Adhesive for aluminum-plastic film, aluminum-plastic film and preparation method of aluminum-plastic film

By using special adhesives in aluminum-plastic films, the high temperature problem of aluminum-plastic films during charging and discharging is solved, and the heat resistance and thermal conductivity of aluminum-plastic films are improved, which extends the battery life and improves safety performance.

CN119081613APending Publication Date: 2024-12-06HUANGPU INST OF MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411211513.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing aluminum-plastic films are prone to high temperatures during multiple charges and discharges, resulting in gas generation, bulging and electrolyte corrosion, reducing the service life and stability of lithium-ion batteries, affecting its safety performance and widespread application.

Method used

Adhesive for aluminum-plastic films, including components A and components B. Component A is composed of amorphous polyester resin, thermal slurry and phenolic additives, and the number average molecular weight of the amorphous polyester resin is adjusted. and reaction density, combined with thermal filler and connecting agent, form a thermal framework structure, improve the coating performance and thermal conductivity of the adhesive, and ensure the heat resistance and adhesion properties of the aluminum-plastic film.

Benefits of technology

The aluminum-plastic film is not layered at high temperatures, and has excellent cold-burning depth molding and thermal conductivity, which improves heat seal defects such as thermal radiation and aluminum leakage, extends the service life of the battery and improves safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020423790000061
    Figure BDA0005020423790000061
  • Figure BDA0005020423790000071
    Figure BDA0005020423790000071
  • Figure BDA0005020423790000081
    Figure BDA0005020423790000081
Patent Text Reader

Abstract

The invention discloses an adhesive for an aluminum-plastic film, the aluminum-plastic film and a preparation method of the aluminum-plastic film, and belongs to the technical field of aluminum-plastic films. The adhesive for the aluminum plastic film comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 10: (1-3); the component A is prepared from the following components in percentage by mass: 20 to 40 percent of amorphous polyester resin, 10 to 30 percent of heat conduction slurry, 0.1 to 5.0 percent of phenolic additive and 40 to 60 percent of first solvent; wherein the heat-conducting slurry comprises a heat-conducting filler, a coupling agent and a second solvent, and the coupling agent is at least one of vinyl chloride-vinyl acetate resin, aldehyde-ketone resin and amorphous polyester resin; the number average molecular weight of the amorphous polyester resin is 10000 to 80000; and the component B is polyisocyanate. The adhesive is prepared by selecting the amorphous polyester resin with the specific number-average molecular weight, the heat-conducting filler and the phenolic additive, the aluminum-plastic film prepared by using the adhesive has excellent cold-deep-punching-resistant formability, is not layered at a high temperature and has good heat conductivity, and the heat sealing defects such as heat radiation and aluminum leakage are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery aluminum-plastic films, and in particular to an adhesive for aluminum-plastic films, an aluminum-plastic film and a preparation method thereof. Background Art

[0002] Due to its advantages in energy density, cycle life, flexibility, etc., soft-pack power batteries have become one of the most widely used battery types in the new energy industry. Soft-pack lithium-ion batteries mainly use aluminum-plastic film to cover bare cells, and perform hot-pressing packaging on the top and sides. With the continuous expansion of application areas, all walks of life have put forward more stringent requirements on the performance, quality and cost of soft-pack lithium-ion battery products. However, judging from the product performance of various battery manufacturers in my country, the performance of battery products, especially battery safety performance, such as overcharging, mechanical vibration, impact, extrusion and high temperature, is still a major problem that restricts the large-scale promotion and popularization of soft-pack lithium-ion batteries.

[0003] As the most important component to ensure battery safety, aluminum-plastic film has been a hot topic in the field of soft-pack lithium-ion battery safety applications in recent years. At present, soft-pack aluminum-plastic film is generally composed of three layers of films with different functions. The outer layer is a PA layer as a protective layer, the middle layer is an aluminum foil as a barrier layer, and the inner layer is a CPP as a heat-sealing layer. However, researchers have found that batteries packaged in this aluminum-plastic film are prone to generate high heat during multiple charge and discharge processes. The battery is used at a high temperature, which makes the battery more likely to generate gas and bulge. The electrolyte accelerates the corrosion of the packaging aluminum-plastic film, reducing the service life of the lithium-ion battery and affecting the stability and wide application of the lithium-ion battery. Summary of the invention

[0004] The purpose of the present application is to overcome the deficiencies of the prior art and provide an adhesive for aluminum-plastic film, an aluminum-plastic film and a preparation method thereof. The aluminum-plastic film prepared using the adhesive of the present application has excellent cold-drawing deep forming resistance, no delamination at high temperature, good thermal conductivity, and improves heat radiation, aluminum leakage and other heat sealing defects.

[0005] To achieve the above-mentioned purpose, the technical solution adopted in the present application is: an adhesive for aluminum-plastic film, comprising component A and component B, wherein the mass ratio of component A to component B is 10:(1-3);

[0006] Component A comprises, by mass percentage, 20%-40% of amorphous polyester resin, 10%-30% of thermal conductive paste, 0.1%-5.0% of phenolic additives, and 40%-60% of a first solvent; wherein the thermal conductive paste comprises a thermal conductive filler, a connector, and a second solvent, wherein the connector is at least one of chloroacetic resin, aldehyde-ketone resin, and amorphous polyester resin; and the number average molecular weight of the amorphous polyester resin is 10,000-80,000;

[0007] Component B is polyisocyanate.

[0008] As an example, the number average molecular weight of the non-crystalline polyester resin is 30,000-70,000.

[0009] The present application provides an adhesive for aluminum-plastic film, which has excellent cold-drawing deep-forming resistance, no delamination at high temperature, good thermal conductivity, and improves heat radiation, aluminum leakage and other heat-sealing defects. The present invention adjusts the number average molecular weight of the non-crystalline polyester resin to obtain non-crystalline polyester resins with different chain lengths and hydroxyl contents, reacts with polyisocyanate, adjusts the reaction density of the adhesive and the formed network structure, and reduces the sagging and aging time after the adhesive is coated, thereby improving the cold punching performance, adhesion performance, flexibility and heat resistance of the aluminum-plastic film, and ensuring that the heat sealing layer of the aluminum-plastic film is not damaged during subsequent processing and use; the inventors have found through research that the number average molecular weight of the non-crystalline polyester resin is less than 10,000, which is likely to cause uneven coating of the adhesive, and the flow after coating causes a tunnel effect of the aluminum-plastic film, resulting in a decrease in the overall performance of the aluminum-plastic film; the number average molecular weight of the non-crystalline polyester resin is greater than 80,000, which will cause the viscosity of the adhesive to be too high, thereby causing difficulties in the production of the aluminum-plastic film; the present invention preferably has a number average molecular weight of 30,000-70,000 for the non-crystalline copolyester resin to further improve the overall performance of the aluminum-plastic film.

[0010] In the adhesive for aluminum-plastic film of the present application, the thermal conductive paste improves the thermal conductivity of the aluminum-plastic film, and can conduct heat out (in) the battery cell in time when the battery cell generates heat due to excessive local current or local short circuit, or when the battery cell needs to be preheated externally to work normally under low temperature conditions, so as to achieve high thermal conductivity and improve the safety performance and service life of the battery cell; the connector can not only improve the dispersibility of the thermal conductive filler in the adhesive, but also improve the compatibility of the thermal conductive filler with the organic matter in the adhesive, and construct a thermal conductive skeleton structure, which plays a role in filling and further improving the thermal conductivity of the aluminum-plastic film; and the A component of the adhesive has a suitable viscosity, so that the adhesive can be more highly coated; the preferred connector of the present application is a non-crystalline polyester resin, so as to further obtain an aluminum-plastic film with better performance.

[0011] In the adhesive for aluminum-plastic film of the present application, the phenolic additive can act as an antioxidant to avoid the molecular chain breakage of the non-crystalline polyester resin, and at the same time provide a proton environment to avoid the rapid reaction of the non-crystalline polyester resin and polyisocyanate after mixing, thereby extending the activation period of the adhesive and improving the bonding performance, cold punching performance, thermal conductivity and heat resistance of the aluminum-plastic film.

[0012] As an example, the non-crystalline polyester resin is obtained by reacting an aromatic dibasic acid, an aliphatic dibasic acid, ethylene glycol and 1,4-cyclohexanedimethanol, and the molar ratio of the aromatic dibasic acid, the aliphatic dibasic acid, ethylene glycol and 1,4-cyclohexanedimethanol is aromatic dibasic acid: aliphatic dibasic acid: ethylene glycol: 1,4-cyclohexanedimethanol = (20-50): (0.5-30): (20-50): (0.5-30).

[0013] The present application adjusts the moles of aromatic dibasic acid, aliphatic dibasic acid, ethylene glycol and 1,4-cyclohexanedimethanol to obtain non-crystalline polyester resins with different number average molecular weights. The obtained non-crystalline polyester resin has good flexibility, hydrolysis resistance and heat resistance, and is conducive to deep punching.

[0014] As an example, the aromatic dibasic acid is at least one of terephthalic acid, isophthalic acid, and phthalic acid; preferably, the aromatic dibasic acid is terephthalic acid and isophthalic acid, or terephthalic acid and phthalic acid; more preferably, the molar ratio of terephthalic acid to isophthalic acid is (2:4)-(4:4); the molar ratio of terephthalic acid to phthalic acid is (2:4)-(4:4). The aromatic dibasic acid with the above molar ratio can obtain a non-crystalline polyester resin with better performance.

[0015] As an example, the aliphatic dibasic acid is at least one of azelaic acid, sebacic acid, dodecanedioic acid, and dimer acid. The long-chain aliphatic dibasic acid acts as a flexibility modifier to improve the flexibility and hydrolysis resistance of the non-crystalline polyester resin.

[0016] As an example, the method for preparing the non-crystalline polyester resin comprises the following steps:

[0017] Aromatic dibasic acid, aliphatic dibasic acid, ethylene glycol, 1,4-cyclohexanedimethanol, a polycondensation catalyst and an ester exchange agent are added to a reaction kettle, and the temperature is raised to 180-210°C for esterification reaction. After the esterification reaction is completed, an ester exchange agent and an antioxidant are added, the pressure is reduced to vacuum, and a polycondensation reaction is carried out at a temperature of 270-275°C to obtain a non-crystalline polyester resin.

[0018] 1,4-cyclohexanedimethanol has a lower reactivity than ethylene glycol. Part of the ethylene glycol is replaced by ester exchange and the exchange time is extended to increase the 1,4-cyclohexanedimethanol content. The amount of ester exchange agent added in the ester exchange reaction is greater than that in the polycondensation reaction to avoid excessively rapid growth of the polycondensation viscosity.

[0019] As an example, the polycondensation catalyst is at least one of tetraisobutyl titanate, organic tin, organic bismuth, and organic antimony.

[0020] As an example, the transesterification agent is phosphoric acid.

[0021] As an example, the antioxidant is antioxidant 1010 .

[0022] As an example, the phenolic additive is at least one of cardanol, phenol, cresol, phenylphenol, 2,6-di-tert-butyl-p-cresol, hydroquinone, and biphenol.

[0023] The above-mentioned types of phenolic additives can better improve the environment for the reaction between the non-crystalline polyester resin and the polyisocyanate, and improve the bonding performance, cold punching performance, thermal conductivity and heat resistance of the aluminum-plastic film.

[0024] As an example, the mass ratio of the thermally conductive filler, the connector and the second solvent is thermally conductive filler: connector: second solvent = (0.5-1.5): (0.1-0.2): (0.5-1.5).

[0025] As an example, the thermally conductive filler is at least one of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, carbon black, and graphite. To avoid short circuits caused by the battery cell manufacturing process, the thermally conductive filler is an insulating thermally conductive filler.

[0026] As an example, the first solvent is at least one of an ester, a ketone, and an aromatic hydrocarbon having a solvent volatilization rate greater than 2.

[0027] As an example, the second solvent is at least one of cyclohexanone, N-methylpyrrolidone, xylene, dipropylene glycol methyl ether acetate, butanone, and ethyl acetate.

[0028] As an example, the volatilization rate of the first solvent is greater than the volatilization rate of the second solvent.

[0029] As an example, the preparation method of the thermal conductive slurry is: placing a thermal conductive filler, a connector and a second solvent in a sand mill, and grinding to obtain the thermal conductive slurry.

[0030] As an example, the D of the thermal conductive paste 50 It is 10-100nm.

[0031] As an example, the polyisocyanate is at least one of an adduct of toluene diisocyanate (TDI) and trimethylolpropane (TMP), a TDI trimer, a hexamethylene diisocyanate isocyanurate (HDI) trimer, and a polymeric diphenylmethane-4,4'-diisocyanate (MDI).

[0032] In a second aspect, the present application provides a method for preparing the adhesive for aluminum-plastic film, comprising the following steps:

[0033] Adding a non-crystalline polyester resin and a phenolic additive to a first solvent, heating and stirring, then adding a thermal conductive slurry, stirring evenly and filtering to obtain a component A;

[0034] Before use, component A and component B are mixed evenly according to a certain proportion to obtain an adhesive for aluminum-plastic film.

[0035] In a third aspect, the present application provides an aluminum-plastic film, which at least includes a protective film, an aluminum foil layer, and an adhesive layer formed between the protective film and the aluminum foil layer, wherein the adhesive layer includes the adhesive of the above-mentioned solution.

[0036] As an example, the protective film may be, but is not limited to, one of a nylon film, a polyester film, a polyvinylidene chloride film, and an ethylene vinyl alcohol film.

[0037] The aluminum-plastic film of the present application can enhance the adhesion between the protective layer and the aluminum foil layer through the adhesive layer, further prevent the aluminum-plastic film from delamination, and enhance the heat resistance, thermal conductivity and cold punching resistance of the aluminum-plastic film.

[0038] In a fourth aspect, the present application provides a method for preparing an aluminum-plastic film, comprising the following steps:

[0039] The adhesive provided in the present application is coated on the surface of the aluminum foil and dried; the protective film and the dried adhesive are hot-pressed and laminated, and then aged to obtain an aluminum-plastic film.

[0040] As an example, the coating amount of the adhesive is 5 g / m 2 -7g / m 2 Preferably, the coating amount of the adhesive is 6g / m 2 .

[0041] As an example, the temperature of the hot pressing and laminating is 80-120°C; preferably, the temperature of the hot pressing and laminating is 100°C.

[0042] As an example, the aging temperature is 40-70° C., and the aging time is 1-7 days; preferably, the aging temperature is 50° C., and the aging time is 7 days.

[0043] Compared with the prior art, the beneficial effects of the present application are as follows: the present application adjusts the number average molecular weight of the non-crystalline polyester resin to obtain non-crystalline polyester resins with different chain lengths and hydroxyl contents, reacts with polyisocyanate, adjusts the reaction density of the adhesive and the formed network structure, and reduces the sagging and aging time after the adhesive is coated, thereby improving the cold punching performance, bonding performance, flexibility and heat resistance of the aluminum-plastic film; the thermal conductivity of the aluminum-plastic film is improved by adding a thermal conductive slurry, the connector can not only improve the dispersibility of the thermal conductive filler in the adhesive, but also improve the compatibility of the thermal conductive filler with the organic matter in the adhesive, and the constructed thermal conductive skeleton structure plays a role in filling and further improving the thermal conductivity of the aluminum-plastic film; and the A component of the adhesive has a suitable viscosity, so that the adhesive can be coated more highly. Phenolic additives can act as antioxidants to prevent the molecular chain of non-crystalline polyester resin from breaking, while providing a proton environment to prevent the rapid reaction of non-crystalline polyester resin and polyisocyanate after mixing, prolong the activation period of the adhesive, and improve the bonding performance, cold punching performance, thermal conductivity and heat resistance of the aluminum-plastic film. DETAILED DESCRIPTION

[0044] In order to better illustrate the purpose, technical scheme and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of the present application are all commonly used ordinary reagents and instruments unless otherwise specified.

[0045] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials:

[0046] 1. The preparation method of non-crystalline polyester resin comprises the following steps:

[0047] The components and weight proportions of the non-crystalline polyester resin are shown in Table 1. Aromatic dibasic acid, aliphatic dibasic acid, ethylene glycol, 1,4-cyclohexanedimethanol, tetraisobutyl titanate and the first phosphoric acid are added to a stainless steel reactor according to the ratio in Table 1. The temperature is raised to 200° C. under normal pressure for esterification reaction, and water is distilled off at the same time. When the water produced in the esterification reaction reaches the theoretical water output, the esterification reaction is considered to be completed; then the second phosphoric acid and antioxidant 1010 are added to the reaction system, the pressure of the reactor is reduced to a vacuum pressure minus 0.02-0.06 MPa, and the temperature is raised to 273° C. for polycondensation reaction, and the final reaction pressure is minus 0.1 MPa, and ethylene glycol is removed at the same time; the end point of the polycondensation reaction is judged according to the stirring power growth value, and then nitrogen is introduced to restore the pressure of the reactor to normal pressure to obtain a polymer melt, which is water-cooled and cast into a strip and pelletized to obtain a non-crystalline polyester resin.

[0048] Table 1

[0049]

[0050] 2. The preparation method of the thermal conductive slurry comprises the following steps:

[0051] The components and weight proportions of the thermal conductive slurry are shown in Table 2. The thermal conductive filler and colorant are vacuum dried at 200°C, cooled to room temperature by passing nitrogen, and the obtained thermal conductive filler, colorant and second solvent are added to a 1L sand mill. The second solvent is xylene and ethyl acetate, and the mass ratio of xylene to ethyl acetate is 1:1. The mixture is ground at a speed of 1500r / min for 2h, and then a connector is added and the grinding is continued for 3h to obtain the thermal conductive slurry.

[0052] Table 2

[0053]

[0054] In Table 2, aluminum nitride, D 50 =40nm, purchased from Anhui Kerun Nanotechnology Co., Ltd.;

[0055] Boron Nitride, D 50 =100nm, purchased from Beijing Dekedaojin Technology Co., Ltd.;

[0056] Nano-alumina, D 50 =15nm, purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.;

[0057] Carbon black ML, D 50 =24nm, purchased from Cabot High Performance Materials (Zhuhai) Co., Ltd.

[0058] Phenolic additive 1: cardanol, commercially available;

[0059] Phenolic additive 2: phenol, commercially available;

[0060] Examples and Comparative Examples

[0061] The components and weight proportions of the adhesive for aluminum-plastic film of the embodiment and comparative example are shown in Table 3 and Table 4; wherein, the preparation method of the adhesive for aluminum-plastic film of the embodiment and comparative example comprises the following steps:

[0062] The first solvent, the non-crystalline polyester resin, and the phenolic additive are added to a 10L planetary mixer in proportion, and stirred at 50°C, 80 rpm, and 2000 rpm until the components are fully dissolved, and the obtained mixture is filtered with a self-circulating 0.5um filter bag; the obtained filtrate and the thermal conductive slurry are added to a 10L planetary mixer, and stirred evenly at 80 rpm and 6000 rpm, and the obtained product is filtered with a self-circulating 0.5um folded filter element, and the obtained filtrate is component A;

[0063] Before use, component A and component B are mixed evenly, and the mass ratio of component A to component B is 10:3; thus, an adhesive for aluminum-plastic film is obtained; wherein the first solvent is ethyl acetate, and component B is HDI trimer.

[0064] The method for preparing the aluminum-plastic film of the embodiment and the comparative example comprises the following steps: using a roller coating method, applying the adhesive of the embodiment and the comparative example at a rate of 6 g / m 2 The coating amount is applied on the surface of the aluminum foil. After the solvent is dried in an oven, the nylon film and the aluminum foil are hot-pressed and compounded. The drying oven temperature is 50℃-60℃, 70℃-80℃, 90℃-120℃, and the temperature of the composite rubber roller is 100℃. The composite aluminum-plastic film is placed in a aging room for 7 days at a aging temperature of 50℃; an aluminum-plastic composite film of aluminum foil and nylon is obtained.

[0065] Table 3

[0066]

[0067] Table 4

[0068]

[0069] Performance Testing:

[0070] 1. The test method for single pit cold punching depth is: use a punch shape of 60mm×110mm, R angle = 1.0mm, punch every 0.3mm, depth 7.0mm; evaluate 40 pieces in each group, and check the number of pit damage;

[0071] 2. The wet aging test method is as follows: the aluminum-plastic film obtained in the embodiment and the comparative example is placed in an environment of temperature of 85°C and humidity of 85%RH for 7 days, and then the aluminum-plastic film is checked for white line delamination, bubble delamination, surface delamination, wrinkles, etc.;

[0072] 3. The test method for heat sealing performance is: side sealing at 190℃, pressure 0.3Mpa, time 3s, check whether there is heat radiation.

[0073] The performance test results are shown in Table 5.

[0074] Table 5

[0075]

[0076]

[0077] As shown in Table 5, the aluminum-plastic film prepared by using the adhesive prepared in the embodiment of the present application has excellent cold-drawing deep forming resistance, no delamination at high temperature, good thermal conductivity, improved heat radiation, and heat sealing defects such as aluminum leakage.

[0078] It can be seen from Examples 1-6 and Comparative Examples 1-4 that the adhesive for aluminum-plastic film generally requires a thermally conductive slurry to improve the thermal conductivity of the product. However, the most commonly used type of existing thermally conductive slurry is a commercially available white slurry. Although it has a good thermal conductivity effect, it often leads to a decrease in the cold-drawing and deep-forming resistance and moisture-heat resistance of the aluminum-plastic film. Adding a thermally conductive filler including a thermally conductive filler, a connector and a second solvent to the adhesive of the present invention can further improve the cold-drawing and deep-forming resistance, moisture-heat resistance and thermal radiation performance of the aluminum-plastic film. The composition of the thermally conductive slurry has a great influence on the performance of the aluminum-plastic film. When the connector in the thermally conductive slurry is at least one of a chloroacetic resin, an aldehyde-ketone resin, and a non-crystalline polyester resin, the deep-drawing damage of the aluminum-plastic film is low, especially when the connector is a non-crystalline polyester resin, the performance of the aluminum-plastic film is the best.

[0079] It can be seen from Examples 1, 7-11 and Comparative Example 5 that when the number average molecular weight of the non-crystalline polyester resin is less than 10,000, the probability of moisture-heat delamination of the aluminum-plastic film is higher; when the number average molecular weight of the non-crystalline polyester resin is 30,000-70,000 and dodecanedioic acid is used, the probability of moisture-heat delamination of the aluminum-plastic film is lower.

[0080] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.

Claims

1. An adhesive for aluminum-plastic film, characterized in that: It comprises component A and component B, and the mass ratio of component A to component B is 10:(1-3); Component A comprises, by mass percentage, 20%-40% of amorphous polyester resin, 10%-30% of thermal conductive paste, 0.1%-5.0% of phenolic additives, and 40%-60% of a first solvent; wherein the thermal conductive paste comprises a thermal conductive filler, a connector, and a second solvent, and the connector is at least one of a chloroacetic resin, an aldehyde-ketone resin, and amorphous polyester resin; and the number average molecular weight of the amorphous polyester resin is 10,000-80,000; Component B is polyisocyanate.

2. The adhesive for aluminum-plastic films according to claim 1, characterized in that: The number average molecular weight of the non-crystalline polyester resin is 30,000-70,000.

3. The adhesive for aluminum-plastic films according to claim 1, characterized in that: The non-crystalline polyester resin is obtained by reacting an aromatic dibasic acid, an aliphatic dibasic acid, ethylene glycol and 1,4-cyclohexanedimethanol; the molar ratio of the aromatic dibasic acid, the aliphatic dibasic acid, ethylene glycol and 1,4-cyclohexanedimethanol is aromatic dibasic acid: aliphatic dibasic acid: ethylene glycol: 1,4-cyclohexanedimethanol = (20-50): (0.5-30): (20-50): (0.5-30).

4. The adhesive for aluminum-plastic films according to claim 3, characterized in that: The aromatic dibasic acid is at least one of terephthalic acid, isophthalic acid, and phthalic acid; and / or the aliphatic dibasic acid is at least one of azelaic acid, sebacic acid, dodecanedioic acid, and dimer acid.

5. The adhesive for aluminum-plastic films according to claim 3, characterized in that: The method for preparing the non-crystalline polyester resin comprises the following steps: Aromatic dibasic acid, aliphatic dibasic acid, ethylene glycol, 1,4-cyclohexanedimethanol, a polycondensation catalyst and an ester exchange agent are added to a reaction kettle, and the temperature is raised to 180-210°C for esterification reaction. After the esterification reaction is completed, an ester exchange agent and an antioxidant are added, the pressure is reduced to vacuum, and a polycondensation reaction is carried out at a temperature of 270-275°C to obtain a non-crystalline polyester resin.

6. The adhesive for aluminum-plastic films according to claim 5, characterized in that: The polycondensation catalyst is tetraisobutyl titanate; and / or the transesterification agent is phosphoric acid; and / or the antioxidant is antioxidant 1010.

7. The adhesive for aluminum-plastic films according to claim 1, characterized in that: The mass ratio of the thermally conductive filler, the connector and the second solvent is thermally conductive filler: connector: second solvent = (0.5-1.5): (0.1-0.2): (0.5-1.5).

8. The adhesive for aluminum-plastic films according to claim 1, characterized in that: The preparation method of the thermal conductive slurry is: placing the thermal conductive filler, the connecting agent and the second solvent in a sand mill, and grinding to obtain the thermal conductive slurry; preferably, the D of the thermal conductive slurry is 50 It is 10-100nm.

9. The adhesive for aluminum-plastic films according to claim 1, characterized in that: The phenolic additive is at least one of cardanol, phenol, cresol, phenylphenol, 2,6-di-tert-butyl-p-cresol, hydroquinone, and biphenol; and / or the thermally conductive filler is at least one of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, carbon black, and graphite; and / or, the first solvent is at least one of an ester, a ketone, and an aromatic hydrocarbon having a solvent volatilization rate greater than 2; and / or the second solvent is at least one of cyclohexanone, N-methylpyrrolidone, xylene, dipropylene glycol methyl ether acetate, and butanone; And / or the polyisocyanate is at least one of TDI adduct, TDI trimer, HDI trimer and polymer MDI.

10. A method for preparing the adhesive for aluminum-plastic film according to any one of claims 1 to 9, characterized in that: The following steps are involved: Adding a non-crystalline polyester resin and a phenolic additive to a first solvent, heating and stirring, then adding a thermal conductive slurry, stirring evenly and filtering to obtain a component A; Before use, component A and component B are mixed evenly according to a certain proportion to obtain an adhesive for aluminum-plastic film.

11. An aluminum-plastic film, characterized in that: The aluminum-plastic film at least comprises a protective film, an aluminum foil layer, and an adhesive layer formed between the protective film and the aluminum foil layer, wherein the adhesive layer comprises the adhesive for the aluminum-plastic film according to any one of claims 1 to 11.

12. A method for preparing an aluminum-plastic film as claimed in claim 11, characterized in that: The method comprises the following steps: coating the adhesive provided by the present application on the surface of the aluminum foil and drying it; hot-pressing and compounding the protective film with the dried adhesive, and then aging it to obtain an aluminum-plastic film.

13. The method for preparing the aluminum-plastic film according to claim 12, characterized in that: The coating amount of the adhesive is 5g / m 2 -7g / m 2 ; and / or the temperature of the hot pressing composite is 80-120°C; and / or the aging temperature is 40-70°C, and the aging time is 1-7 days.

Citation Information

Cited By

  • Aluminum plastic film and electrochemical device and electronic device comprising same

    CN121290870A