Pretreatment composition for bonding to metal substrate and preparation method thereof

By combining the graft copolymer pretreated composition with the aluminum alloy surface, a multifunctional surface coating is provided, which solves the problems of aluminum alloy in terms of corrosion, adhesion durability and weldability, and improves the overall performance of aluminum alloy.

CN119081499APending Publication Date: 2024-12-06NOVELIS INC(US)
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411205859.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-06-10
Filing Date
2021-06-09
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing pretreatment compositions cannot effectively solve a variety of surface-related problems associated with aluminum alloys, such as corrosion, poor adhesion durability, difficulty in separating stacked materials, uneven coating, and insufficient weldability and weld durability.

Method used

A graft copolymer pretreatment composition is used, which includes a polymer backbone, surface-bonded or bonded parts and multiple functional parts. It is bonded to the metal surface through covalent bonds, ionic bonds and other means to provide a multifunctional surface coating that enhances corrosion resistance, adhesion, lubricity and weldability.

Benefits of technology

It significantly improves the corrosion resistance, adhesion, lubricity, and weldability of aluminum alloy surfaces, thereby enhancing the overall performance and service life of aluminum alloy products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081499A_ABST
    Figure CN119081499A_ABST
Patent Text Reader

Abstract

The invention relates to a pretreatment composition for bonding to a metal substrate and a preparation method thereof. Described herein are graft copolymer pretreatment compositions that impart improved corrosion resistance, enhanced adhesion properties, lubrication, improved coating properties (e.g., enhanced wettability) and / or improved weldability and / or weld durability to metals (e.g., aluminum alloys), such as compared to unpretreated metal surfaces. Also provided herein are aluminum alloys coated with the disclosed graft copolymer pretreatment compositions, and methods for applying the disclosed graft copolymer pretreatment compositions to the aluminum alloys.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention application with patent application number 202180041667.4, application date June 9, 2021, and invention name “Pretreatment composition bonded to a metal substrate and preparation method thereof”.

[0002] CROSS-REFERENCE TO RELATED APPLICATIONS

[0003] This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 705,094, filed on June 10, 2020, which is incorporated herein by reference in its entirety. Technical Field

[0004] The present disclosure relates to the fields of materials science, materials chemistry, surface science, metal manufacturing, aluminum alloys and aluminum manufacturing. Compositions and methods that can be used for automotive, transportation, electronics, industrial and other applications are disclosed herein. Compositions and methods disclosed herein are particularly suitable for motor vehicles. Background Art

[0005] Aluminum alloys are often used in environments that may cause harmful effects to the surface or at least a portion of the surface of the aluminum alloy. Therefore, the aluminum alloy may suffer from corrosion, poor bonding durability, difficulty in separating stacked aluminum alloy products, uneven coatings, and poor weldability and / or welding durability. Many pretreatment compositions provide functions to solve single surface related problems. Therefore, it is desirable to incorporate a pretreatment composition of multiple surface functionalizations. Summary of the invention

[0006] The embodiments covered by the present invention are defined by the claims rather than by this summary. This summary is a high-level summary of various aspects of the present invention and introduces some concepts that are further described in the following detailed description. This summary is not intended to identify the key features or essential features of the claimed subject matter, nor is it intended to be used to determine the scope of the claimed subject matter in isolation. This subject matter should be understood with reference to appropriate portions of the entire specification, any or all of the drawings, and each claim.

[0007] Described herein are graft copolymer pretreatment compositions comprising: a polymer backbone; at least one surface binding or bonding portion (e.g., an anchoring group) attached to the polymer backbone and configured to bind or bond the polymer backbone to a first surface of the metal product; at least one functional portion attached to the polymer backbone and configured to provide at least a first surface functionalization to the first surface of the metal product; and at least one second functional portion attached to the polymer backbone and configured to provide at least a second surface functionalization to the first surface of the metal product, wherein the at least one functional portion and the at least one second functional portion provide a multi-functional surface coating.

[0008] In some examples, the polymer backbone includes an acrylic chain polymer structure, a methacrylic chain polymer structure, a vinyl chain polymer structure, a diene chain polymer structure, a vinylidene chain polymer structure, or any combination thereof. For example, the polymer backbone can be poly(methyl methacrylate), poly(ethyl methacrylate), poly(ethyl acrylate), polyacrylonitrile, polyethylene, polypropylene, polystyrene, poly(vinyl chloride), poly(vinyl acetate), poly(vinyl alcohol), polybutadiene, polyisoprene, polychloroprene, or any combination thereof.

[0009] In certain aspects, the at least one surface binding or bonding portion includes a phosphonate group, a carboxyl group, a catechol group or a trialkoxysilyl group. For example, the phosphonate group can be poly (vinyl phosphonate). In addition, the at least one functional portion includes an adhesion promoter (e.g., a hydroxyl group, an amide group, a thiol group, an epoxy group, a vinyl group, a diol group, an adhesive composition, a covalently bonded group or an ionically bonded group). In some cases, the at least one functional portion includes a polymer side chain that provides a lubricating function (e.g., polyethylene glycol, polytetrahydrofuran, polyisobutylene, polysilicone or any combination thereof). In some further cases, the at least one functional portion includes a humectant (e.g., polypropylene glycol, hexylene glycol, butanediol, lactic acid, sodium hexametaphosphate, glycerol, sorbitol, xylitol, maltitol, urea or any combination thereof). In some instances, the at least one functional portion includes a welding promoter.

[0010] In some cases, the at least one functional portion includes a corrosion inhibitor (e.g., an inorganic corrosion inhibitor, an inorganic barrier corrosion inhibitor, an organic corrosion inhibitor, an organic barrier corrosion inhibitor, or any combination thereof). For example, the inorganic corrosion inhibitor may include a transition metal, a transition metal salt, a rare earth metal, or a rare earth metal salt. In some cases, the transition metal includes titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), hafnium (Hf), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), or gold (Au), and / or a salt of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, Hf, Ta, W, Re, Os, Ir, Pt, or Au. In some examples, the rare earth metal includes cerium (Ce), scandium (Sc), yttrium (Y), lanthanum (La), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb) or lutetium (Lu), and / or a salt of Ce, Sc, Y, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu. In some aspects, the corrosion inhibitor includes an organic corrosion inhibitor such as mercaptobenzothiazole, benzotriazole, salicylaldehyde oxime, dithiooxamide, quinolic acid, thioacetamide or 8-hydroxyquinoline. In certain examples, the at least one second functional moiety comprises an adhesion promoter, a polymer side chain providing lubricity, a humectant, a welding accelerator, or a corrosion inhibitor.

[0011] In certain aspects, the graft copolymer pretreatment composition is crosslinked with a crosslinking agent (eg, a zirconium salt or a zirconium complex). Optionally, the crosslinking agent is an aqueous solution of a zirconium salt or a zirconium complex.

[0012] Also described herein is a method of pretreating at least a portion of a metal surface, comprising applying a graft copolymer pretreatment composition to at least a portion of the metal surface. In some cases, applying the graft copolymer pretreatment composition comprises coating at least a portion of the metal surface with a solution (e.g., rolling, dipping, coating, spin coating, or spraying at least a portion of the metal surface).

[0013] Other objects and advantages will become apparent from the following detailed description of non-limiting examples and formulae. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1is a graph showing the thickness of spin-coated films according to Examples described herein.

[0015] Figure 2 Atomic force microscopy (AFM) images of spin-coated thin films according to examples described herein are shown.

[0016] Figure 3 Shown are atomic force microscopy (AFM) images of spin-coated and washed thin films according to examples described herein.

[0017] Figures 4 to 6 X-ray photoelectron spectroscopy (XPS) scans are shown for thin films according to examples described herein.

[0018] Figure 7 Shown are film thicknesses of spin-coated samples of cross-linked polymer films according to examples described herein.

[0019] Figure 8 is a schematic diagram showing a cross-linked graft copolymer layer applied to an aluminum surface to form a polymer gel according to examples described herein, wherein Zr acts as a cross-linker for the phosphonic acid groups.

[0020] Fig. 9 X-ray photoelectron spectroscopy (XPS) scans are shown of films before and after cross-linking according to the examples described herein.

[0021] Figure 10 to Figure 11 Shown are the zirconium contents and corresponding tribological properties determined by XPS according to the examples described herein.

[0022] Figures 12 to 19 is a graph showing the coefficient of friction on films obtained by cyclic testing according to the Examples described herein.

[0023] Figure 20 to Figure 22 It was shown that the tribological performance of the polymer gel layers according to the examples described herein is dependent on the amount of polymer applied.

[0024] Fig.23 Shown are film thickness and tribological properties determined by ellipsometry at different storage conditions according to the Examples described herein.

[0025] Fig.24 is a graph showing water contact angle and lubricant contact angle of films according to examples described herein.

[0026] Figure 25 to Figure 26 is a graph showing the coefficient of friction of lubricated samples tested through cycles according to the Examples described herein.

[0027] Figures 27 to 30 is a graph showing the coefficient of friction of films tested through cycles according to the Examples described herein. DETAILED DESCRIPTION

[0028] Provided herein is a graft copolymer pretreatment composition that imparts functionalization to the surface of a metal (including an alloy, such as an aluminum alloy). Also provided herein is a metal (e.g., an aluminum alloy) coated with the disclosed graft copolymer pretreatment composition, and a method for applying the disclosed graft copolymer pretreatment composition to a metal. As used herein, pretreatment refers to surface modification, usually in the form of a solution or suspension, which is applied to a surface and converted into a layer by a physical reaction and / or a chemical reaction. The pretreatment layer is applied before the metal is subjected to processing or use (e.g., before a forming process, before the metal is placed in an outdoor environment for use, etc.). The pretreatment layer imparts features and performance characteristics that are significantly different from the metal body or metal surface. For example, the graft copolymer pretreatment composition and method described herein provide improved corrosion resistance for the metal surface, as compared to an unpretreated metal surface. In addition, the disclosed coating and method improve the corrosion resistance of metals (e.g., aluminum and aluminum alloys) under corrosive conditions, such as when put into use in automotive structural components and / or automotive body components.

[0029] In some cases, the graft copolymer pretreatment composition and method described herein impart enhanced adhesion properties to metal surfaces, such as compared to unpretreated metal surfaces. In some aspects, the graft copolymer pretreatment composition and method described herein provide lubrication for metal surfaces, such as compared to unpretreated metal surfaces. In some instances, the graft copolymer pretreatment composition and method described herein provide improved coating properties (e.g., enhanced wettability) for alloy surfaces, such as compared to unpretreated metal surfaces. In some cases, the graft copolymer pretreatment composition and method described herein improve the weldability and / or welding durability of metal surfaces, such as compared to unpretreated metal surfaces. In some aspects, the graft copolymer pretreatment composition and method described herein provide multifunctional surface coatings, which impart lubrication, corrosion resistance, enhanced adhesion properties, improved coating properties and / or improved weldability and / or welding durability, at least one of them.

[0030] Definition and Description:

[0031] The terms "invention," "the invention," "this invention," and "the present invention" as used herein are intended to refer broadly to all subject matter of this patent application and the appended claims. Statements containing these terms should not be construed as limiting the subject matter described herein or limiting the meaning or scope of the appended patent claims.

[0032] In this specification, reference is made to alloys identified by aluminum industry designations such as "Series" or "6xxx." To understand the most commonly used numerical designation systems for naming and identifying aluminum and its alloys, refer to "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Compositions Limits for Aluminum Alloys in the Form of Castings and Ingots," both published by The Aluminum Association.

[0033] As used herein, the meaning of "a", "an" or "the" includes both singular and plural referents unless the context clearly indicates otherwise.

[0034] As used herein, the thickness of a plate is generally greater than about 15 mm. For example, a plate can refer to an aluminum product having a thickness greater than about 15 mm, greater than about 20 mm, greater than about 25 mm, greater than about 30 mm, greater than about 35 mm, greater than about 40 mm, greater than about 45 mm, greater than about 50 mm, greater than about 100 mm, or up to about 200 mm.

[0035] As used herein, the thickness of the Saudi board (also referred to as a sheet board) is generally about 4 mm to about 15 mm. For example, the Saudi board can have a thickness of about 4 mm, about 5 mm, about 6 mm, about 7 mm, about 8 mm, about 9 mm, about 10 mm, about 11 mm, about 12 mm, about 13 mm, about 14 mm, or about 15 mm.

[0036] As used herein, sheet generally refers to an aluminum product having a thickness of less than about 4 mm. For example, the sheet can have a thickness of less than about 4 mm, less than about 3 mm, less than about 2 mm, less than about 1 mm, less than about 0.5 mm, less than about 0.3 mm, or less than about 0.1 mm.

[0037] Reference is made to alloy tempers or conditions in this application. For descriptions of the most commonly used alloy tempers, see "American National Standard (ANSI) H35 on Alloy and Temper Nomenclature System". The F condition or temper refers to aluminum alloys as fabricated. The O condition or temper refers to aluminum alloys after annealing. The Hxx condition or temper, also referred to herein as the H temper, refers to non-heat-treatable aluminum alloys that have been subjected to or not subjected to heat treatment (e.g., annealing) after cold rolling. Suitable H tempers include Hx1, Hx2, Hx3, Hx4, Hx5, Hx6, Hx7, Hx8, or Hx9 tempers. The T1 condition or temper refers to aluminum alloys that have been cooled from hot working and naturally aged (e.g., at room temperature). The T2 condition or temper refers to aluminum alloys that have been cooled from hot working, cold worked, and naturally aged. The T3 condition or temper refers to aluminum alloys that have been solution heat treated, cold worked, and naturally aged. The T4 condition or temper refers to aluminum alloys that have been solution heat treated and naturally aged. The T5 temper or temper refers to aluminum alloys that have been cooled from hot working and artificially aged (at elevated temperatures). The T6x temper or temper refers to aluminum alloys that have been solution heat treated and artificially aged. The T7 temper or temper refers to aluminum alloys that have been solution heat treated and artificially overaged. The T8x temper or temper refers to aluminum alloys that have been solution heat treated, cold worked, and artificially aged. The T9 temper or temper refers to aluminum alloys that have been solution heat treated, artificially aged, and cold worked. The W temper or temper refers to aluminum alloys that have been solution heat treated.

[0038] As used herein, "room temperature" may include temperatures from about 15°C to about 30°C, for example, about 15°C, about 16°C, about 17°C, about 18°C, about 19°C, about 20°C, about 21°C, about 22°C, about 23°C, about 24°C, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C or about 30°C.

[0039] All ranges disclosed herein should be understood to encompass any and all endpoints, as well as any and all subranges contained therein. For example, a specified range of "1 to 10" should be considered to include any and all subranges between a minimum of 1 and a maximum of 10 (and including 1 and 10); that is, all subranges start with a minimum of 1 or greater (e.g., 1 to 6.1) and end with a maximum of 10 or less (e.g., 5.5 to 10).

[0040] As used herein, terms such as "cast metal product", "cast product", "cast aluminum alloy product" and the like are used interchangeably and refer to products produced by direct chill casting (including direct chill co-casting) or semi-continuous casting, continuous casting (including, for example, by using a twin-belt caster, a twin-roll caster, a twin-block caster or any other continuous casting machine), electromagnetic casting, hot top casting or any other casting method.

[0041] The term "and / or", when used in a list of two or more items, means that any of the listed items can be taken alone or in combination with any one or more of the listed items. For example, the expression "A and / or B" means one or both of A and B, i.e., A alone, B alone, or A and B in combination. The expression "A, B, and / or C" means A alone, B alone, C alone, A and B in combination, A and C in combination, B and C in combination, or A, B, and C in combination.

[0042] As used herein, the term "surface functionalization" refers to methods and compositions used to alter the surface properties and / or characteristics of a material to obtain desired surface properties, including but not limited to corrosion resistance, enhanced adhesion, uniform wetting, accelerated drying, any other desired surface properties or characteristics, or any combination thereof.

[0043] As used herein, an acrylic chain polymer structure is formed by polymerizing a functionalized and / or unfunctionalized acrylate monomer (e.g., a monomer having the structure -CH2=CHCOOR) into a chain polymer; a methacrylic chain polymer structure is formed by polymerizing a functionalized and / or unfunctionalized methacrylate monomer (e.g., a monomer having the structure -CH2=CCH3COOR) into a chain polymer; a vinyl chain polymer structure is formed by polymerizing a functionalized and / or unfunctionalized vinyl monomer (e.g., a monomer having the structure -CH2=CH—R) into a chain polymer; a diene chain polymer structure is formed by polymerizing a functionalized and / or unfunctionalized diene monomer (e.g., a monomer having the structure -CH2=CR—CR'=CH2) into a chain polymer; and a vinylidene chain polymer structure is formed by polymerizing a functionalized and / or unfunctionalized vinylidene monomer (e.g., a monomer having the structure -C=CRR') into a chain polymer. In the above examples, R and R' are each independently selected from hydrogen, a functionalized or unfunctionalized alkyl substituent, a functionalized or unfunctionalized alkenyl substituent, a functionalized or unfunctionalized alkynyl substituent, any suitable substituent described herein, or any suitable polymer side chain.

[0044] As used herein, the terms alkyl, alkenyl, and alkynyl include straight and branched monovalent substituents. Examples include methyl, ethyl, isobutyl, 3-butynyl, and the like. The range of these groups useful in the compositions and methods described herein includes C1-C 20 Alkyl, C2-C 20 Alkenyl and C2-C 20 Alkynyl. Additional ranges of these groups useful in the compositions and methods described herein include C1-C 12 Alkyl, C2-C 12 Alkenyl, C2-C 12Alkyl, C1-C6 alkyl, C2-C6 alkenyl, C2-C6 alkynyl, C1-C4 alkyl, C2-C4 alkenyl and C2-C4 alkynyl.

[0045] Heteroalkyl, heteroalkenyl, and heteroalkynyl groups are defined similarly to alkyl, alkenyl, and alkynyl groups, but may contain O, S, or N heteroatoms, or combinations thereof, within the backbone. These groups useful in the compositions and methods described herein range from C1 to C 20 Heteroalkyl, C2-C 20 Heteroalkenyl and C2-C 20 Additional ranges of these groups useful in the compositions and methods described herein include C1-C 12 Heteroalkyl, C2-C 12 Heteroalkenyl, C2-C 12 C1-C6 heteroalkyl, C2-C6 heteroalkenyl, C2-C6 heteroalkynyl, C1-C4 heteroalkyl, C2-C4 heteroalkenyl and C2-C4 heteroalkynyl.

[0046] The terms cycloalkyl, cycloalkenyl, and cycloalkynyl include cycloalkyl groups having a single ring or multiple fused rings. Examples include cyclohexyl, cyclopentylethyl, and adamantyl. The range of these groups useful in the compositions and methods described herein includes C3-C 20 Cycloalkyl, C3-C 20 Cycloalkenyl and C3-C 20 Cycloalkynyl. Additional ranges of these groups useful in the compositions and methods described herein include C5-C 12 Cycloalkyl, C5-C 12 Cycloalkenyl, C5-C 12 cycloalkynyl, C5-C6 cycloalkyl, C5-C6 cycloalkenyl and C5-C6 cycloalkynyl.

[0047] Heterocycloalkyl, heterocycloalkenyl, and heterocycloalkynyl are defined similarly to cycloalkyl, cycloalkenyl, and cycloalkynyl, but may contain O, S, or N heteroatoms, or combinations thereof, within the backbone. These groups useful in the compositions and methods described herein range from C3 to C 20 Heterocycloalkyl, C3-C 20 Heterocycloalkenyl and C3-C 20 Heterocycloalkynyl. Additional ranges of these groups useful in the compositions and methods described herein include C5-C 12 Heterocycloalkyl, C5-C 12 Heterocycloalkenyl, C5-C 12 C5-C6 heterocycloalkynyl, C5-C6 heterocycloalkyl, C5-C6 heterocycloalkenyl and C5-C6 heterocycloalkynyl.

[0048] The term hydroxyl as used herein is represented by the formula—OH.

[0049] Aryl molecules include, for example, cyclic hydrocarbons incorporating one or more planar groups of six carbon atoms connected by delocalized electrons, which are numbered identically as if they were composed of alternating single covalent bonds and double covalent bonds. An example of an aryl molecule is benzene. Heteroaryl molecules include substitutions of atoms such as O, N, or S along the main cyclic chain of the heteroaryl molecule. Examples of heteroaryl molecules include furans, pyrroles, thiophene, imidazoles, oxazoles, pyridines, and pyrazines. Aryl and heteroaryl molecules may also include additional fused rings, such as benzofuran, indole, benzothiophene, naphthalene, anthracene, and quinoline. Unless otherwise indicated, aryl and heteroaryl molecules may be attached to any position on the ring.

[0050] As used herein, the term alkoxy is an alkyl group that is connected to the rest of the molecule by an oxygen atom. As used herein, the term aryloxy is an aryl group that is connected to the rest of the molecule by an oxygen atom. Likewise, as used herein, the terms alkenyloxy, alkynyloxy, heteroalkoxy, heteroalkenyloxy, heteroalkynyloxy, heteroaryloxy, cycloalkyloxy, and heterocycloalkyloxy are alkenyloxy, alkynyloxy, heteroalkoxy, heteroalkenyloxy, heteroalkynyloxy, heteroaryloxy, cycloalkyloxy, and heterocycloalkyloxy groups that are connected to the rest of the molecule by an oxygen atom, respectively.

[0051] Alkoxy, aryloxy, amino, alkyl, alkenyl, alkynyl, aryl, heteroalkyl, heteroalkenyl, heteroalkynyl, heteroaryl, cycloalkyl or heterocycloalkyl molecules used herein may be substituted or unsubstituted. As used herein, the term "substituted" includes the addition of alkoxy, aryloxy, amino, alkyl, alkenyl, alkynyl, aryl, heteroalkyl, heteroalkenyl, heteroalkynyl, heteroaryl, cycloalkyl or heterocycloalkyl groups to the position connected to the main chain of the alkoxy, aryloxy, amino, alkyl, alkenyl, alkynyl, aryl, heteroalkyl, heteroalkenyl, heteroalkynyl, heteroaryl, cycloalkyl or heterocycloalkyl, for example, by replacing hydrogen in one of these molecules. Examples of substituents include, but are not limited to, hydroxyl, halides (e.g., fluoride, chloride, bromide or iodide) and carboxyl groups. In contrast, as used herein, the term "unsubstituted" means that the alkoxy, aryloxy, amino, alkyl, alkenyl, alkynyl, aryl, heteroalkyl, heteroalkenyl, heteroalkynyl, heteroaryl, cycloalkyl or heterocycloalkyl group has a full quota of hydrogens, i.e., equivalent to its saturation level, without substitution, for example, linear decane (-(CH2)9-CH3).

[0052] Structures depicted herein encompass all enantiomeric, diastereomeric, and geometric (or conformational) forms of the structure; for example, R and S configurations for each asymmetric center, cis and trans isomers, (Z) and (E) double bond isomers and (Z) and (E) conformational isomers.

[0053] As used herein, the term "polymer" includes homopolymers and copolymers. A homopolymer refers to a polymer derived from a single polymerizable monomer. A copolymer refers to a polymer derived from two or more polymerizable monomers.

[0054] As used herein, a cross-linked polymer is defined as the presence of interchain linkages connecting two or more individual polymer chains. A cross-linked polymer may be permanently or temporarily cross-linked.

[0055] As used herein, a polymer gel is a substantially diluted cross-linked polymer. The polymer gel can be formed during polymerization of polymerizable monomers by adding a cross-linking agent or a small portion of a di(or multi)functional monomer in the presence of a solvent. Alternatively, cross-linking can be achieved in a subsequent step by applying a cross-linking agent to a suitable polymer incorporating cross-linkable functional groups. The latter can be implemented after further processing of the cross-linkable functional groups, including application as a film on a metal surface.

[0056] As used herein, a cross-linking agent can link two or more individual chains by reacting with appropriate functional groups in a polymer.

[0057] Pretreatment composition:

[0058] Graft copolymer pretreatment compositions are described herein, and in some instances, the graft copolymer pretreatment compositions are bonded to at least a portion of the surface of a metal product (including a metal alloy product, such as an aluminum alloy product). Although aluminum alloy products are described in the full text, the method and product are applicable to any metal. In some instances, the metal product can be aluminum, aluminum alloy, magnesium, magnesium-based materials, titanium, titanium-based materials, copper, copper-based materials, steel, steel-based materials, bronze, bronze-based materials, brass, brass-based materials, composite materials, sheets used in composite materials, or any other suitable metal or material combination. The metal product can include monolithic materials and non-monolithic materials, such as roll-bonded materials, cladding materials, composite materials or various other materials. In some instances, the metal product is a metal coil, a metal strip, a metal plate, a metal sheet, a metal billet, a metal ingot, etc.

[0059] In some non-limiting examples, the graft copolymer pretreatment compositions described herein include a polymer backbone, a side group portion that can bind or bond the graft copolymer pretreatment composition to a metal surface (i.e., a surface binding or bonding portion), and at least one functional side group portion (i.e., a functional portion) that can impart a functional pretreatment characteristic to the metal surface.

[0060] Polymer backbone

[0061] In some cases, the polymer backbone is an acrylic chain polymer structure, a methacrylic chain polymer structure, a vinyl chain polymer structure, a diene chain polymer structure, a vinylidene chain polymer structure, or any combination thereof. For example, the polymer backbone can be poly(methacrylic acid), poly(methyl methacrylate), poly(ethyl methacrylate), poly(acrylic acid), poly(methyl acrylate), poly(ethyl acrylate), poly(butyl acrylate), polyacrylonitrile, polyethylene, polypropylene, polystyrene, poly(vinyl chloride), poly(vinyl acetate), poly(vinyl alcohol), polybutadiene, polyisoprene, polychloroprene, or any combination thereof.

[0062] In some cases, the chain polymer structure can be prepared from vinyl-containing monomers to form a backbone according to the following Formula I:

[0063]

[0064] In Formula I, n is in the range of from 10 to 1000 (e.g., from 15 to 750, from 20 to 700, from 25 to 650, from 50 to 600, from 100 to 500, or from 200 to 400). Also in Formula I, R includes a functional portion that can impart functional pretreatment characteristics to the metal surface (e.g., the functional portion can be a corrosion inhibitor, an adhesion promoter, a polymer side chain that provides lubrication function (i.e., a lubricant and / or a lubricant functional portion), a humectant and / or a welding accelerator, as described below). Optionally, the functional portion can include an oxirane group, a phosphonic acid group, a hydroxyethyl group, a 2-methacryloyloxyethyl group, a 2,2,2-trifluoroethyl group, or a butyl group. Further functional groups that can be used in the graft copolymer pretreatment composition are described in detail below. In some cases, the functional moiety is attached to the backbone through a linker group such as a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, or a substituted or unsubstituted carbonyl (eg, a substituted or unsubstituted carboxyl).

[0065] In some cases, the chain polymer structure can be prepared from diene-containing monomers to form a backbone according to the following Formula II:

[0066]

[0067] In formula II, n is in the range of from 10 to 1000 (e.g., from 15 to 750, from 20 to 700, from 25 to 650, from 50 to 600, from 100 to 500 or from 200 to 400). Also in formula II, R includes a functional portion that can impart functional pretreatment characteristics to the metal surface (e.g., the functional portion can be a corrosion inhibitor, adhesion promoter, lubricant, moisturizer and / or welding promoter as described below). Optionally, the functional portion can include an oxirane group, a phosphonic acid group, a hydroxyethyl group, a 2-methacryloyloxyethyl group, a 2,2,2-trifluoroethyl group or a butyl group. Further functional groups that can be used for the graft copolymer pretreatment composition are described in detail below. In some cases, the functional portion is connected to the main chain through a linker group such as a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl or a substituted or unsubstituted carbonyl (e.g., a substituted or unsubstituted carboxyl). In some instances, one or more double bonds present in Formula II may be in the E-configuration. In some instances, one or more double bonds present in Formula II may be in the Z-configuration.

[0068] In some cases, the chain polymer structure can be prepared from acrylic acid or methacrylic acid containing monomers to form a backbone according to the following Formula III:

[0069]

[0070] In formula III, n is in the range of from 10 to 1000 (e.g., from 15 to 750, from 20 to 700, from 25 to 650, from 50 to 600, from 100 to 500 or from 200 to 400). Also in formula III, R includes a functional portion that can impart functional pretreatment characteristics to the metal surface (e.g., the functional portion can be a corrosion inhibitor, adhesion promoter, lubricant, humectant and / or welding promoter as described below). Optionally, the functional portion can include an oxirane group, a phosphonic acid group, a hydroxyethyl group, a 2-methacryloyloxyethyl group, a 2,2,2-trifluoroethyl group or a butyl group. Further functional groups that can be used for the graft copolymer pretreatment composition are described in detail below. In some cases, the functional portion is connected to the main chain through a linker group such as a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl or a substituted or unsubstituted carbonyl (e.g., a substituted or unsubstituted carboxyl). Furthermore, in Formula III, when the polymer is prepared from monomers containing acrylic acid, X is hydrogen. In Formula III, when the polymer is prepared from monomers containing methacrylic acid, X is methyl.

[0071] Surface binding or bonding part

[0072] As further described below, the surface binding or bonding part can bind or bond the chain polymer structure described herein to the metal surface through covalent bonds, ionic bonds, hydrogen bonds, dipole interactions or any combination thereof. In some aspects, the surface binding or bonding part is one or more reactive groups that can react with the metal surface and covalently bond to the metal surface. Reactive group examples may include, for example, phosphorus-containing parts (e.g., phosphoric acid, phosphonic acid), silicon-containing parts (e.g., siloxanes and silanes), sulfur-containing parts (e.g., sulfuric acid, sulfonic acid), carboxylic acids (e.g., acrylic acid, methacrylic acid) or metal hydrides, etc. In some cases, the reactive group may optionally be substituted with a substituent (e.g., another hydroxyl group) that can provide additional covalent bonding. For example, the hydroxyl functional group of the phosphorus-containing or silicon-containing part may react on the surface of the metal product, such as directly reacting with the metal atoms of the metal product to form a metal-oxygen-phosphorus bond or a metal-oxygen-silicon bond in a condensation reaction. Optionally, the reactive group of the graft copolymer pretreatment composition may react with the oxide surface layer of the metal product.

[0073] Functional part

[0074] In some aspects, the graft copolymer pretreatment composition described herein also includes at least one functional part to impart functionalization to the metal surface. For example, the at least one functional part can be an adhesion promoter, an adhesive, a lubricant, a humectant, a corrosion inhibitor, a welding promoter, or any combination thereof. In some instances, the graft copolymer pretreatment composition described herein includes an adhesion promoter functional part. In some instances, the adhesion promoter functional part can be a hydroxyl group, an amine group, a carboxylic acid group, an amide group, a thiol group, an epoxy group, a vinyl group, a diol group, or a combination thereof.

[0075] In some examples, the graft copolymer pretreatment composition described herein includes a lubricant functional portion. For example, the lubricant functional portion can be polyethylene glycol, polytetrahydrofuran, polyisobutylene, polybutadiene, polyisoprene, polysiloxane, or any combination thereof. The incorporation of a lubricant functional portion can destroy the surface tension between metal products stacked together, thereby improving the ability to de-stacking. In addition, the incorporation of a lubricant functional portion can reduce and / or stabilize the friction between, for example, the forming die and the sheet metal surface, thereby obtaining better formability, while reducing earing, reducing wrinkling and tearing rates, increasing processing speeds, reducing wear, extending tool life, and improving surface properties in the formed metal parts.

[0076] In some examples, the graft copolymer pretreatment composition described herein may include a humectant functional portion. For example, the humectant functional portion may be polypropylene glycol, hexylene glycol, butanediol, lactic acid, sodium hexametaphosphate, glycerol, sorbitol, xylitol, maltitol, urea, or any combination thereof. Incorporation of a humectant functional portion may disrupt the surface tension between the metal surface and certain aqueous solutions (e.g., additional pretreatment compositions, coatings, cleaning solutions, etc., or any combination thereof). In addition, incorporation of a humectant functional portion may provide a metal surface suitable for downstream coating processes, thereby achieving an efficient coating process, uniform coating coverage, and reduced coating waste.

[0077] In some examples, the graft copolymer pretreatment composition described herein includes a corrosion inhibitor functional part. In some cases, the corrosion inhibitor functional part is a galvanic corrosion inhibitor (e.g., an inorganic chemical corrosion inhibitor, an organic corrosion inhibitor, or any combination thereof), or a barrier corrosion inhibitor (e.g., an inorganic barrier corrosion inhibitor, an organic barrier corrosion inhibitor, or any combination thereof). In some aspects, the graft copolymer pretreatment composition described herein may include one or more inorganic chemical corrosion inhibitors. The inorganic chemical corrosion inhibitor for the pretreatment composition includes any inorganic chemical substance capable of chemically inhibiting or preventing aluminum alloy corrosion, such as forming different chemical substances (e.g., oxides) on the alloy surface by reaction and / or providing additional protection for the surface metal by embedding in the coating. In some cases, the graft copolymer pretreatment composition may optionally include an organic corrosion inhibitor. Non-limiting examples of suitable organic corrosion inhibitors include mercaptobenzothiazole (MBT), benzotriazole (BTA), salicylaldehyde oxime, dithiooxamide, quinalic acid, thioacetamide, 8-hydroxyquinoline (HXQ) and mixtures thereof.

[0078] In some examples, the inorganic chemical corrosion inhibitor as described herein includes one or more transition metals or salts thereof, and / or one or more rare earth metals or salts thereof. Suitable transition metals used as inorganic chemical corrosion inhibitors may include, for example, titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), hafnium (Hf), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt) or gold (Au). Suitable rare earth metals for use as inorganic chemical corrosion inhibitors may include, for example, cerium (Ce), scandium (Sc), yttrium (Y), lanthanum (La), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb) and lutetium (Lu).

[0079] Optionally, the inorganic chemical corrosion inhibitor is a transition metal salt or a rare earth metal salt. Optionally, the transition metal salt or rare earth metal salt includes a transition metal salt or a rare earth metal with an oxidation state of +1, +2, +3, +4, +5 or +6. For example, the transition metal salt or rare earth metal salt can be a salt including platinum II ions, platinum III ions, platinum IV ions, platinum V ions, platinum VI ions, zirconium II ions, zirconium III ions, zirconium IV ions, titanium II ions, titanium III ions, titanium IV ions, cerium II ions, cerium III ions or cerium IV ions. In some examples, the above-mentioned metal ions can be incorporated between at least two layers of the graft copolymer pretreatment compositions described herein to enhance corrosion resistance. For example, the graft copolymer pretreatment composition can be used to coat metal products to form a layer. Metal ions can be deposited on the graft copolymer pretreatment composition layer. Optionally, another layer of the graft copolymer pretreatment composition can be applied to the resulting product.

[0080] In some cases, the rare earth metal salt can be an anhydrous salt. In some cases, the rare earth metal salt can be a hydrated salt, such as a monohydrated salt, a dihydrated salt, a trihydrated salt, a tetrahydrated salt, a pentahydrated salt, a hexahydrated salt, a heptahydrated salt, an octahydrated salt, a nonahydrated salt and / or a decahydrated salt. In some instances, the rare earth metal salt is a rare earth metal nitrate. Examples of suitable inorganic chemical corrosion inhibitors include cerium (III) nitrate hexahydrate (Ce (NO3) 3 6H2O), yttrium nitrate hexahydrate (Y (NO3) 3 6H2O), ytterbium nitrate hexahydrate (Yb (NO3) 3 6H2O) and lanthanum nitrate hexahydrate (La (NO3) 3 6H2O).

[0081] In certain aspects, multiple layers of the graft copolymer pretreatment composition described herein can impart corrosion resistance to the metal surface. For example, the corrosion inhibition coating may include at least one first layer of a graft copolymer pretreatment composition comprising anionic functional groups (e.g., phosphonic acid) and at least one second layer comprising multivalent cations (e.g., any transition metal ions). Optionally, the multiple layers may include a third layer of a graft copolymer pretreatment composition comprising a phosphonic acid functional group. As used herein, multiple layers may refer to a series of thin films deposited on a metal surface. For example, multiple layers of graft copolymer pretreatment compositions may include a first layer deposited on a metal surface that completely covers the metal surface. Then, subsequent layers may be deposited on the first layer, thereby completely covering the first layer, and so on. In some cases, multiple layers may refer to the continuous deposition of multiple graft copolymer pretreatment composition layers, and the multiple layers form a single merged layer. The composition and morphology of the single merged layer may depend on the surface wettability of each of the graft copolymer pretreatment compositions, the miscibility of any solvent used to carry the graft copolymer pretreatment composition, or the design positioning of each layer in the multiple graft copolymer pretreatment composition layers. Thus, the metal surface can be pretreated with multiple layers of the graft copolymer pretreatment composition in a layer-by-layer configuration, in a mixture configuration, or in any desired film configuration.

[0082] In some examples, the graft copolymer pretreatment compositions described herein include a welding accelerator functional portion. Incorporation of the welding accelerator functional portion can disrupt surface tension between metal products that are in contact for a welding process (e.g., resistance spot welding, resistance seam welding, friction stir welding, gas metal arc welding (e.g., metal inert gas welding or tungsten inert gas welding), plasma arc welding, laser welding, refilled friction stir spot welding, any suitable welding process, or any combination thereof). In some embodiments, the welding accelerator functional portion may include titanium (Ti), zirconium (Zr), or a combination thereof.

[0083] In some examples, the graft copolymer pretreatment composition described herein comprises a crosslinkable functional portion. For example, the metal product can be coated with the graft copolymer pretreatment composition to form a layer. Subsequently, a crosslinking agent can be applied to form a covalent or non-covalent bond with the crosslinkable functional portion of the graft copolymer pretreatment composition layer connecting two or more individual polymer chains. Alternatively, a crosslinking precursor can be incorporated into the graft copolymer pretreatment composition and activated by an external stimulus (e.g., heat, light, pH, mechanical activation, etc.).

[0084] The crosslinking agent can be a small functional organic molecule (e.g., a bifunctional organic molecule) or a multifunctional organic molecule that reacts with the corresponding crosslinkable functional moieties in the graft copolymer pretreatment composition layer. Examples include, but are not limited to, 1,4-phenylene diacryl chloride or polyglycidyl ether cyclosiloxane (e.g., CS-697), which forms interchain linkages by reacting with hydroxyl or amino functional groups in the graft copolymer composition, with alkyl dithiols in the presence of disulfide bonds, and with poly(ethylene glycol) bisazide in the presence of alkynes.

[0085] Optionally, divalent or polyvalent metal ions can be applied to the graft copolymer pretreatment composition layer to crosslink suitable crosslinkable parts in the composition. The crosslinked parts formed in the presence of divalent or polyvalent metal ions include but are not limited to carboxylic acid, phosphonic acid and / or sulfonic acid groups. Inorganic chemical crosslinking agents as described herein include but are not limited to polyvalent metal cations (such as alkaline earth metals or their salts), and / or one or more transition metals or their salts, and / or one or more rare earth metals or their salts. The metal ions can be applied from a solution (including an aqueous solution) to cause instantaneous crosslinking. Suitable metals for use as inorganic chemical crosslinking agents may include, for example, beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), hafnium (Hf), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), or gold (Au). Suitable rare earth metals used as inorganic chemical corrosion inhibitors may include, for example, cerium (Ce), scandium (Sc), yttrium (Y), lanthanum (La), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb) and lutetium (Lu). Certain metal ions may provide multiple functions simultaneously, such as corrosion inhibition and crosslinking. In certain aspects, the crosslinking agent is a zirconium salt or a zirconium complex, for example, bis(acetylacetonate)zirconium.

[0086] Exemplary Graft Copolymer Pretreatment Compositions

[0087] In some examples, the graft copolymer pretreatment composition described herein, together with the binding or bonding part, can provide a multifunctional surface coating for the metal surface. In some cases, the graft copolymer pretreatment composition may include any combination of a binding or bonding part, a corrosion inhibitor functional part, an adhesion promoter functional part, a lubricant functional part, a humectant functional part, and / or a welding promoter functional part. For example, the graft copolymer pretreatment may include a binding or bonding part and a lubricant functional part. In some cases, the graft copolymer pretreatment may include a binding or bonding part and a corrosion inhibitor part. In some cases, the graft copolymer pretreatment may include a binding or bonding part and an adhesion promoting part. In some other cases, the graft copolymer pretreatment may include a binding or bonding part, a lubricant functional part, and an adhesion promoting part. In certain examples, the graft copolymer pretreatment may include a binding or bonding part, a lubricant functional part, and a humectant part. In addition, the graft copolymer pretreatment may include a binding or bonding part and a humectant part. Further, the graft copolymer pretreatment may include a binding or bonding part and a welding promoting part. In some non-limiting examples, the graft copolymer pretreatment may include a binding or bonding portion, a corrosion inhibiting portion, and an adhesion promoting portion. In certain aspects, the graft copolymer pretreatment may include a binding or bonding portion, a corrosion inhibiting portion, an adhesion promoting portion, and a lubricant functional portion. In some examples, the graft copolymer pretreatment may include a binding or bonding portion, a corrosion inhibiting portion, an adhesion promoting portion, and a welding promoting portion. In some aspects, the graft copolymer pretreatment may include a binding or bonding portion, a corrosion inhibiting portion, and a lubricant functional portion. These are some non-limiting examples, as the graft copolymer pretreatment may include any combination of a binding or bonding portion and any suitable functional portion.

[0088] An exemplary graft copolymer pretreatment composition as described herein, comprising a surface-bonding moiety and a functional moiety, is depicted in Formula IV below:

[0089]

[0090] In Formula IV, X 1 , X 2 , X 3 and X 4 Each is independently selected from hydrogen and methyl. Also in Formula IV, each of m, n, o and p is independently and optionally present in a range from 1 to 1000 (e.g., from 1 to 100, from 1 to 50, or from 1 to 30). In some examples, one or more of m, n, o and p is present (e.g., two of m, n, o and p are present; three of m, n, o and p are present; or each of m, n, o and p is present). In addition, in Formula IV, R 1 , R2 , R 3 and R 4 Each is independently selected from (if present) -O- or -NR 6 -, where R 6 is a substituted or unsubstituted alkyl, a substituted or unsubstituted alkenyl, a substituted or unsubstituted alkynyl, a substituted or unsubstituted aryl, a substituted or unsubstituted heteroaryl, a substituted or unsubstituted cycloalkyl or a substituted or unsubstituted heterocycloalkyl. 5 is a spacer group, such as (CH2) q , where q is in the range of 1 to 30 (e.g., q=1-30, q=1-25, q=1-20, q=1-15, q=1-10, q=1-5, q=5-30q=5-25, q=5-20, q=5-15, q=5-10q=10-30, q=10-25, q=10-20, q=10-15, q=15-30, q=15-25, q=15-20, q=20-30, q=20-25, or q=25-30).

[0091] In addition, in Formula IV, A is a surface binding or bonding moiety as described herein. Optionally, A is selected from the group consisting of: phosphonic acid (PO3H2), carboxylic acid (COOH), trialkoxysilyl (-Si(OR)3 (wherein R is alkyl, alkenyl, alkynyl, heteroalkyl, heteroalkenyl, heteroalkynyl, cycloalkyl, cycloalkenyl, cycloalkynyl, heterocycloalkyl, heterocycloalkenyl or heterocycloalkynyl)) and / or various catechol derivatives as shown in Formula V and Formula VI below:

[0092]

[0093] In Formula V and Formula VI, R 7 is selected from hydrogen, a hydroxyl group, an electron withdrawing group (eg, a nitro group, a carboxyl group, or a halide (eg, fluoride, chloride, bromide, or iodide)).

[0094] In some examples, Pol in Formula IV is an optionally present functional moiety. In some examples, Pol is a polymer chain that can be used as a lubricant, such as a poly(ethylene glycol) chain, a poly(tetrahydrofuran) chain, a poly(isoprene) chain, a hydrogenated poly(isoprene) chain, a poly(butadiene) chain, a hydrogenated poly(butadiene) chain, or a polyisobutylene chain.

[0095] In some cases, FG in formula IV is an optionally present functional moiety, wherein the functional moiety can be an adhesive compound or any other functional moiety as described herein. Optionally, FB can be a hydroxyl, amide, thiol, epoxide, vinyl, glycol, phosphonic acid, carboxylic acid, sulfonic acid, a polyvalent cation including any transition metal ion or any rare earth metal ion. In some non-limiting examples, when FG is a phosphonic acid, any one of a platinum ion, a zirconium ion or a titanium ion can be incorporated into the graft copolymer pretreatment composition. In some cases, FG can be a halide, ethylene oxide, a trialkoxysilyl group, a hydroxyethyl group, a 2-methacryloyloxyethyl group, a 2,2,2-trifluoroethyl group or a butyl group.

[0096] Aluminum alloy treated with graft copolymer pretreatment composition

[0097] Disclosed herein are metals and alloys, such as aluminum alloys, containing at least one surface treated with a graft copolymer pretreatment composition as described herein. The coatings described herein are suitable for providing corrosion protection, improved adhesion, lubrication, improved wetting, and / or improved welding properties to any metal or alloy (e.g., aluminum alloy). The graft copolymer pretreatment compositions disclosed herein may also be coatings, films, or layers. Although aluminum alloys are described and exemplified, the compositions and methods described herein may also be used to treat other metals and alloys, including mild steel, galvanized steel, and magnesium alloys, to name a few, as described above.

[0098] The disclosed coated metal and / or alloy has a surface coating layer, the surface coating layer comprising: a polymer backbone (e.g., a chain polymer polymerized from acrylic acid monomers or methacrylic acid monomers); at least one phosphonate bonding portion, which is connected to the polymer backbone and configured to bond the graft copolymer pretreatment composition to the metal and / or alloy surface; and at least one functional portion, which is connected to the polymer backbone and configured to impart surface functionalization to the metal and / or alloy surface. As described above, the surface functionalization includes corrosion resistance, improved adhesion, lubrication, improved wetting and / or improved welding performance.

[0099] Optionally, the method comprises the step of degreasing the surface of the aluminium alloy and / or etching the surface of the aluminium alloy prior to the coating being applied.The method may further comprise cleaning the aluminium alloy, rinsing the aluminium alloy and drying the aluminium alloy prior to applying the pretreatment solution.

[0100] In some examples, at least one surface of a metal and / or alloy (e.g., an aluminum alloy substrate, such as an aluminum alloy coil) can be coated by applying a graft copolymer pretreatment composition as described herein to the alloy to form an initial coating layer. The pretreatment composition can be applied to at least one surface of the aluminum alloy by any suitable method. In some cases, the graft copolymer pretreatment composition is coated by a solution containing the graft copolymer pretreatment composition (e.g., a graft copolymer pretreatment aqueous solution, a graft copolymer pretreatment organic solvent solution, or a combination thereof). For example, the coating described herein can be applied by roller coating, spraying, dipping, electrodeposition, glazing, or dripping a suitable graft copolymer pretreatment solution. These methods are generally known in the art.

[0101] Optionally, after applying the graft copolymer pretreatment solution, the graft copolymer pretreatment solution may be cured to form an aluminum alloy comprising a coating layer of the graft copolymer pretreatment composition. For example, curing the graft copolymer pretreatment solution may include heating the metal or alloy and / or the graft copolymer pretreatment solution to the glass transition temperature (Tg) of the polymer backbone. g ) to remove the residual solvent without causing any harmful effects on the graft copolymer pretreatment composition in the solution. After curing, the graft copolymer pretreatment composition becomes a coating layer having a desired graft copolymer pretreatment composition (e.g., including any one or any combination or all of the following: corrosion inhibitors, adhesion promoters, lubricants, moisturizers, welding promoters, hydrophobic functionality (e.g., self-cleaning surfaces and / or water-repellent surfaces), oleophobic functionality (e.g., antifouling surfaces), hydrophilic functionality (e.g., biocompatible surfaces), optical functionality (e.g., dyes, pigments, optical waveguides, photoluminescent surfaces, or negative refractive index surfaces), or any combination thereof).

[0102] Optionally, after applying the graft copolymer pretreatment solution, the polymer layer can be crosslinked by applying a crosslinking agent or a solution thereof by incubation, dipping, rolling, spraying or any suitable application technique. Crosslinking results in increased structural stability and robustness of the graft copolymer pretreatment composition layer. When in contact with a good solvent (usually water), the crosslinked polymer layer swells and forms a polymer gel layer. The polymer gel exhibits viscoelastic properties that can improve lubrication.

[0103] Optionally, the coated aluminum alloy can be part of a joined structure comprising the coated aluminum alloy and a second metal or alloy of different composition. For example, the coated aluminum alloy can be a 1xxx series alloy, a 2xxx series alloy, a 3xxx series alloy, a 4xxx series alloy, a 5xxx series alloy, a 6xxx series alloy, a 7xxx series alloy, or an 8xxx series alloy made from a cast aluminum alloy product joined to another alloy or metal.

[0104] Optionally, the aluminum alloy can be a 1xxx series aluminum alloy according to one of the following aluminum alloy designations: AA1100, AA1100A, AA1200, AA1200A, AA1300, AA1110, AA1120, AA1230, AA1230A, AA1235, AA1435, AA1145, AA1345, AA1445, AA1150, AA1350, AA1350A, AA1450, AA1370, AA1275, AA1185, AA1285, AA1385, AA1188, AA1190, AA1290, AA1193, AA1198 or AA1199.

[0105] Optionally, the aluminum alloy may be a 2xxx series aluminum alloy according to one of the following aluminum alloy designations: AA2001, A2002, AA2004, AA2005, AA2006, AA2007, AA2007A, AA2007B, AA2008, AA2009, AA2010, AA2011, AA2011A, AA2111, AA2111A, AA2111B, AA2012, AA2013, AA2014, A2015, A2016, A2017, A2018, A2019, A2020, A2021A, A2022B, A2023, A2024, A2025 A2014A, AA2214, AA2015, AA2016, AA2017, AA2017A, AA2117, AA2018, AA2218, AA2618, AA2618A, AA2219, AA2319, AA2419, AA2519, AA2021, AA2022, AA2023, AA2024, AA2024A, AA2124, AA2224, AA2224A, AA2324, A A2424, AA2524, AA2624, AA2724, AA2824, AA2025, AA2026, AA2027, AA2028, AA2028A, AA2028B, AA2028C, AA2029, AA2030, AA2031, AA2032, AA2034, AA2036, AA2037, AA2038, AA2039, AA2139, AA2040, AA2041, AA 2044, AA2045, AA2050, AA2055, AA2056, AA2060, AA2065, AA2070, AA2076, AA2090, AA2091, AA2094, AA20 95, AA2195, AA2295, AA2196, AA2296, AA2097, AA2197, AA2297, AA2397, AA2098, AA2198, AA2099 or AA2199.

[0106] Optionally, the aluminum alloy may be a 3xxx series aluminum alloy according to one of the following aluminum alloy designations: AA3002, AA3102, AA3003, AA3103, AA3103A, AA3103B, AA3203, AA3403, AA3004, AA3004A, AA3104, AA3204, AA3304, AA3005, AA3005A, AA3105, AA3105A, AA3105 ... AA3007, AA3107, AA3207, AA3207A, AA3307, AA3009, AA3010, AA3110, AA3011, AA3012, AA3012A, AA3013, AA3014, AA3015, AA3016, AA3017, AA3019, AA3020, AA3021, AA3025, AA3026, AA3030, AA3130, or AA3065.

[0107] Optionally, the aluminum alloy can be a 4xxx series aluminum alloy according to one of the following aluminum alloy designations: AA4004, AA4104, AA4006, AA4007, AA4008, AA4009, AA4010, AA4013, AA4014, AA4015, AA4015A, AA4115, AA4016, AA4017, AA4018, AA4019, AA4020, AA4021, AA4026, AA4032, AA4043, AA4043A, AA4143, AA4343, AA4643, AA4943, AA4044, AA4045, AA4145, AA4145A, AA4046, AA4047, AA4047A, or AA4147.

[0108] Optionally, the aluminum alloy can be a 5xxx series aluminum alloy according to one of the following aluminum alloy designations: AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA5119, AA5119A, AA5119B, AA5110C, AA5111D, AA5111E, AA5111F, AA5111F, AA5111F, AA5111F, AA5111F, AA5111G ... 021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA5049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA5251, AA5251A ,AA5351,AA5451,AA5052,AA5252,AA5352,AA5154,AA5154A,AA5154B,AA5154C,AA5254,AA5354,AA5454,AA5554 ,AA5654,AA5654A,AA5754,AA5854,AA5954,AA5056,AA5356,AA5356A,AA5456,AA5456A,AA5456B,AA5556,AA5556 A. AA5556B, AA5556C, AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182 , AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187 or AA5088.

[0109] Optionally, the aluminum alloy can be a 6xxx series aluminum alloy according to one of the following aluminum alloy designations: AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015, A A6016, AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA6 028, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA605 3. AA6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A , AA6261, AA6361, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092.

[0110] Optionally, the aluminum alloy may be a 7xxx series aluminum alloy according to one of the following aluminum alloy designations: AA7011, AA7019, AA7020, AA7021, AA7039, AA7072, AA7075, AA7085, AA7108, AA7108A, AA7015, AA7017, AA7018, AA7019A, AA7024, AA7025, AA70 28. AA7030, AA7031, AA7033, AA7035, AA7035A, AA7046, AA7046A, AA7003, AA7004, AA7005, A A7009, AA7010, AA7011, AA7012, AA7014, AA7016, AA7116, AA7122, AA7023, AA7026, AA7029, AA7129, AA7229, AA7032, AA7033, AA7034, AA7036, AA7136, AA7037, AA7040, AA7140, AA7041 ,AA7049,AA7049A,AA7149,AA7249,AA7349,AA7449,AA7050,AA7050A,AA7150,AA7250,AA7 7055, AA7055, AA7255, AA7056, AA7060, AA7064, AA7065, AA7068, AA7168, AA7175, AA7475, AA7076, AA7178, AA7278, AA7278A, AA7081, AA7181, AA7185, AA7090, AA7093, AA7095, or AA7099.

[0111] Optionally, the aluminum alloy may be an 8xxx series aluminum alloy according to one of the following aluminum alloy designations: AA8005, AA8006, AA8007, AA8008, AA8010, AA8011, AA8011A, AA8111, AA8211, AA8112, AA8014, AA8015, AA8016, AA8017, AA8018, AA8019, AA80210, AA8022 1. AA8021A, AA8021B, AA8022, AA8023, AA8024, AA8025, AA8026, AA8030, AA8130, AA8040, AA8050, AA8150, AA8076, AA8076A, AA8176, AA8077, AA8177, AA8079, AA8090, AA8091, or AA8093.

[0112] Optionally, the coated aluminum alloy can be provided in any metallurgical state, for example, any suitable temper or state. For example, the aluminum alloy can be provided in F temper, O temper or W temper as described above. In some cases, heat-treatable aluminum alloys (e.g., 2xxx series aluminum alloys, 6xxx series aluminum alloys, 7xxx series aluminum alloys and some 8xxx aluminum alloys) can be subjected to natural aging process and / or artificial aging process. As described herein, natural aging process includes storing the aluminum alloy that can be hardened at a temperature of about room temperature for a period of time to provide an aluminum alloy of T1 temper, T2 temper, T3 temper or T4 temper that is hardened by age. Optionally, the aluminum alloy that can be hardened by age can be subjected to artificial aging process, including heating the aluminum alloy to a high temperature lower than the liquidus temperature of the aluminum alloy, to provide an aluminum alloy of T5 temper, T6x temper, T7 temper, T8x temper or T9 temper that is hardened by age. In other examples, a strain-hardenable aluminum alloy (e.g., a 1xxx series aluminum alloy, a 3xxx series aluminum alloy, a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, and certain 8xxx series aluminum alloys) can be subjected to a strain hardening process to provide a strain-hardened Hxx tempered aluminum alloy as described above. As described herein, the strain hardening process includes cold working and optionally annealing the strain-hardenable aluminum alloy to provide a strain-hardened H tempered aluminum alloy (such as an Hx1 temper, an Hx2 temper, an Hx3 temper, an Hx4 temper, an Hx5 temper, an Hx6 temper, and an Hx7 temper, an Hx8 temper, or an Hx9 temper).

[0113] The aluminum alloy coated can be made into aluminum alloy products, including aluminum alloy plates, sheets or Saudi plates. In some instances, the alloy can be made into aluminum alloy sheets, which include graft copolymer coatings with any desired functionality as described herein. In some instances, the alloy can be made into a molded product formed by any aluminum alloy sheet as described herein and including any coating layer formed by graft copolymer pretreatment compositions as described herein. In some instances, the aluminum alloy is a molded product formed by any aluminum alloy sheet as described herein, and includes any graft copolymer coating as described herein, wherein the molded product is engaged with another product formed by different alloys or different metals (e.g., a second alloy or a second metal). In some non-limiting examples, the aluminum alloy and the second metal and / or alloy are bonded to form a joint of any suitable configuration (including lap joint, edge, butt joint, T-butt joint, hemming, T-edge, etc.).

[0114] The disclosed graft copolymer coatings and methods adjust the surface characteristics of aluminum and aluminum alloys. Aluminum alloys that may benefit from the protective coatings disclosed herein include those used in the automotive industry (e.g., automotive joints), manufacturing applications, electronic applications, industrial applications, and the like. Optionally, the alloy is part of a jointed structure such as, for example, the chassis of an automobile or other motor vehicle. The chassis may be in a body in white step or painted.

[0115] Polymer synthesis

[0116] The polymers used in the pretreatment compositions described herein can be prepared by polymerizing or copolymerizing suitable monomers to synthesize polymers having surface binding or bonding moieties and functional moieties by chain polymerization methods such as free radical polymerization, cationic polymerization, anionic polymerization, catalytic polymerization, or group transfer polymerization. In some cases, the polymer backbone is a homopolymer backbone provided by polymerizing a single type of repeating unit (e.g., a monomer). Optionally, the polymer backbone can be a copolymer backbone provided by polymerizing a plurality of different monomers by chain polymerization methods such as free radical polymerization, cationic polymerization, anionic polymerization, catalytic polymerization, or group transfer polymerization. Each repeating unit can include a surface binding or bonding moiety, a functional moiety, both a surface binding or bonding moiety and a functional moiety, or the repeating unit can be free of pendant functional moieties (e.g., a backbone spacer).

[0117] In some non-limiting cases, the polymers used in the pretreatment compositions described herein can be prepared by synthesizing a polymer backbone having a surface binding moiety and optionally a functional moiety by free radical polymerization or copolymerization of methacrylic acid or acrylic acid monomers such as methyl methacrylate, methacryloyloxy (methyl)phosphonic acid (MMPA), hydroxyethyl methacrylate (HEMA), or poly (ethylene glycol) methyl ether methacrylate (PEGMEMA). The number average molecular weight (M) of the poly (ethylene glycol) chain is 1000 Å. n ) can be, for example, in the range from 300 to 5000 (e.g., 300, 400, 700, 1000, 2000, or 5000).

[0118] In certain aspects, monomers (e.g., poly(ethylene glycol) methyl ether methacrylate, having M n=2000 (PEGMEMA-2000)), an initiator (e.g., ammonium persulfate (APS)) and a base (e.g., N,N,N',N'-tetramethylenediamine (TEMED)) in a predetermined stoichiometric ratio in a solvent (e.g., water, methanol, ethanol, isopropanol, n-butanol, dimethylformamide, dimethyl sulfoxide, acetonitrile, acetone, tetrahydrofuran, methyl ethyl ketone, or any combination thereof) for polymerization. In addition, copolymer polymerization can be performed using at least two monomers (e.g., PEGMEA-2000 and (methacryloyloxy)methylphosphonic acid (MMPA)), an initiator (e.g., APS) and a base (e.g., TEMED) in a predetermined stoichiometric ratio in a solvent as described above. An exemplary synthetic method for preparing a polymer for use in the pretreatment composition described herein is described in detail in Example 1 below.

[0119] How to use

[0120] The disclosed aluminum alloy products provided with the tempering described herein can be incorporated into existing processes and production lines for producing aluminum alloy products, such as hot-formed aluminum products (e.g., hot-formed automotive structural members), thereby improving the process and the resulting products in a streamlined and economical manner. Systems and methods for performing the forming processes and producing products described herein are included within the scope of the present disclosure.

[0121] The aluminum alloy products and processes can be advantageously used in the transportation industry, including but not limited to automobile manufacturing, truck manufacturing, ship and boat manufacturing, train manufacturing, aircraft manufacturing and spacecraft manufacturing. Some non-limiting examples of automotive parts include floor panels, rear walls, rockers, engine hoods, fenders, roofs, door panels, B-pillars, body sides, rockers or anti-collision members. As used herein, the term "automobile" and related terms are not limited to automobiles and include various vehicle categories, such as automobiles, cars, buses, motorcycles, marine vehicles, off-road vehicles, light trucks, trucks or vans. However, aluminum alloy products are not limited to automotive parts; it is envisioned that other types of aluminum products manufactured according to the process described in this application. For example, the process can be advantageously used to manufacture various parts of machinery and other devices or machines, including weapons, tools, the body of electronic devices and other parts and devices.

[0122] The aluminum alloy products and processes described herein can also be used in electronic applications to make, for example, external and internal packaging. For example, the alloys and methods described herein can also be used to make housings for electronic devices, including mobile phones and tablet computers. In some examples, the alloys can be used to make housings for mobile phones (e.g., smart phones) and outer covers for tablet chassis.

[0123] Description of suitable compositions, products and methods

[0124] Description 1 is a graft copolymer pretreatment composition, which comprises: a polymer backbone; at least one surface binding or bonding portion, which is connected to the polymer backbone and is configured to bind or bond the polymer backbone to the first surface of the metal product; at least one functional portion, which is connected to the polymer backbone and is configured to provide at least a first surface functionalization to the first surface of the metal product; and at least one second functional portion, which is connected to the polymer backbone and is configured to provide at least a second surface functionalization to the first surface of the metal product, wherein the at least one functional portion and the at least one second functional portion provide a multi-functional surface coating.

[0125] Description 2 is a graft copolymer pretreatment composition as described in any preceding or subsequent description, wherein the polymer backbone comprises an acrylic chain polymer structure, a methacrylic chain polymer structure, a vinyl chain polymer structure, a diene chain polymer structure, a vinylidene chain polymer structure, or any combination thereof.

[0126] Description 3 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the polymer backbone is poly(methyl methacrylate), poly(ethyl methacrylate), poly(ethyl acrylate), polyacrylonitrile, polyethylene, polypropylene, polystyrene, poly(vinyl chloride), poly(vinyl acetate), poly(vinyl alcohol), polybutadiene, polyisoprene, polychloroprene, or any combination thereof.

[0127] Description 4 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one surface binding or bonding moiety comprises a phosphonate group, a carboxyl group, a catechol group, or a trialkoxysilyl group.

[0128] Description 5 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the phosphonate group comprises poly(vinyl phosphonate).

[0129] Description 6 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one functional moiety comprises an adhesion promoter.

[0130] Description 7 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the adhesion promoter comprises a hydroxyl group, an amide group, a thiol group, an epoxy group, a vinyl group, a diol group, an adhesive composition, a covalent bonding group, or an ionically bonding group.

[0131] Description 8 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one functional moiety comprises a polymer side chain that provides a lubricating function.

[0132] Description 9 is a graft copolymer pretreatment composition as described in any preceding or subsequent description, wherein the polymer side chains providing lubricity function include polyethylene glycol, polytetrahydrofuran, polyisobutylene, polysilicone, or any combination thereof.

[0133] Description 10 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one functional moiety comprises a humectant.

[0134] Description 11 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the humectant comprises polypropylene glycol, hexylene glycol, butylene glycol, lactic acid, sodium hexametaphosphate, glycerin, sorbitol, xylitol, maltitol, urea, or any combination thereof.

[0135] Description 12 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one functional moiety comprises a welding accelerator.

[0136] Description 13 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one functional moiety comprises a corrosion inhibitor.

[0137] Description 14 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the corrosion inhibitor comprises an inorganic corrosion inhibitor, an inorganic barrier-type corrosion inhibitor, an organic corrosion inhibitor, an organic barrier-type corrosion inhibitor, or any combination thereof.

[0138] Description 15 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the corrosion inhibitor comprises an inorganic corrosion inhibitor, and wherein the inorganic corrosion inhibitor comprises a transition metal, a transition metal salt, a rare earth metal, or a rare earth metal salt.

[0139] Description 16 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the inorganic corrosion inhibitor comprises a transition metal, and wherein the transition metal comprises titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), zirconium (Zr), niobium (Nb), molybdenum (Mo), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), hafnium (Hf), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt) or gold (Au).

[0140] Description 17 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the inorganic corrosion inhibitor comprises a transition metal salt, and wherein the transition metal salt comprises a salt of Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, Hf, Ta, W, Re, Os, Ir, Pt or Au.

[0141] Description 18 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the inorganic corrosion inhibitor comprises a rare earth metal, and wherein the rare earth metal comprises cerium (Ce), scandium (Sc), yttrium (Y), lanthanum (La), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb) or lutetium (Lu).

[0142] Description 19 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the inorganic corrosion inhibitor comprises a rare earth metal salt, and wherein the rare earth metal salt comprises a salt of Ce, Sc, Y, La, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu.

[0143] Description 20 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the corrosion inhibitor comprises an organic corrosion inhibitor, and wherein the organic corrosion inhibitor comprises mercaptobenzothiazole, benzotriazole, salicylaldehyde oxime, dithiooxamide, quinalcoholic acid, thioacetamide or 8-hydroxyquinoline.

[0144] Description 21 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the at least one second functional moiety comprises an adhesion promoter, a polymer side chain providing lubricity, a humectant, a welding accelerator, or a corrosion inhibitor.

[0145] Description 22 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the graft copolymer pretreatment composition is crosslinked with a crosslinking agent.

[0146] Description 23 is a graft copolymer pretreatment composition of any preceding or subsequent description, wherein the crosslinking agent is a zirconium salt or a zirconium complex.

[0147] Description 24 is the graft copolymer pretreatment composition of any preceding or subsequent description, wherein the crosslinking agent is an aqueous solution of the zirconium salt or the zirconium complex.

[0148] Description 25 is a method of pretreating at least a portion of a metal surface, comprising: applying a graft copolymer pretreatment composition as described in any preceding or subsequent description to at least a portion of the metal surface.

[0149] Statement 26 is the method of any preceding or subsequent statement, wherein applying the graft copolymer pretreatment composition comprises solution coating at least the portion of the metal surface.

[0150] Description 27 is the method of any preceding description, wherein the solution coating comprises roller coating, dipping, coating, spin coating, or spraying at least the portion of the metal surface.

[0151] The following examples will be used to further illustrate the present invention, but do not constitute any limitation of the present invention. On the contrary, it should be clearly understood that, without departing from the spirit of the present invention, those skilled in the art can conceive of adopting various embodiments, modifications and their equivalent forms after reading the description herein.

[0152] Example

[0153] Example 1: Polymer Synthesis

[0154] Chemicals and materials used in polymer synthesis include number average molecular weight (M n ) is 2000 poly (ethylene glycol) methyl ether methacrylate (PEGMEMA-2000), M n 950 poly (ethylene glycol) methyl ether methacrylate (PEGMEMA-950), M n 500 poly (ethylene glycol) methyl ether methacrylate (PEGMEMA-500), M n The products were analyzed by gel permeation chromatography (GPC) and nuclear magnetic resonance (NMR) spectroscopy.

[0155]

[0156] Homopolymer 1a: poly(methacrylate)-grafted-poly(ethylene glycol). Polymerization was performed using PEGMEMA-2000, APS as initiator and TEMED as base in a stoichiometric ratio of 1.0 / 0.5 / 2.3 equivalents. PEGMEMA-2000 (0.6 g; 50 wt % aqueous solution, 0.15 mmol), 17.4 mg APS (0.076 mmol) and 3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. Then, TEMED (52 μL, 0.345 mmol) was added under positive argon pressure. The flask was resealed and the mixture was stirred at 400 revolutions per minute (rpm) for 2 hours at room temperature. Homopolymer 1a was obtained by freeze-drying.

[0157] Homopolymer 1b: poly(methacrylate)-grafted-poly(ethylene glycol). Polymerization was performed using PEGMEMA-2000 as monomer and 5 mol% V-501 as initiator. PEGMEMA-2000 (0.6 g; 50 wt% aqueous solution, 0.15 mmol), 2.1 mg V-501 (0.0075 mmol) and 3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 18 hours. Homopolymer 1b was obtained by freeze-drying.

[0158] Homopolymer 2a: poly(methacryloyloxy)methylphosphonic acid). The polymerization was carried out using MMPA monomer, APS as initiator and TEMED as base in a stoichiometric ratio of 1.0 / 0.5 / 2.3 equivalents. MMPA (0.3 g, 1.67 mmol), 193 mg APS (0.846 mmol) and 33.3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. TEMED (574 μL, 3.83 mmol) was added under positive argon pressure. The flask was resealed and the mixture was stirred at 400 rpm for 2 hours at room temperature. Homopolymer 2a was obtained by freeze-drying.

[0159] Homopolymer 2b: Poly(methacryloyloxy)methylphosphonic acid) 2b. Polymerization was performed using MMPA monomer and 5 mol% V-501 as initiator. MMPA (0.3 g, 1.67 mmol), 23.3 mg V-501 (0.0831 mmol) and 0.6 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 104 hours.

[0160] Homopolymer 2b was obtained by freeze-drying.

[0161]

[0162] Copolymer 3a: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-300 and MMPA in a stoichiometric ratio of 3.0 / 1.0 and V-501 as an initiator. PEGMEMA-300 (276 mg, 0.92 mmol), MMPA (55.8 mg, 0.31 mmol), V-501 (17.2 mg, 0.062 mmol) and 0.3 mL of methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3a was obtained by freeze-drying.

[0163] Copolymer 3b: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-300 and MMPA in a stoichiometric ratio of 1.0 / 1.0 and V-501 as initiator. PEGMEMA-300 (186 mg, 0.62 mmol), MMPA (111.7 mg, 0.62 mmol), V-501 (17.4 mg, 0.062 mmol) and 0.3 mL of methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3b was obtained by freeze-drying.

[0164] Copolymer 3c: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-300 and MMPA in a stoichiometric ratio of 1.0 / 3.0 and V-501 as an initiator. PEGMEMA-300 (108 mg, 0.36 mmol), MMPA (192.7 mg, 1.07 mmol), V-501 (20.0 mg, 0.072 mmol) and 0.3 mL of methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3c was obtained by freeze-drying.

[0165] Copolymer 3d: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-500 and MMPA in a stoichiometric ratio of 3.0 / 1.0 and V-501 as initiator. PEGMEMA-500 (267.8 mg, 0.54 mmol), MMPA (32.2 mg, 0.18 mmol), V-501 (10 mg, 0.034 mmol), 0.3 mL of methanol and 0.3 mL of water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging the volume above the solution with argon for 15 minutes, and then argon was bubbled through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3d was obtained by freeze-drying.

[0166] Copolymer 3e: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-500 and MMPA in a stoichiometric ratio of 1.0 / 1.0 and V-501 as initiator. PEGMEMA-500 (220.6 mg, 0.44 mmol), MMPA (79.4 mg, 0.44 mmol), V-501 (6.2 mg, 0.022 mmol), 0.3 mL methanol and 0.3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging the volume above the solution with argon for 15 minutes, and then argon was bubbled through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3e was obtained by freeze-drying.

[0167] Copolymer 3f: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-500 and MMPA in a stoichiometric ratio of 1.0 / 3.0 and V-501 as initiator. PEGMEMA-500 (144.2 mg, 0.29 mmol), MMPA (155.8 mg, 0.87 mmol), V-501 (8.1 mg, 0.029 mmol), 0.15 mL of methanol and 0.15 mL of water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging the volume above the solution with argon for 15 minutes, and then argon was bubbled through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 24 hours. Copolymer 3f was obtained by freeze-drying.

[0168] Copolymer 3g: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-950 and MMPA in a stoichiometric ratio of 3.0 / 1.0 and V-501 as an initiator. PEGMEMA-950 (282.2 mg, 0.30 mmol), MMPA (17.8 mg, 0.099 mmol), V-501 (5.5 mg, 0.020 mmol), 0.8 mL of methanol and 0.8 mL of water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging the volume above the solution with argon for 15 minutes, and then argon was bubbled through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3g was obtained by freeze-drying.

[0169] Copolymer 3h: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-950 and MMPA in a stoichiometric ratio of 1.0 / 1.0 and V-501 as initiator. PEGMEMA-950 (252.2 mg, 0.27 mmol), MMPA (47.8 mg, 0.27 mmol), V-501 (3.7 mg, 0.013 mmol), 0.8 mL of methanol and 0.8 mL of water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging the volume above the solution with argon for 15 minutes, and then argon was bubbled through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 3h was obtained by freeze-drying.

[0170] Copolymer 3i: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-950 and MMPA in a stoichiometric ratio of 1.0 / 3.0 and V-501 as initiator. PEGMEMA-950 (191.2 mg, 0.20 mmol), MMPA (108.8 mg, 0.60 mmol), V-501 (5.6 mg, 0.020 mmol), 0.4 mL methanol and 0.4 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging the volume above the solution with argon for 15 minutes, and then argon was bubbled through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 24 hours. Copolymer 3i was obtained by freeze-drying.

[0171] Copolymer 3j: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-2000 and MMPA in a stoichiometric ratio of 3.0 / 1.0 and 0.7 wt % V-501 as initiator. PEGMEMA-2000 (600 mg, 50 wt % aqueous solution, 0.15 mmol), 9 mg MMPA (0.05 mmol), 2.2 mg V-501 (0.0078 mmol) and 3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 80 hours. Copolymer 3j was obtained by freeze-drying.

[0172] Copolymer 3k: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-2000 and MMPA in a stoichiometric ratio of 1.0 / 1.0 and 0.7 wt % V-501 as initiator. PEGMEMA-2000 (600 mg, 50 wt % aqueous solution, 0.15 mmol), 27 mg MMPA (0.15 mmol), 2.3 mg V-501 (0.0082 mmol) and 3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 80 hours. Copolymer 3k was obtained by freeze-drying.

[0173] Copolymer 31: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-2000 and MMPA in a stoichiometric ratio of 1.0 / 3.0 and 0.7 wt % V-501 as initiator. PEGMEMA-2000 (600 mg, 50 wt % aqueous solution, 0.15 mmol), 81.1 mg MMPA (0.45 mmol), 2.7 mg V-501 (0.0096 mmol) and 3 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. The flask was placed in a preheated oil bath at 70° C. and the mixture was stirred at 400 rpm for 80 hours. Copolymer 31 was obtained by freeze-drying.

[0174] Copolymer 3m: poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-2000 and MMPA, using APS as initiator and TEMED as base in a stoichiometric ratio of 3.0 / 1.0 / 2.0 / 9.2. PEGMEMA-2000 (583 mg, 50 wt % aqueous solution, 0.146 mmol), 8.7 mg MMPA (0.0485 mmol), 22.5 mg APS (0.0987 mmol) and 3.9 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. Then, TEMED (67 μL, 0.446 mmol) was added under positive argon pressure. The flask was resealed and the mixture was stirred at 400 rpm for 2 hours at room temperature. Copolymer 3m was obtained by freeze-drying.

[0175] Copolymer 3n: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-2000 and MMPA, using APS as initiator and TEMED as base in a stoichiometric ratio of 1.0 / 1.0 / 1.0 / 4.6. PEGMEMA-2000 (550 mg, 50 wt % aqueous solution, 0.138 mmol), 24.8 mg MMPA (0.138 mmol), 31.9 mg APS (0.140 mmol) and 5.5 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. TEMED (95 μL, 0.633 mmol) was added under positive argon pressure. The flask was resealed and the mixture was stirred at 400 rpm for 2 hours at room temperature. Copolymer 3n was obtained by freeze-drying.

[0176] Copolymer 3o: Poly(methacryloyloxymethylphosphonic acid)-co-(methacrylate-grafted-poly(ethylene oxide)). Polymerization was performed using monomers PEGMEMA-2000 and MMPA, using APS as initiator and TEMED as base in a stoichiometric ratio of 1.0 / 3.0 / 2.0 / 9.2. PEGMEMA-2000 (472 mg, 50 wt % aqueous solution, 0.118 mmol), 63.8 mg MMPA (0.354 mmol), 54.8 mg APS (0.240 mmol) and 9.4 mL water were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and the solution was subjected to three freeze-pump-thaw cycles. Then, TEMED (162.8 μL, 1.09 mmol) was added under positive argon pressure. The flask was resealed and the mixture was stirred at 400 rpm for 2 hours at room temperature. Copolymer 3o was obtained by freeze-drying.

[0177] Copolymer 4: Poly(hydroxyethyl methacrylate)-co-(methacryloyloxymethylphosphonic acid). Polymerization was performed using monomers HEMA and MMPA in a stoichiometric ratio of 3.0 / 1.0 and 5 mol% V-501 as an initiator. HEMA (300 mg, 2.31 mmol), 136 mg MMPA (0.77 mmol), 41.3 mg V-501 (0.147 mmol) and 2 mL methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging with argon for 15 minutes, followed by bubbling argon through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 4 was obtained by precipitation in n-hexane.

[0178]

[0179] Copolymer 5: Poly(2-methacryloyloxyethylphosphorylcholine)-co-(methacryloyloxymethylphosphonic acid). Polymerization was performed using monomers MPC and MMPA in a stoichiometric ratio of 3.0 / 1.0 and 5 mol% V-501 as initiator. MPC (300 mg, 1.02 mmol), 61 mg MMPA (0.339 mmol), 19 mg V-501 (0.068 mmol) and 0.8 mL methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging with argon for 15 minutes, followed by bubbling argon through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 5 was obtained by precipitation in acetone.

[0180] Copolymer 6: Poly(2,2,2-trifluoroethyl methacrylate)-co-(methacryloyloxymethylphosphonic acid). Polymerization was performed using monomers TFEMA and MMPA in a stoichiometric ratio of 3.0 / 1.0 and 5 mol% V-501 as initiator. TFEMA (300 mg, 1.78 mmol), 107 mg MMPA (0.595 mmol), 33.3 mg V-501 (0.119 mmol) and 0.8 mL methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging with argon for 15 minutes, followed by bubbling argon through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 6 was obtained by precipitation in n-hexane.

[0181]

[0182] Copolymer 7: Poly(butyl methacrylate)-co-(methacryloyloxymethylphosphonic acid). Polymerization was performed using monomers BMA and MMPA in a stoichiometric ratio of 3.0 / 1.0 and 5 mol% V-501 as an initiator. BMA (300 mg, 2.10 mmol), 126.7 mg MMPA (0.703 mmol), 39.3 mg V-501 (0.140 mmol), 0.4 mL isopropanol and 0.6 mL methanol were added to a Schlenk flask equipped with a magnetic stirring bar. The flask was sealed and deoxygenated by purging with argon for 15 minutes, followed by argon bubbling through the solution for 5 minutes. The flask was placed in a preheated oil bath at 70°C and the mixture was stirred at 400 rpm for 72 hours. Copolymer 7 was obtained by precipitation in methanol / water (1:1, v / v).

[0183] Example 2: Coating a Metal Product with a Pretreatment Solution

[0184] Analytical instruments and methods :

[0185] Water contact angle measurement. Water contact angle was measured using DataPhysics OCA 35 water contact angle measurement system (Dataphysics, San Jose, CA, USA). Droplets of liquid and lubricant (1 μL each) were deposited on the substrate and equilibrated for 10 seconds. The contact angle was calculated based on the drop shape using the Young-Laplace equation.

[0186] Ellipsometry analysis of dry film thickness. The dry film thickness was determined using a variable angle spectroscopic ellipsometer (Semilab SE2000, Semilab ZRt, Budapest, Hungary). The ellipsometric data were recorded at angles of incidence of 65°, 70° and 75° using a wavelength range of 245 nm–990 nm. The ellipsometric data, i.e. the angles Ψ and Δ, were analyzed using the software provided with the instrument (Spectroscopic Ellipsometry Analyzer v1.6.1 (Semilab)). The calculation method is based on a five-layer silicon / silicon oxide / aluminum oxide / polymer brush / surrounding environment model, assuming that the polymer brush layer is isotropic and homogeneous. The refractive index (n) of the polymer brush layer was approximated by the Cauchy approximation (n = A n +B n / λ 2 ) and fitted by the layer thickness by software. All reported ellipsometric film thicknesses on silicon wafers were corrected for an approximately 1.5 nm thick native oxide layer on the silicon substrate and a 10 nm aluminum oxide layer grown by atomic layer deposition (ALD).

[0187] Atomic force microscopy (AFM). AFM imaging was performed in tapping mode (AC Airtopography) on a Cypher VRS platform (Asylum Research, Oxford Instruments, Oxford, United Kingdom) using a HQ-NSC18 / Al BS silicon cantilever (resonance frequency f = 60–90 kHz, force constant k = 1.2–5.5 N / m). The oscillation of the cantilever was driven by photothermal excitation. A 2.5 Hz scan rate was used and the analysis area was 2 μm × 2 μm.

[0188] Friction analysis by nanotribometer. TTX, STeP–NTR 3 The instrument (Nano Tribometer, Anton Paar GmbH, Graz, Austria) was compared with ST-S (maximum normal and friction load, F n , F t =100mN) or HL-S (maximum F n , F t =1N) cantilever was used for friction measurement. Nanotribology tests were performed on polymer coated silicon / alumina wafers using a 100Cr6 ball with a diameter of 2 mm at loads of 1 mN, 10 mN, 100 mN (using ST-S cantilever) and 300 mN (using HL-S cantilever). The sliding distance was 2 mm at 0.8 Hz (maximum linear velocity 5 mm / s) in 500 cycles. No additional lubricant was used.

[0189] Coating Procedure :

[0190] Spin coating is performed to evaluate the graft copolymer coating on the aluminum oxide layer applied to the silicon wafer as a model substrate. The spin-coated substrate (e.g., silicon wafer or wafer coated with aluminum oxide) is ultrasonically treated for 5 minutes in acetone and isopropanol respectively. Then, the wafer is rinsed with isopropanol and blown dry with argon. Subsequently, the wafer is placed in an oxygen plasma generator, which is powered to 92W under a 10mL / min oxygen flow for 5 minutes. The cleaned wafer is spin-coated with an aqueous solution of 2 wt %, 5 wt % and 10 wt % of homopolymer 2a of 10 μL. Spin coating is performed for 5 minutes at 1000rpm and 2000rpm, and performed for 1 minute at 4000rpm and 8000rpm to evaluate the spin coating characteristics. The coated wafer is then placed on a heating stage preheated to 70°C and dried for 2 hours. The sample is stored in ambient atmosphere and analyzed by water contact angle measurement and spectral ellipsometry. The thickness of the 2 wt% spin-cast solution was in the range of 5 nm - 15 nm, the thickness of the 5 wt% spin-cast solution was in the range of 20 nm - 55 nm, and the thickness of the 10 wt% spin-cast solution was in the range of 35 nm - 95 nm. Ellipsometry measurements were performed within one week after coating.

[0191] Figure 1 The figure shows the polymer dry film thickness of three solutions of homopolymer 2a in water with concentrations of 2 wt%, 5 wt% and 10 wt% as a function of the spin coating speed (in Figure 1 The film thickness scales well with the theoretical dependence indicated by the dashed line (i.e., the film thickness is proportional to the inverse square root of the rotation speed, d = A·w). (-1 / 2) , where d is the film thickness, w is the rotation speed, and A is the rotation duration).

[0192] Copolymer 3j, copolymer 3k and copolymer 3l were spin coated onto an alumina layer on a silicon wafer to evaluate the film thickness. The wafer cleaned as described above was spin coated with 10 μL of a 2 wt % aqueous solution of copolymer 3j, copolymer 3k and copolymer 3l at 2000 rpm for 5 minutes and at 4000 rpm and 8000 rpm for 1 minute. The coated wafer was then placed on a heating stage preheated to 70°C and dried for 2 hours. The samples were stored in an ambient atmosphere and analyzed by water contact angle measurement, spectroscopic ellipsometry and atomic force microscopy. The thickness of the spin-cast solution was in the range of 5.3 nm-8.2 nm at 2000 rpm, in the range of 14.9 nm-48.3 nm at 4000 rpm, and in the range of 15.2 nm-35.9 nm at 8000 rpm. These values ​​are similar to those obtained from the atomic force microscopy step analysis, in which part of the copolymer coating was removed by scraping with a sharp steel needle (see Figure 2 and Figure 3 ). Figure 2 AFM images of substrates spin coated with 2 wt% aqueous solution of copolymer 3j are shown. The cross section indicates copolymer coating from 33.7 nm - 43.6 nm. Figure 3 AFM images of substrates spin coated with a 2 wt% aqueous solution of copolymer 3j and subsequently washed with water are shown. The cross section indicates a copolymer coating from 8.8 nm - 9.3 nm thick.

[0193] Copolymer 3a, copolymer 4, copolymer 5, copolymer 6 and copolymer 7 were spin coated onto an aluminum oxide layer on a silicon wafer to evaluate film thickness. The cleaned wafer was spin coated with 50 μL of a 2 wt % aqueous solution of polymer 3a, copolymer 4, copolymer 5, copolymer 6 and copolymer 7 at 8000 rpm for 1 minute. The coated wafer was then placed on a heating stage preheated to 70° C. and dried for 10 minutes. The samples were stored in ambient atmosphere and the polymer coating thickness was evaluated by spectroscopic ellipsometry as shown in Table 1 below:

[0194] Table 1

[0195] Polymer coating Thickness(nm) Copolymer 3a 27.5±3.0 Copolymer 4 24.5±2.8 Copolymer 5 29.96±0.85 Copolymer 6 56.1±2.1 Copolymer 7 70.72±0.36

[0196] In addition, copolymer 3a, copolymer 4, copolymer 5, copolymer 6 and copolymer 7 were spin-coated on a clean aluminum oxide layer on a silicon wafer at 8000 rpm for 1 minute. The coated wafer was then placed on a heating stage preheated to 70° C. and dried for 10 minutes. Then, the sample was immersed in water (copolymer 3a, 4 and 5) or isopropanol (copolymer 6 and 7) for 15 minutes, then rinsed with their respective solvents, then rinsed with isopropanol, and dried with argon. The sample was stored in an ambient atmosphere, and the film thickness was evaluated by spectral ellipsometry, as shown in Table 2 below:

[0197] Table 2

[0198] Polymer coating Thickness(nm) Copolymer 3a 9.66±0.25 Copolymer 4 5.13±0.40 Copolymer 5 7.22±0.62 Copolymer 6 7.4±1.5 Copolymer 7 3.99±0.28

[0199] Copolymer 3a, Copolymer 3b and Copolymer 3c, which were spin-coated onto an aluminum oxide layer on a silicon wafer, were analyzed by X-ray photoelectron spectroscopy (XPS) with high resolution scanning of C1s, P 2s and P 2p to confirm the presence of the copolymer. Figures 4 to 6 It shows that copolymer 3a ( Figure 4 ), copolymer 3b( Figure 5 ) and copolymer 3c( Figure 6 ) film. Deconvoluted C1s scan ( Figures 4 to 6 The left panel of each figure in FIG. 1 indicates the presence of aliphatic carbon atoms (signal at 285 eV), carbon atoms in the PEG chain (signal at 286.3 eV), and carbonyl atoms of the methacrylate group belonging to the polymer backbone (signal at 289 eV). The phosphorus scan shows a peak at 191 eV in the P2s scan and a peak at 134 eV in the P 2p scan. The P 2s region ( Figures 4 to 6 The central graph of each graph in Figures 4 to 6 The phosphorus scan intensity in the right panel of each figure in the Figure 1 scales well with increasing amounts of phosphonic acid in the copolymer sample (i.e., copolymer 3b has twice the P signal of copolymer 3a, and copolymer 3c has three times the P signal of copolymer 3a).

[0200] Copolymer 3h was spin-coated onto the alumina layer on the silicon wafer to evaluate the film thickness of the polymer gel layer. The wafer cleaned as described above was spin-coated with 40 μL of 2 wt % of copolymer 3h in a 9:1 methanol-water mixture at 2500rpm, 5000rpm, 7000rpm and 8000rpm for 1 minute. Subsequently, the silicon wafer was incubated for 1 hour in a solution of 5mM bis(acetylacetone) zirconium in ethanol. The zirconium ions cross-link the phosphonic acid functional groups in the copolymer and form a polymer gel layer. After rinsing with ethanol, the silicon wafer was spin-dried at 8000rpm for 30 seconds. The resulting film thickness determined by ellipsometry was 58.6 ± 1.9nm at 2500rpm, 42.5 ± 1.2 at 5000rpm, 38.8 ± 1.4nm at 7000rpm and 38.1 ± 1.4 at 8000rpm, respectively.

[0201] Copolymer 3h was spin coated onto an aluminum oxide layer on a silicon wafer and onto a 5754 aluminum sample (e.g., 5754EDT aluminum) pretreated with EDT (tetrahydroacridine derivative) at 8000 rpm for one minute as described above. The thickness of the polymer layer was controlled by varying the polymer concentration in the spin coating solution (ranging from 0.38 wt % to 3.0 wt % in a methanol-water mixture (9:1). After spin coating, the sample was incubated for 1 hour in a 5 mM solution of zirconium bis(acetylacetonate) in ethanol to crosslink. The sample was rinsed with ethanol and spin dried at 8000 rpm for 10 seconds. Figure 7 Table 3 shows how the gel layer thickness is related to the polymer concentration in the spin coating step. The thickness of the polymer gel layer can be controlled by the polymer concentration in the spin coating step. Figure 8 is a schematic diagram of the polymer gel layer. Fig. 9 and Table 4 shows cross-linking (in Fig. 9 before ( Fig. 9 , above) and after ( Fig. 9 , lower figure), indicating the presence of zirconium cross-linking.

[0202] Table 3

[0203] Concentration of polymer solution (wt%) Thickness(nm) 0.38 17.0±0.5 0.75 33.6±0.3 1.5 65.7±1.6 3.0 158.2±2.8

[0204] Table 4

[0205]

[0206] Crosslinking of the spin-coated layers of copolymer 3h with zirconium ions was typically achieved by incubation at room temperature for up to 15 minutes at concentrations in the millimolar range. For zirconium concentrations in the sub-millimolar range, the thickness of the polymer gel layer decreased significantly after rinsing, indicating that a sufficient degree of crosslinking was not achieved to form a structurally stable polymer gel layer. The reduction in polymer gel layer thickness was also reflected in the reduction in sliding distance in the nanotribology experiments. Higher concentrations did not further improve the stability of the polymer gel layer ( Fig.10 and Table 5). After incubation in a 5 mM zirconium bis(acetylacetonate) (Zr(acac)4) solution in ethanol for 1 min at room temperature, a stable polymer gel layer was formed. XPS data showed that crosslinking was complete after a maximum of 15 min ( Fig.11 and Table 6). At longer incubation times, no significant increase in zirconium content was observed. For the non-crosslinked comparative sample, a significant decrease in polymer layer thickness was observed after rinsing, indicating that a significant amount of polymer was removed from the surface during the rinsing step in the absence of crosslinking zirconium ions.

[0207] Table 5

[0208]

[0209]

[0210] Table 6

[0211] Incubation time (min) Thickness(nm) XPS (Zr3d / P2p) 0 15.3±0.4 0.05 1 131.5±1.8 0.86 15 135±3 1.26 60 129.3±2.1 0.95 420 125.9±2.3 1.04

[0212] Crosslinking with zirconium bis(acetylacetonate) can also be achieved by immersion in aqueous solution. Fig.19 The tribological properties of polymer gel layers under a normal load of 300 mN are shown, which are prepared by crosslinking a 239 nm copolymer 3h layer spin-coated on 5457EDT aluminum in a 5 mM solution of bis(acetylacetonate) zirconium in ethanol in water at pH 6.19 and a slightly acidic aqueous solution at pH 4.56, respectively. In the latter solution, the pH value is reduced by adding a small amount of sulfuric acid. Lower pH values ​​are conducive to the solubility and stability of bis(acetylacetonate) zirconium in aqueous solution, which is shown by the enhanced tribological properties of the surface modified by the corresponding polymer gel. The decomposition products can form a precipitate on the surface and cause an increase in the initial friction coefficient and a reduction in the sliding distance, as seen in the polymer gel prepared in water at pH 6.19. Application from aqueous solution is an important factor for environmental and economic aspects.

[0213] Example 3: Coating properties

[0214] The homopolymer 2a films were analyzed by nanotribology to determine the coefficient of friction of the coated surface. Nanotribology testing was performed on an aluminum oxide layer on a silicon wafer coated with homopolymer 2a using the method described above. Nanotribology testing was performed at forces of 100 mN, 10 mN, and 1 mN. Fig.12 Nanotribology results are shown for wafers coated with a 4.6 nm thick film and a 2.3 nm thick film. The 4.6 nm thick film and the 2.3 nm thick film were tested for 500 cycles at a force of 100 mN. Fig.12 As shown, both the 4.6 nm thick film and the 2.3 nm thick film provided a friction coefficient (μ) of about 0.7, which remained unchanged over 500 cycles. Fig.13 Nanotribology results are shown for a wafer coated with a 30.6 nm thick film. The 30.6 nm thick film was tested for 500 cycles at a force of 10 mN. Fig.13 As shown, the 30.6 nm thick film provides an unstable friction coefficient over 500 cycles. Fig.14 is a graph comparing nanotribology results for wafers coated with a 30.6 nm thick film, a 4.6 nm thick film, and a 2.3 nm thick film. The 30.6 nm thick film, the 4.6 nm thick film, and the 2.3 nm thick film were tested for 500 cycles at a force of 1 mN. The 4.6 nm thick film and the 2.3 nm thick film exhibit lower coefficients of friction and greater stability than the thicker 30.6 nm film. Fig.14As shown, both the 4.6 nm thick film and the 2.3 nm thick film provided a friction coefficient less than about μ=0.4 and remained constant over 500 cycles, and the 30.6 nm thick film provided a higher and unstable friction coefficient over 500 cycles.

[0215] Copolymer 3a, Copolymer 4, Copolymer 5, Copolymer 6 and Copolymer 7 films were analyzed by nanotribology to determine the coefficient of friction of the coated surface and the maximum sliding distance of the initial coefficient of friction. Nanotribology testing was performed on an aluminum oxide layer on a silicon wafer coated with Copolymer 3a, Copolymer 4, Copolymer 5, Copolymer 6 and Copolymer 7 using the method described above. Nanotribology testing was performed at 300 mN ( Fig.15 and Fig.17 ) and 100mN( Fig.16 and Fig.18 All of these tests showed an initial low coefficient of friction, followed by a rapid increase, indicating mechanical damage to the coating.

[0216] Fig.15 and Fig.16 Performance is shown for spin-coated films with thicknesses of 24nm–71nm. Fig.17 and Fig.18 The performance of spin-coated films with a thickness of 24nm-71nm is shown, and the spin-coated films are further subjected to a washing step to remove unbound and / or excess copolymer material. Under both 300mN and 100mN forces, the films containing copolymer 3a showed a lower initial friction coefficient of 0.15 for tests performed under a normal load of 300mN and 0.2 for tests performed under a normal load of 100mN. Similarly, the copolymer 3a film maintained its lowest friction coefficient over a longer sliding distance, 43cm for tests performed under a load of 100mN for the spin-coated film and 10cm for tests performed under a load of 300mN. These results indicate that the copolymers described herein have surprisingly good performance, assuming that the film thickness is nanometer-sized and there is no additional lubricant. Films containing copolymers without grafted PEG chains showed consistently poor performance. After washing the excess copolymer, the test (see Fig.17 and Fig.18 ) shows negligible effect on the lowest friction coefficient. In the 100 mN test (see Fig.17 ), the maximum sliding distance of the copolymer 3a film decreased from 43 cm to about 23 cm. In contrast, in the 300 mN test (see Fig.18 ), this distance does not decrease. Surprisingly, at 300 mN, the thicker coating appears to play little role and the performance is determined solely by the stronger connecting layer.

[0217] The copolymer 3a ( Fig.24"PEGMEMA300-MMPA"), copolymer 4 ( Fig.24 referred to as "HEMA-MMPA"), copolymer 5 ( Fig.24 referred to as "MPC-MMPA"), copolymer 6 ( Fig.24 referred to as "FEMA-MMPA") and copolymer 7 ( Fig.24 The water contact angle of the film (referred to as "BMA-MMPA") Fig.24 “WCA”) and the contact angle of lubricant AL200 ( Fig.24 The measured values ​​are referred to as "AL200 CA" in the figure, and their comparison is shown in Fig.24 The water contact angle of copolymer 3a is about 60°. For copolymer 5 including a highly polar zwitterionic comonomer component, a water contact angle of about 42° was observed.

[0218] A film of copolymer 3a with a 9.66 nm coating was lubricated with AL200 by spin coating with a 1 wt % solution of AL200 in isopropanol at 8000 rpm for 1 min. The thickness of the lubricated surface was approximately 54 nm as assessed by spectroscopic ellipsometry. In addition, a reference substrate not coated with the polymer was lubricated in a similar manner. The lubricated samples were analyzed by nanotribology to determine the coefficient of friction of the coated surface and the maximum sliding distance of the initial coefficient of friction (see Fig.25 and Fig.26 ). At 100mN( Fig.25 and Fig.26 The left figure of each figure), 300mN( Fig.25 and Fig.26 Each figure is the second one from the left), 600mN( Fig.25 and Fig.26 Each figure in the third one from the left) and 1000mN ( Fig.25 and Fig.26 Nanotribology tests were performed under a force of 100 mN (right figure of each figure in FIG). For all samples, the initial friction coefficient was about 0.1. After a certain sliding distance, the friction coefficient increased rapidly to about 0.7, indicating that the AL200 lubricant was removed. For copolymer 3a films, this maximum sliding distance at low friction coefficients was generally much higher. For example, at 100 mN, the sliding distance increased from 600 cm-800 cm to more than 1200 cm; for 300 mN, it increased from 100 cm to more than 600 cm; for 600 mN, no increase was observed; for 1000 mN, an increase from 0 cm-50 cm to 200 cm-230 cm was observed.

[0219] The effects of chemical structural features (such as PEG chain length and density of phosphonic acid anchoring groups) on the coating properties were systematically investigated by nanotribological analysis of copolymer 3a, copolymer 3b, copolymer 3c, copolymer 3d, copolymer 3e, copolymer 3h, and copolymer 3k films. The nanotribological tests were performed at 300 mN ( Fig. 27 and Fig.29 ) and 100mN( Fig.28 and Fig.30 ) shall be executed under the power of

[0220] Fig. 27 and Fig.28 It shows that copolymer 3a ( Figure 27 to Figure 28 The left column), copolymer 3b ( Figure 27 to Figure 28 center column) and copolymer 3c ( Figure 27 to Figure 28 (right column in Figure 5) Tribological properties of films composed of copolymer chains synthesized using PEGMEMA-300 and increasing amounts of MMPA (molar ratios of 3:1, 1:1, and 1:3). These films provided only moderate lubrication because the initial friction coefficients of these substrates were above 0.3 for tests under a normal load of 100 mN. In addition, the maximum sliding distances at these lower friction coefficients were mostly below 10 cm. Increasing the amount of phosphonic acid methacrylate bound within the copolymer chains did not improve these distances, but instead reduced performance because the initial friction coefficient increased from 0.3 at the lowest phosphonic acid content to 0.5 at the highest phosphonic acid content. During testing at a higher load of 300 mN, these effects were slightly lower (e.g., the initial friction coefficient increased from 0.2 at the lowest phosphonic acid content to 0.4 at the highest phosphonic acid content, and the maximum sliding distance was only slightly affected).

[0221] Fig.29 and Fig.30 The copolymer 3d( Figure 29 to Figure 30 in the left column) and copolymer 3e ( Figure 29 to Figure 30 The tribological properties of copolymers 3d and 3e at the initial friction coefficient were significantly improved when the amount of phosphonic acid anchoring groups was increased to 50 mol%. For the spin-coated samples, the maximum sliding distance increased from about 10 cm to 25 cm. Copolymers 3h ( Figure 29 to Figure 30 The third one from the left column) and copolymer 3k ( Figure 29 to Figure 30(middle right column). Copolymer 3h films exhibited similar maximum sliding distances compared to copolymer 3d and copolymer 3e, but showed a lower initial friction coefficient of 0.1 compared to 0.2 for copolymer 3e films. Further increasing the length of the PEG chain did not lead to further improvements, as the initial friction coefficient remained approximately 0.1 and the maximum sliding distance of the spin-coated samples decreased from 20 cm to 10 cm.

[0222] Fig.21 The tribological properties of zirconium-crosslinked polymer gel films of copolymer 3h are shown, the thickness of which was applied by roller coating from an aqueous polymer solution. 5754EDT aluminum sheets of size 210×297 mm (A4) were coated. The sheets were dried at 35°C for 5 minutes and then incubated in a 5mM solution of zirconium bis(acetylacetonate) in ethanol for 1 hour at room temperature. Polymer concentrations of 2.22 wt%, 1.11 wt%, 0.55 wt% and 0.28 wt% in water were used, and zirconium-crosslinked polymer gel films of copolymer 3h with thicknesses ranging from 16.5 nm to 147 nm were achieved. Prior to performing nanotribological measurements, the sheets were rinsed with ethanol and dried at room temperature. A force of 300 mN normal load was applied to the film. This example shows that the polymer can be applied from an aqueous solution using techniques commonly used in large-scale production. Fig.21 The tribological properties under a normal load of 300 mN were shown. The films showed an initial coefficient of friction (COF, μ) < 0.2. The sliding distance ranged between 11.7 cm for a 16.5 nm thick polymer gel layer and 71 cm for a 128 nm thick polymer gel layer. These results indicate that the copolymers described herein have good lubrication properties, assuming that the film thickness is in the nanometer range and that no additional lubricant is present.

[0223] The storage stability of polymer gels prepared from copolymer 3h was studied under the following conditions: up to 72 h in a lyophilizer, up to 64 h in an oven at 60 °C, and up to 1 month under ambient conditions ( Fig.23 ). The thickness of the polymer gel layer during storage was monitored by ellipsometry using alumina-coated silicon wafers as substrates, and the tribological performance was monitored by applying a normal load of 300 mN using 5754EDT aluminum as substrate. Fig.23 As can be seen in the Figures, the tribological properties do not significantly decrease when stored under ambient conditions and are not compromised even under high vacuum conditions of up to 72°C in the freeze dryer. At elevated temperatures, for example, when stored in an oven at 60°C for 64 hours, the tribological properties decrease after incubation for more than one hour. The lubricity properties are unacceptable after 64 hours of incubation. The samples were not rewetted or otherwise treated prior to the tribological measurements. The presented data demonstrate the favorable storage stability of the polymer gels.

[0224] Layered structures can be achieved by repeating the spin coating and cross-linking steps multiple times. The copolymer 3h was spin-coated onto an alumina-coated silicon wafer and subsequently cross-linked by incubation in a 5 mM zirconium bis(acetylacetonate) solution in ethanol. This two-step procedure was repeated up to two more times. Fig. 22 , the nanotribological performance of an applied force of 300 mN normal load is shown after one (second panel from the left), two (third panel from the left), and three (rightmost panel) applications.

[0225] All patents, patent applications, publications and abstracts cited above are incorporated herein by reference in their entirety. Reference has been made in detail to various embodiments of the disclosed subject matter, one or more examples of which have been set forth above. Each example is provided by way of explanation of the subject matter, not limitation. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the subject matter without departing from the scope or spirit of the present disclosure. For example, a feature illustrated or described as part of one example may be used together with another example to produce yet another example.

Claims

1. A graft copolymer pretreatment composition comprising: polymer backbone; at least one surface binding or bonding moiety attached to the polymer backbone and configured to bind or bond the polymer backbone to a surface of a metal product; and A functional moiety is attached to the polymer backbone and is configured to provide at least one surface functionalization to the surface of the metal product.

2. The graft copolymer pretreatment composition of claim 1, wherein the polymer backbone comprises an acrylic chain polymer structure, a methacrylic chain polymer structure, a vinyl chain polymer structure, a diene chain polymer structure, a vinylidene chain polymer structure, or any combination thereof.

3. The graft copolymer pretreatment composition of claim 1 or 2, wherein the polymer backbone is poly(methyl methacrylate), poly(ethyl methacrylate), poly(ethyl acrylate), polyacrylonitrile, polyethylene, polypropylene, polystyrene, poly(vinyl chloride), poly(vinyl acetate), poly(vinyl alcohol), polybutadiene, polyisoprene, polychloroprene, or any combination thereof.

4. The graft copolymer pretreatment composition of any one of claims 1 to 3, wherein the at least one surface binding or bonding moiety comprises a reactive group.

5. The graft copolymer pretreatment composition of claim 4, wherein the reactive group comprises a phosphorus-containing moiety, a silicon-containing moiety, a sulfur-containing moiety, a carboxylic acid, or a metal hydride.

6. The graft copolymer pretreatment composition of claim 5, wherein the reactive group comprises a phosphorus-containing moiety, and wherein the phosphorus-containing moiety comprises phosphoric acid.

7. The graft copolymer pretreatment composition of any one of claims 4-6, wherein the reactive groups are substituted.

8. The graft copolymer pretreatment composition of any one of claims 1 to 3, wherein the at least one surface binding or bonding moiety comprises a phosphonate group, a carboxyl group, a catechol group, or a trialkoxysilyl group.

9. The graft copolymer pretreatment composition of claim 8, wherein the phosphonate groups comprise poly(vinyl phosphonate).

10. The graft copolymer pretreatment composition of any one of claims 1 to 9, wherein the at least one functional moiety comprises an adhesion promoter.

11. The graft copolymer pretreatment composition of claim 10, wherein the adhesion promoter comprises a hydroxyl group, an amide group, a thiol group, an epoxy group, a vinyl group, a diol group, an adhesive composition, a covalently bonded group, or an ionically bonded group.

12. The graft copolymer pretreatment composition of any one of claims 1 to 11, wherein the functional moiety comprises a polymer side chain that provides a lubricating function.

13. The graft copolymer pretreatment composition of claim 12, wherein the polymer side chain providing lubricating function comprises polyethylene glycol, polytetrahydrofuran, polyisobutylene, polysilicone, or any combination thereof.

14. The graft copolymer pretreatment composition of any one of claims 1 to 13, wherein the functional moiety comprises a humectant, a welding accelerator, and / or a corrosion inhibitor.

15. The graft copolymer pretreatment composition of any one of claims 1 to 14, wherein the graft copolymer pretreatment composition is crosslinked with a crosslinking agent.

16. The graft copolymer pretreatment composition of claim 15, wherein the crosslinking agent is a zirconium salt or a zirconium complex.

17. The graft copolymer pretreatment composition of claim 15 or 16, wherein the crosslinking agent is an aqueous solution of the zirconium salt or the zirconium complex.

18. The graft copolymer pretreatment composition of claim 15 or 16, wherein the crosslinking agent is an ethanol solution of a zirconium salt or a zirconium complex.

19. A method of pretreating at least a portion of a metal surface, comprising: The graft copolymer pretreatment composition of any one of claims 1 to 18 is applied to at least the portion of the metal surface.

Citation Information

Patent Citations

  • Anti-corrosion agent forming a coating film with good adhesion and method for non-galvanic application thereof

    CN101535356A

  • Corrosion protection treatment for surfaces made of zinc and zinc alloys

    CN102471890A

  • Coating for substrate

    CN104936626A

  • Coating compositions comprising adhesion promoting base layer

    CN107405430A

  • Surface modified porous film and manufacturing method of the same

    JP2017185475A