Environment-friendly prime coat-free double-component polyurethane sealant and preparation method thereof

By introducing specific components and processes into polyurethane sealants, an environmentally friendly primer-free two-component polyurethane sealants are formed, which solves the stability and production efficiency of traditional sealants in high temperature and high humidity environments, and achieves high mechanical properties and simplified operation, suitable for a variety of substrates.

CN119081632APending Publication Date: 2024-12-06BEIJING COMENS NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411374879.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional solvent-based polyurethane sealants cannot meet the stability of the glue layer under high temperature and high humidity conditions under extreme environments, resulting in bubbles and cracks, long curing time, slow production beat, complex process and rapid positioning, which cannot meet the industry's environmental protection. and efficient demand.

Method used

The environmentally friendly primer-free two-component polyurethane sealant is used, consisting of component A and component B in volume ratio of 10:0.95 to 1.05. Component A includes terminal isocyanate polyurethane prepolymer, adhesive accelerator, filler, aging Additives and plasticizers, component B includes end hydroxyl compounds or end silane compounds, plasticizers and curing agents. Through specific component ratios and process preparation methods, a sealant with high mechanical properties is formed, which simplifies the operation process and Used in high temperature and high humidity environments.

Benefits of technology

The glue layer stability in high temperature and high humidity environment is achieved, curing time is shortened, production efficiency is improved, operating process is simplified, environmental protection regulations are met, and bottomless is achieved on substrates such as glass, painted boards, and metal. Coated bonding, with excellent mechanical and retention properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an environment-friendly primer-free double-component polyurethane sealant and a preparation method thereof, and belongs to the field of polyurethane sealants, the sealant comprises: a component A and a component B. The component A comprises, by weight, 10-50 parts of an isocyanate-terminated polyurethane prepolymer, 5-20 parts of an adhesion promoter, 10-50 parts of a first filler, 0.1-10 parts of an aging aid, 0.2-2 parts of a moisture scavenger, 7-20 parts of a first plasticizer and 0.02-1 part of a first catalyst; and the component B comprises the following components in parts by weight: 10-50 parts of a hydroxyl-terminated or silane-terminated compound, 5-20 parts of a second plasticizer, 30-70 parts of a second filler and 2-10 parts of a curing agent. The sealant is good in shape retention, high in mechanical property and short in curing time, the production takt is accelerated, the efficiency is improved, and the sealant can be used in a high-temperature and high-humidity environment; the adhesion promoter is introduced, so that the adhesive can be used for adhering substrates such as glass, paint plates and metal without coating a base coat, the operation process is simplified, and the application range is wide; and environmental protection laws and regulations are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polyurethane sealants, and in particular to an environmentally friendly primer-free two-component polyurethane sealant and a preparation method thereof. Background Art

[0002] Polyurethane sealants are widely used in the automotive industry, aviation industry, civil construction industry and other fields because of their excellent mechanical properties, good elasticity, low temperature compliance, good weather resistance and aging resistance.

[0003] In many industries, one-component moisture-curing polyurethane sealants with polyurethane prepolymer resin as the main component are more common. With the popularization of one-component polyurethane sealants, its high environmental requirements, bubbling and cracking of the adhesive layer under high temperature and high humidity, long curing time, slow production cycle, complex process, and inability to quickly position are gradually showing their disadvantages. Therefore, the development of a primer-free two-component polyurethane sealant can solve the above problems.

[0004] At present, traditional solvent-based polyurethane sealants are gradually fading out of industry applications because they cannot meet the requirements of extreme environments. Therefore, it is of practical significance to provide an environmentally friendly polyurethane sealant.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide an environmentally friendly primer-free two-component polyurethane sealant and a preparation method thereof, which has high mechanical properties and is suitable for a variety of substrates such as metals, organic / inorganic glass, and paint plates. It can solve the technical problems of existing solvent-based polyurethane sealants, such as the inability to meet high environmental requirements, bubbling and cracking of the adhesive layer under high temperature and high humidity, long curing time, slow production cycle, complex process, and inability to quickly position.

[0007] The objective of the present invention is achieved through the following technical solutions:

[0008] An environmentally friendly primer-free two-component polyurethane sealant, the sealant is composed of component A and component B in a volume ratio of 10:0.95-1.05; wherein,

[0009] The A component is mainly composed of the following raw materials in parts by weight:

[0010] 10-50 parts of terminal isocyanate polyurethane prepolymer, 5-20 parts of adhesion promoter, 10-50 parts of first filler, 0.1-10 parts of aging aid, 0.2-2 parts of water remover, 7-20 parts of first plasticizer and 0.02-1 parts of first catalyst;

[0011] The adhesion promoter is a siloxane-terminated prepolymer prepared by dropwise reaction of a double-bond-terminated modified isocyanate prepolymer, a double-bond silane coupling agent, a polymerization inhibitor and an initiator;

[0012] The B component is mainly composed of the following raw materials in parts by weight:

[0013] 10 to 50 parts of terminal hydroxyl compound or terminal silane compound, 5 to 20 parts of second plasticizer, 30 to 70 parts of second filler and 2 to 10 parts of curing agent.

[0014] Preferably, in the component A of the sealant, the isocyanate-terminated polyurethane prepolymer is a reaction product prepared by reacting a first component with a molecular weight of 2000 to 8000, a second component, a catalyst A and a plasticizer A at a molar ratio of 2 to 2.5; wherein the first component is at least one of polyether polyol, polyester polyol, polyacrylic polyol, polycarbonate polyol and polyhydrocarbon polyol with a molecular weight of 2000 to 6000;

[0015] The second component is at least one of aromatic polyisocyanate and aliphatic polyisocyanate.

[0016] Preferably, in the above sealant, in the isocyanate-terminated polyurethane prepolymer, the catalyst A is at least one of a metal tin catalyst, an amine catalyst, a bismuth compound catalyst, a morpholine compound catalyst, and an imidazole derivative catalyst;

[0017] The plasticizer A is at least one of phthalates, adipic acid esters, sulfonates, phosphates, sulfonamides, and chlorinated paraffins.

[0018] Preferably, in the above sealant, in the adhesion promoter, the double-bond terminated modified isocyanate prepolymer is a double-bond terminated modified isocyanate prepolymer prepared by reacting an isocyanate compound, a hydroxyl-containing acrylate and a catalyst B.

[0019] Preferably, in the above-mentioned sealant, in the double-bond terminated modified isocyanate prepolymer, the isocyanate compound is at least one of p-toluenesulfonyl isocyanate, diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate;

[0020] The hydroxyl-containing acrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate.

[0021] Preferably, in the above-mentioned sealant, in the adhesion promoter, the double-bond silane coupling agent is at least one of vinyl trimethoxy silane, vinyl tri (b-methoxyethoxy) silane, and γ-methacryloxypropyl trimethoxy silane;

[0022] The polymerization inhibitor is at least one of a quinone polymerization inhibitor and an inorganic compound polymerization inhibitor;

[0023] The initiator is at least one selected from azo initiators, diacyl peroxides, hydroperoxides and organic peroxides.

[0024] Preferably, in the component A of the sealant, the first filler is at least one of carbon black, mica, talc, kaolin, wollastonite, feldspar, syenite, chlorite, bentonite, montmorillonite, calcium carbonate, dolomite, quartz, calcined silica, precipitated silica, fumed silica, cristobalite, calcium oxide, aluminum hydroxide, magnesium oxide, ceramic hollow spheres, glass hollow spheres, organic hollow spheres, and glass beads;

[0025] The aging aid is at least one of a UV absorber, a light stabilizer and an antioxidant;

[0026] The dehydrating agent is at least one of a terminal isocyanate compound, triethyl orthoformate, an oxazolidine dehydrating agent, a molecular sieve desiccant, calcium oxide, and a silane dehydrating agent;

[0027] The first plasticizer is at least one of phthalates, adipates, sulfonates, phosphates, sulfonamides, and chlorinated paraffins;

[0028] The first catalyst is at least one of dibutyltin diacetate, dibutyltin dilaurate, stannous octoate, dibutyltin dichloride, dibutyltin diacetylacetonate, dioctyltin dilaurate, amine catalysts, bismuth compound catalysts, morpholine compound catalysts, and imidazole derivative catalysts.

[0029] Preferably, in the above sealant, in the component B, the terminal hydroxyl compound or terminal silane compound is at least one of polyether polyol, polyester polyol, polyacrylic polyol, polycarbonate polyol, and terminal silane-modified polyether;

[0030] The second plasticizer is at least one of phthalates, adipates, sulfonates, phosphates, sulfonamides, and chlorinated paraffins;

[0031] The second filler is at least one of carbon black, mica, talc, kaolin, wollastonite, feldspar, syenite, chlorite, bentonite, montmorillonite, calcium carbonate, dolomite, quartz, calcined silicon dioxide, precipitated silicon dioxide, fumed silica, cristobalite, calcium oxide, aluminum hydroxide, magnesium oxide, ceramic hollow spheres, glass hollow spheres, organic hollow spheres, and glass beads;

[0032] The curing agent is at least one of a hydroxyl small molecule compound and an amino small molecule compound.

[0033] A method for preparing the environmentally friendly primer-free two-component polyurethane sealant of the present invention comprises the following steps:

[0034] Prepare component A and component B separately, wherein:

[0035] Prepare component A as follows:

[0036] According to the formulation of component A of the environment-friendly primer-free two-component polyurethane sealant of the present invention, various raw materials are taken, and the isocyanate-terminated polyurethane prepolymer, adhesion promoter, first filler, aging aid, first plasticizer and first catalyst in the raw materials of component A are added into a stirring kettle and mixed evenly to obtain component A;

[0037] Prepare component B as follows:

[0038] According to the B component formula of the environmentally friendly primer-free two-component polyurethane sealant of the present invention, various raw materials are taken, and any one of the terminal hydroxyl compound or terminal silane compound in the B component raw material, the second plasticizer, the second filler and the curing agent are added to another stirring kettle and mixed evenly to obtain the B component;

[0039] The component A and the component B prepared above are put into a rubber hose in a volume ratio of 10:0.95-1.05, mixed and glued, so as to prepare an environmentally friendly primer-free two-component polyurethane sealant.

[0040] Preferably, in the above method, the isocyanate-terminated polyurethane prepolymer in component A is prepared in the following manner, including:

[0041] At least one of polyether polyol, polyester polyol, polyacrylic polyol and polycarbonate polyol with a molecular weight of 2000-6000 is used as the first component, the first component and plasticizer A are added into a reaction kettle, the temperature is raised to 120° C., vacuum dehydration is performed for 2 hours, and then the temperature is lowered to 60-80° C., and the second component is added, wherein the second component is at least one of aromatic polyisocyanate and aliphatic polyisocyanate, and the reaction is carried out at 60-80° C. for 2-3 hours, and catalyst A is added; the reaction is continued at 80-90° C. for 1-2 hours until the NCO content is less than 1%, and the reaction is stopped to obtain a terminal isocyanate polyurethane prepolymer;

[0042] The adhesion promoter in the A component is prepared in the following manner, including:

[0043] Premixing double-bond terminated modified isocyanate prepolymer, double-bond silane coupling agent, polymerization inhibitor and initiator to obtain a premixed solution, taking a solution accounting for 20% of the weight of the premixed solution and adding it into a reactor as a bottom liquid, slowly heating it to 120°C, reacting it for 15 minutes, then dripping the remaining solution into the reactor within 2 to 3 hours using a constant pressure burette, and then keeping it warm for 30 minutes, and discharging the material to obtain an adhesion promoter;

[0044] The double-bond terminated modified isocyanate prepolymer in the adhesion promoter is prepared in the following manner, including:

[0045] Add isocyanate compound and hydroxyl-containing acrylate into the reaction kettle, slowly heat up to 60-80°C and react for 2-3h, add catalyst B, continue to react at 80-90°C for 1-2 hours, until the NCO content is lower than 0.1%, stop the reaction, and the double-bond terminated modified isocyanate prepolymer is obtained.

[0046] Compared with the prior art, the environmentally friendly primer-free two-component polyurethane sealant and the preparation method thereof provided by the present invention have the following beneficial effects:

[0047] In the viscosity test of this two-component polyurethane sealant, it has good shape retention and high mechanical properties, and the shear strength is ≥6MPa under the overlap area of ​​25×12.5×4mm. By introducing the B component composed of terminal hydroxyl compounds or terminal silane compounds, a second plasticizer, a second filler and a curing agent, the curing time is greatly shortened, the production cycle is accelerated to improve efficiency, and it can be used in an environment with higher temperature and humidity. By introducing a specific adhesion promoter into the A component, it can be bonded to glass, paint panels, metal and other substrates without the need for primer, simplifying the operation process and having a wide range of uses. It is solvent-free and meets environmental protection regulations. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0049] Figure 1 This is a structural diagram of a double-bond terminated modified isocyanate prepolymer provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0050] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0051] First, the terms that may be used in this article are explained as follows:

[0052] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.

[0053] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.

[0054] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.

[0055] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.

[0056] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values ​​and all integers and fractions within the numerical range.

[0057] The scheme provided by the present invention is described in detail below. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professionals in the field. If the specific conditions are not specified in the embodiments of the present invention, they are carried out according to the conventional conditions in the field or the conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used in the embodiments of the present invention, they are all conventional products that can be purchased commercially.

[0058] The embodiment of the present invention provides an environmentally friendly primer-free two-component polyurethane sealant, which is mainly composed of component A and component B in a volume ratio of 10:0.95-1.05; wherein,

[0059] Component A is mainly composed of the following raw materials in parts by weight: 10-50 parts of terminal isocyanate polyurethane prepolymer, 5-20 parts of adhesion promoter, 10-50 parts of first filler, 0.1-10 parts of aging aid, 0.2-2 parts of water remover, 7-20 parts of first plasticizer, and 0.02-1 parts of first catalyst;

[0060] The adhesion promoter is a siloxane-terminated prepolymer prepared by dropwise reaction of a double-bond-terminated modified isocyanate prepolymer and a double-bond silane coupling agent, a polymerization inhibitor and an initiator;

[0061] Component B is mainly composed of the following raw materials in parts by weight:

[0062] 10 to 50 parts of terminal hydroxyl compound or terminal silane compound, 5 to 20 parts of second plasticizer, 30 to 70 parts of second filler and 2 to 10 parts of curing agent.

[0063] In some specific embodiments of the present invention, the isocyanate-terminated polyurethane prepolymer in the above-mentioned component A is mainly prepared by reacting a polyol with an isocyanate compound, a catalyst A and a plasticizer A, and its structure is as follows: Figure 1As shown, the isocyanate compound can be a diisocyanate, for example: the isocyanate compound is preferably one of diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), and isophorone diisocyanate (IPDI); the polyol mainly uses polyether polyol with a molecular weight of 2000 to 8000, and the other substances are plasticizer A and catalyst A, and the process is controlled according to R value (NCO / OH) of 2 to 2.5.

[0064] In some specific embodiments of the present invention, in the adhesion promoter of the above-mentioned component A, the double-bond terminated modified isocyanate prepolymer is a double-bond terminated modified isocyanate prepolymer prepared by reacting an isocyanate compound, a hydroxyl-containing acrylate and a catalyst B; the isocyanate compound is at least one of monoisocyanate, p-toluenesulfonyl isocyanate, diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), and isophorone diisocyanate (IPDI); the hydroxyl-containing acrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and hydroxypropyl methacrylate;

[0065] The catalyst B is at least one of a metal tin catalyst, an amine catalyst, a bismuth compound catalyst, a morpholine compound catalyst, and an imidazole derivative catalyst.

[0066] The double bond silane coupling agent is at least one of vinyl trimethoxy silane, vinyl tri (b-methoxyethoxy) silane, and γ-methacryloxypropyl trimethoxy silane.

[0067] The polymerization inhibitor is at least one of a quinone polymerization inhibitor and an inorganic compound polymerization inhibitor.

[0068] The initiator is at least one selected from azo initiators, diacyl peroxides, hydroperoxides, and organic peroxides.

[0069] Preferably, in the above-mentioned isocyanate-terminated polyurethane prepolymer, the plasticizer A is at least one of phthalates, adipates, sulfonates, phosphates, sulfonamides, and chlorinated paraffins;

[0070] The catalyst A is at least one of a metal tin catalyst, an amine catalyst, a bismuth compound catalyst, a morpholine compound catalyst, and an imidazole derivative catalyst.

[0071] In some specific embodiments of the present invention, in the above-mentioned component A, the aging aid is at least one of a UV absorber, a light stabilizer and an antioxidant, and preferably the UV absorber, the light stabilizer and the antioxidant are mixed in proportion for use.

[0072] In some specific embodiments of the present invention, in the above-mentioned component A, the dehydrating agent is at least one of terminal isocyanate compounds, triethyl orthoformate, oxazolidine dehydrating agent, molecular sieve desiccant, calcium oxide, and silane dehydrating agent.

[0073] In some specific embodiments of the present invention, in the above-mentioned component A, the first catalyst is at least one of dibutyltin diacetate, dibutyltin dilaurate, stannous octoate, dibutyltin dichloride, dibutyltin diacetylacetonate, dioctyltin dilaurate, an amine catalyst, a bismuth compound catalyst, a morpholine compound catalyst, and an imidazole derivative catalyst.

[0074] In some specific embodiments of the present invention, in the above-mentioned component B, the terminal hydroxyl compound or the terminal silane compound adopts at least one of polyether polyols, polyester polyols, polyacrylic polyols, polycarbonate polyols, polyhydrocarbon polyols, and terminal silane polyethers. The present invention mainly adopts commercially available terminal silane polyethers.

[0075] In some specific embodiments of the present invention, in the above-mentioned component B, the curing agent is at least one of a hydroxyl small molecule compound and an amino small molecule compound.

[0076] In some specific embodiments of the present invention, in the above-mentioned component A and component B, the first filler and the second filler are both made of at least one of carbon black, mica, talc, kaolin, wollastonite, feldspar, syenite, chlorite, bentonite, montmorillonite, calcium carbonate, dolomite, quartz, calcined silica, precipitated silica, fumed silica, cristobalite, calcium oxide, aluminum hydroxide, magnesium oxide, ceramic hollow spheres, glass hollow spheres, organic hollow spheres, and glass beads.

[0077] In some specific embodiments of the present invention, in the above-mentioned component A and component B, the first plasticizer and the second plasticizer are both at least one of phthalates, adipates, sulfonates, phosphates, sulfonamides, and chlorinated paraffins, preferably, mainly one of DINP or DIDP.

[0078] The embodiment of the present invention provides an environmentally friendly primer-free two-component polyurethane sealant and a preparation method thereof, comprising the following steps:

[0079] Prepare component A and component B separately, wherein:

[0080] Prepare component A, comprising:

[0081] According to the above-mentioned formula of component A of the environmentally friendly primer-free two-component polyurethane sealant, various raw materials are taken, and the isocyanate-terminated polyurethane prepolymer, adhesion promoter, first filler, aging aid, first plasticizer and first catalyst in the raw materials of component A are added into a stirring kettle and mixed evenly to obtain component A;

[0082] Prepare component B, comprising:

[0083] Take the raw materials according to the above-mentioned formula of component B of the environmentally friendly primer-free two-component polyurethane sealant, add the terminal hydroxyl compound or terminal silane compound, the second plasticizer, the second filler, and the curing agent in the raw materials of component B into a stirring kettle and mix them evenly to obtain component B;

[0084] The component A and the component B prepared above are put into a rubber hose in a volume ratio of 10:0.95-1.05, mixed and glued to obtain an environmentally friendly primer-free two-component polyurethane sealant.

[0085] In summary, the environmentally friendly primer-free two-component polyurethane sealant and the preparation method thereof according to the embodiment of the present invention have at least the following beneficial effects compared with the prior art:

[0086] 1) Compared with the existing sealants, the invention synthesizes a special adhesion promoter. By introducing the adhesion promoter, it can be bonded to glass, paint plates, metal and other substrates without the need for primer coating, and the bonding is 100% cohesive failure. At the same time, it is a two-component sealant with the advantage of fast curing speed, which greatly simplifies the operation process, speeds up the production cycle, and has a wide range of applications.

[0087] 2) The present invention can achieve good shape retention without adding solvents, and has excellent mechanical properties and aging properties; it can be used in a wide temperature and humidity environment, which has significant advantages.

[0088] In summary, the environmentally friendly primer-free two-component polyurethane sealant of the embodiment of the present invention has the advantages of being solvent-free, primer-free, having high mechanical properties, excellent shape retention, moderate viscosity, fast curing, and easy operation, and is suitable for various substrates such as glass, painted boards, and metals.

[0089] In order to more clearly demonstrate the technical solution and technical effects provided by the present invention, the solution provided by the embodiment of the present invention is described in detail with specific embodiments below.

[0090] The raw material proportions of Examples 1 to 3 of the present invention and Comparative Example 1 are shown in Table 1 below (measured in parts by weight):

[0091]

[0092]

[0093] Note: Catalyst A and Catalyst B in the above table both use dibutyl dilaurate, and the first catalyst uses dimorpholinyl diethyl ether (DMDEE)

[0094] Embodiment 1:

[0095] This embodiment provides an environmentally friendly primer-free two-component polyurethane sealant, and the preparation method thereof comprises the following steps:

[0096] S1: Preparation of terminal isocyanate polyurethane prepolymer: Add polyether polyol with a molecular weight of 2000-6000 and plasticizer A as the first component into a reactor, heat to 120°C, vacuum dehydrate for 2 hours, then cool to 60-80°C, add diphenylmethane diisocyanate as the second component, react at 60-80°C for 2-3 hours, add catalyst A; continue to react at 80-90°C for 1-2 hours until the NCO content reaches 2.4%, stop the reaction, and obtain the terminal isocyanate polyurethane prepolymer for standby use.

[0097] S2: Preparation of adhesion promoter: premix double-bond terminated modified isocyanate prepolymer and double-bond silane coupling agent A172, dibenzoyl peroxide as initiator and p-dimethylquinone as inhibitor, take 20% of the total volume of the solution and add it into the reactor as the bottom liquid, slowly heat up to 120°C, react for 15 minutes, then use a constant pressure burette to add the remaining solution into the reactor within 2 to 3 hours, then keep warm for 30 minutes, and the adhesion promoter is obtained by discharging the material for use.

[0098] The double-bond terminated modified isocyanate prepolymer of the adhesion promoter is prepared in the following manner, including: adding p-toluenesulfonyl isocyanate and hydroxyethyl acrylate into a reaction kettle, slowly heating to 60-80°C for reaction for 2-3h, adding catalyst B, continuing to react at 80-90°C for 1-2 hours until the NCO content is lower than 0.1%, stopping the reaction, and discharging the material to obtain the double-bond terminated modified isocyanate prepolymer.

[0099] S3: preparing component A: adding the isocyanate-terminated polyurethane prepolymer, adhesion promoter, carbon black, kaolin, aging aid, first plasticizer (DIDP) and first catalyst in the raw materials of component A into a stirring kettle and dispersing and mixing them uniformly to obtain component A;

[0100] S4: preparing component B: adding the terminal hydroxyl or terminal silane compound, the second plasticizer (DIDP), fumed silica, and isophorone diamine in the raw materials of component B into a stirring kettle and dispersing and mixing them uniformly to obtain component B;

[0101] The prepared component A and component B are put into a rubber hose in a volume ratio of 10:1, mixed and glued to obtain an environmentally friendly primer-free two-component polyurethane sealant.

[0102] Example 2

[0103] This embodiment provides an environmentally friendly primer-free two-component polyurethane sealant, and its preparation method is basically the same as that of Example 1, except that: the silane coupling agent used is KH570.

[0104] Example 3

[0105] This embodiment provides an environmentally friendly primer-free two-component polyurethane sealant, and its preparation method is basically the same as that of Example 1, except that: the silane coupling agent used is KH560.

[0106] Comparative Example 1

[0107] This embodiment provides an environmentally friendly primer-free two-component polyurethane sealant, and its preparation method is basically the same as that of Example 1, except that no adhesion promoter is added.

[0108] Performance Testing

[0109] The following performance tests were performed on the environmentally friendly primer-free two-component polyurethane sealants prepared in Examples 1 to 3 of the present invention and the two-component polyurethane sealant composition prepared in Comparative Example 1:

[0110] The surface drying time and curing time of the colloid are tested under a constant temperature of 23±2℃ and 50±5%RH.

[0111] The colloid viscosity was tested using a lamina viscometer 2000+.

[0112] The colloid tensile strength (Type II), fracture productivity, hardness, shear strength (lap size 25*12.5*4mm), and adhesion failure tests were conducted on samples prepared and maintained in a constant temperature of 23±2°C, 50±5%RH environment for 7 days before testing.

[0113] The above performance test results are shown in Table 2

[0114] Table 2

[0115]

[0116] Note: CF in Table 2 above represents cohesive failure, and CF greater than 90% represents good bonding.

[0117] From the performance tests of Examples 1 to 3 and Comparative Example 1 in Table 2 above, it can be seen that:

[0118] Comparative Example 1 does not add the specific adhesion promoter of the present invention, and its adhesion effect on glass, paint plate and metal is not ideal and cannot meet the requirements. Example 3 adds conventional silane coupling agent KH560, and its adhesion effect on the paint plate is slightly improved compared with Comparative Example 1, but there is still no adhesion on glass and metal, and the effect is poor; Example 2 uses Maitu A-1891 silane coupling agent, and its adhesion effect is significantly improved, but it still fails to reach 100% CF (complete cohesive failure), and the adhesion effect is poor; Example 1 uses Maitu A-Link15 silane coupling agent, and its primer-free adhesion effect reaches 100% CF, which is the best effect.

[0119] In addition, the mechanical properties of Example 1 are greater than those of Examples 2, 3 and Comparative Example 1, and have good mechanical properties.

[0120] In summary, the environmentally friendly primer-free two-component polyurethane sealant of the embodiment of the present invention has the advantages of being solvent-free, primer-free, having high mechanical properties, excellent shape retention, moderate viscosity, fast curing, and easy operation, and is suitable for various substrates such as glass, painted boards, and metals.

[0121] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. An environmentally friendly primer-free two-component polyurethane sealant, characterized in that: The sealant is composed of component A and component B in a volume ratio of 10:0.95-1.05; wherein, The A component is mainly composed of the following raw materials in parts by weight: 10-50 parts of terminal isocyanate polyurethane prepolymer, 5-20 parts of adhesion promoter, 10-50 parts of first filler, 0.1-10 parts of aging aid, 0.2-2 parts of water remover, 7-20 parts of first plasticizer and 0.02-1 parts of first catalyst; The adhesion promoter is a siloxane-terminated prepolymer prepared by dropwise reaction of a double-bond-terminated modified isocyanate prepolymer, a double-bond silane coupling agent, a polymerization inhibitor and an initiator; The B component is mainly composed of the following raw materials in parts by weight: 10 to 50 parts of terminal hydroxyl compound or terminal silane compound, 5 to 20 parts of second plasticizer, 30 to 70 parts of second filler and 2 to 10 parts of curing agent.

2. The environmentally friendly primer-free two-component polyurethane sealant according to claim 1, characterized in that: In the component A, the isocyanate-terminated polyurethane prepolymer is a reaction product prepared by reacting a first component with a molecular weight of 2000 to 8000, a second component, a catalyst A and a plasticizer A at a molar ratio of 2 to 2.5; wherein the first component is at least one of polyether polyol, polyester polyol, polyacrylic polyol, polycarbonate polyol and polyhydrocarbon polyol with a molecular weight of 2000 to 6000; The second component is at least one of aromatic polyisocyanate and aliphatic polyisocyanate.

3. The environmentally friendly primer-free two-component polyurethane sealant according to claim 2, characterized in that: In the isocyanate-terminated polyurethane prepolymer, the catalyst A is at least one of a metal tin catalyst, an amine catalyst, a bismuth compound catalyst, a morpholine compound catalyst, and an imidazole derivative catalyst; The plasticizer A is at least one of phthalates, adipic acid esters, sulfonates, phosphates, sulfonamides, and chlorinated paraffins.

4. The environmentally friendly primer-free two-component polyurethane sealant according to claim 1, characterized in that: In the adhesion promoter, the double-bond terminated modified isocyanate prepolymer is a double-bond terminated modified isocyanate prepolymer prepared by reacting an isocyanate compound, a hydroxyl-containing acrylate and a catalyst B.

5. The environmentally friendly primer-free two-component polyurethane sealant according to claim 4, characterized in that: In the double-bond terminated modified isocyanate prepolymer, the isocyanate compound is at least one of p-toluenesulfonyl isocyanate, diphenylmethane diisocyanate, toluene diisocyanate, hexamethylene diisocyanate, and isophorone diisocyanate; The hydroxyl-containing acrylate is at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate and hydroxypropyl methacrylate; The catalyst B is at least one of a metal tin catalyst, an amine catalyst, a bismuth compound catalyst, a morpholine compound catalyst, and an imidazole derivative catalyst.

6. The environmentally friendly primer-free two-component polyurethane sealant according to claim 1, characterized in that: In the adhesion promoter, the double-bond silane coupling agent is at least one of vinyl trimethoxy silane, vinyl tri (b-methoxyethoxy) silane, and γ-methacryloxypropyl trimethoxy silane; The polymerization inhibitor is at least one of a quinone polymerization inhibitor and an inorganic compound polymerization inhibitor; The initiator is at least one selected from azo initiators, diacyl peroxides, hydroperoxides and organic peroxides.

7. The environmentally friendly primer-free two-component polyurethane sealant according to any one of claims 1 to 3, characterized in that: In the component A, the first filler is at least one of carbon black, mica, talc, kaolin, wollastonite, feldspar, syenite, chlorite, bentonite, montmorillonite, calcium carbonate, dolomite, quartz, calcined silica, precipitated silica, fumed silica, cristobalite, calcium oxide, aluminum hydroxide, magnesium oxide, ceramic hollow spheres, glass hollow spheres, organic hollow spheres, and glass beads; The aging aid is at least one of a UV absorber, a light stabilizer and an antioxidant; The dehydrating agent is at least one of a terminal isocyanate compound, triethyl orthoformate, an oxazolidine dehydrating agent, a molecular sieve desiccant, calcium oxide, and a silane dehydrating agent; The first plasticizer is at least one of phthalates, adipates, sulfonates, phosphates, sulfonamides, and chlorinated paraffins; The first catalyst is at least one of dibutyltin diacetate, dibutyltin dilaurate, stannous octoate, dibutyltin dichloride, dibutyltin diacetylacetonate, dioctyltin dilaurate, amine catalysts, bismuth compound catalysts, morpholine compound catalysts, and imidazole derivative catalysts.

8. The environmentally friendly primer-free two-component polyurethane sealant according to any one of claims 1 to 3, characterized in that: In the B component, the terminal hydroxyl compound or the terminal silane compound is at least one of polyether polyol, polyester polyol, polyacrylic acid polyol, polycarbonate polyol, and terminal silane-modified polyether; The second plasticizer is at least one of phthalates, adipates, sulfonates, phosphates, sulfonamides, and chlorinated paraffins; The second filler is at least one of carbon black, mica, talc, kaolin, wollastonite, feldspar, syenite, chlorite, bentonite, montmorillonite, calcium carbonate, dolomite, quartz, calcined silicon dioxide, precipitated silicon dioxide, fumed silica, cristobalite, calcium oxide, aluminum hydroxide, magnesium oxide, ceramic hollow spheres, glass hollow spheres, organic hollow spheres, and glass beads; The curing agent is at least one of a hydroxyl small molecule compound and an amino small molecule compound.

9. A method for preparing the environmentally friendly primer-free two-component polyurethane sealant according to any one of claims 1 to 8, characterized in that: The following steps are involved: Prepare component A and component B separately, wherein: Prepare component A as follows: According to the formulation of component A of the environment-friendly primer-free two-component polyurethane sealant according to any one of claims 1 to 8, various raw materials are taken, and the isocyanate-terminated polyurethane prepolymer, adhesion promoter, first filler, aging aid, first plasticizer and first catalyst in the raw materials of component A are added into a stirring kettle and mixed evenly to obtain component A; Prepare component B as follows: According to the B component formula of the environmentally friendly primer-free two-component polyurethane sealant according to any one of claims 1 to 8, take the raw materials, add any one of the terminal hydroxyl compound or terminal silane compound in the B component raw material, the second plasticizer, the second filler and the curing agent into another stirring kettle and mix them evenly to obtain the B component; The component A and the component B prepared above are put into a rubber hose in a volume ratio of 10:0.95-1.05, mixed and glued, so as to prepare an environmentally friendly primer-free two-component polyurethane sealant.

10. The method for preparing the environment-friendly primer-free two-component polyurethane sealant according to claim 9, characterized in that: The isocyanate-terminated polyurethane prepolymer in the A component is prepared in the following manner, including: At least one of polyether polyol, polyester polyol, polyacrylic polyol and polycarbonate polyol with a molecular weight of 2000-6000 is used as the first component, the first component and plasticizer A are added into a reaction kettle, the temperature is raised to 120° C., vacuum dehydration is performed for 2 hours, and then the temperature is lowered to 60-80° C., and the second component is added, wherein the second component is at least one of aromatic polyisocyanate and aliphatic polyisocyanate, and the reaction is carried out at 60-80° C. for 2-3 hours, and catalyst A is added; the reaction is continued at 80-90° C. for 1-2 hours until the NCO content is less than 1%, and the reaction is stopped to obtain a terminal isocyanate polyurethane prepolymer; The adhesion promoter in the A component is prepared in the following manner, including: Premixing double-bond terminated modified isocyanate prepolymer, double-bond silane coupling agent, polymerization inhibitor and initiator to obtain a premixed solution, taking a solution accounting for 20% of the weight of the premixed solution and adding it into a reactor as a bottom liquid, slowly heating it to 120°C, reacting it for 15 minutes, then dripping the remaining solution into the reactor within 2 to 3 hours using a constant pressure burette, and then keeping it warm for 30 minutes, and discharging the material to obtain an adhesion promoter; The double-bond terminated modified isocyanate prepolymer in the adhesion promoter is prepared in the following manner, including: Add isocyanate compound and hydroxyl-containing acrylate into the reaction kettle, slowly heat up to 60-80°C and react for 2-3h, add catalyst B, continue to react at 80-90°C for 1-2 hours, until the NCO content is lower than 0.1%, stop the reaction, and the double-bond terminated modified isocyanate prepolymer is obtained.