Table 5.

[0055] Table 5 Performance comparison of Examples 1 to 3 and Comparative Examples 1 to 5

[0056] The new concrete is a newly constructed concrete base material with no looseness, no powdering or falling off, and a hard and complete surface.

[0057] The old concrete is a repair concrete base material that has been used for more than 5 years, and the surface may be loose, powdered, and exposed. After the dust or loose surface layer is cleaned with a brush, it can be directly constructed.

[0058] As can be seen from Table 5, the adhesion of Examples 1-3 on the new concrete surface is greater than or equal to 2.4 MPa, and the adhesion on the old concrete surface is greater than or equal to 1.5 MPa. As can be seen from Comparative Example 1, by using conventional emulsion polymerization, without adding any inorganic nanomaterials, an adhesion of 1.2 MPa can be generated on the new concrete surface and 0.5 MPa on the old concrete surface. However, compared with Example 1, it is shown that the adhesion is greatly improved by using the lithium acrylate-silica sol precursor. Comparative Example 2 reduces the content of lithium hydroxide compared with Example 1, resulting in a decrease in adhesion. The reason is that the ionic radius of lithium ions is small, which can help latex particles penetrate deep into the surface of concrete to react with dicalcium silicate and free calcium oxide to solidify and form a dense solidified layer. The reduction in lithium ion content reduces the curing effect. Comparative Example 3 does not have acrylic acid to react to form a reactive lithium acrylate-silica sol precursor, which is equivalent to lithium silicate directly mixed in the emulsion. Its dispersion effect is not uniform, so it cannot improve adhesion. Comparative Example 4 is a physical cold splicing of ordinary polyacrylate emulsion and lithium silicate solution, and its effect should be equivalent to that of Comparative Example 3. However, from the test data, the adhesion of Comparative Example 4 on the new concrete surface is inferior to that of Comparative Example 3. This is because Comparative Example 3 is added dropwise into the emulsion during the reaction, and the dispersion effect is better than that of the physical cold splicing of Comparative Example 4.

[0059] A person skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of protection of the present application is limited to these examples. In line with the concept of the present application, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of different aspects of one or more embodiments of the present application as described above, which are not provided in detail for the sake of simplicity.

[0060] One or more embodiments of the present application are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the present application. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of one or more embodiments of the present application should be included in the protection scope of the present application.

Claims

1. A concrete interface agent, characterized in that: The composition comprises the following components in percentage by weight: Lithium acrylate-silica sol precursor 5-10%, Emulsifier 0.5-2%, Initiator 0.1-0.5%, Olefin monomer 10-20%, Water 67.5-80%; The lithium acrylate-silica sol precursor comprises the following components in percentage by weight: Acrylic monomer 15-25%, Inhibitor 0.005-0.01%, Lithium hydroxide 5-15%, Silica sol 35-45%, Water 30-40%.

2. The concrete interface agent according to claim 1, characterized in that: The composition comprises the following components in percentage by weight: Lithium acrylate-silica sol precursor 6-9%, Emulsifier 0.8-1.8%, Initiator 0.2-0.4%, Olefin monomer 12-18%, Water 70-79%; The lithium acrylate-silica sol precursor comprises the following components in percentage by weight: Acrylic monomer 18-22%, Inhibitor 0.008-0.01%, Lithium hydroxide 8-12%, Silica sol 32-36%, Water 32-36%.

3. The concrete interface agent according to claim 1 or 2, characterized in that: The acrylic monomer is one or more of acrylic acid, methacrylic acid, crotonic acid, maleic acid, and itaconic acid; the polymerization inhibitor is one or more of hydroquinone, p-hydroxyanisole, p-benzoquinone, methylhydroquinone, 2-tert-butylhydroquinone, and 2,5-di-tert-butylhydroquinone.

4. The concrete interface agent according to claim 1 or 2, characterized in that: The emulsifier is an anionic surfactant or a nonionic surfactant; The initiator is one or more of ammonium persulfate, sodium persulfate, and potassium persulfate; The vinyl monomer is one or more of styrene, butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, hydroxyethyl (meth)acrylate, glycidyl (meth)acrylate, acrylamide, diacetone acrylamide, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dibutyl maleate, vinyl triethoxysilane, and vinyl trimethoxysilane.

5. The concrete interface agent according to claim 4, characterized in that: The anionic surfactant is one or more of ammonium dodecyl sulfate, sodium dodecylbenzene sulfonate, alkylphenol polyoxyethylene ether sulfate, and fatty alcohol polyether sulfate, and the nonionic surfactant is one or more of OP and NP.

6. The concrete interface agent according to claim 1 or 2, characterized in that: The preparation method of the lithium acrylate-silica sol precursor is to add lithium hydroxide aqueous solution to a mixture of acrylic monomer, inhibitor and silica sol, the reaction temperature is 50-70° C., keep warm, and obtain the lithium acrylate-silica sol precursor after cooling.

7. The concrete interface agent according to claim 6, characterized in that: The reaction temperature is 60° C., the adding method is dropwise addition, and the dropwise addition time is 1-3 hours.

8. A method for preparing a concrete interface agent according to any one of claims 1 to 7, characterized in that: The pre-emulsifier and the initiator aqueous solution are added to the emulsifier aqueous solution simultaneously, the reaction temperature is 80-85°C, the temperature is kept, and the concrete interface agent is obtained by cooling; the pre-emulsifier is a mixture of lithium acrylate-silica sol precursor, emulsifier, olefin monomer and water.

9. The method for preparing a concrete interface agent according to claim 8, characterized in that: The reaction temperature is 82° C., the adding method is dropwise addition, and the adding time is 3-5 h.

10. An application of the concrete interface agent according to any one of claims 1 to 7, characterized in that: The concrete interface agent is used for repairing concrete.

Citation Information

Patent Citations

  • Hydrophobic acrylate polymer emulsion, concrete interface agent, and preparation methods of hydrophobic acrylate polymer emulsion and concrete interface agent

    CN109553717A

  • Penetration reinforced concrete interface agent, preparation method and application thereof

    CN115820053A