Tungsten oxide-loaded boron fuel and isopyknic impregnation preparation method
The equal volume impregnation of tungsten oxide on boron powder surfaces addresses ignition and combustion issues, enhancing boron fuel's efficiency and cost-effectiveness.
Patent Information
- Application Number
- CN202411228314.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
AI Technical Summary
Boron fuel faces challenges in ignition delay time and combustion exothermic peak due to its low melting point and high boiling point, which hinder its efficient combustion.
An equal volume impregnation method is used to load tungsten oxide on boron powder surfaces, forming a tungsten oxide-loaded boron fuel through steps involving soaking, ultrasonication, stirring, and calcination with an ammonium tungstate aqueous solution.
The method reduces ignition delay time to 52.0 ms to 25.1 ms and achieves a combustion exothermic peak temperature of 643°C to 548°C, with improved combustion performance and economic benefits.
Smart Images

Figure CN119081749A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-energy fuels, relates to boron fuel, and specifically relates to a boron fuel loaded with tungsten oxide and a preparation method thereof by an isovolumetric impregnation method. Background Art
[0002] In the field of high-energy fuels, boron is widely used due to its high energy density and high combustion heat (mass calorific value 58.7 kJ / kg, volume calorific value 135.2 kJ / cm 3 ), which has attracted much attention. However, the practical application of boron is limited by its low melting point (718K) and high boiling point, which is difficult to ignite and low combustion efficiency. The natural oxide layer on the surface of boron, due to its low melting point and high boiling point, easily forms a liquid barrier, adheres to the surface of boron powder, blocks the diffusion of oxygen, hinders the ignition and combustion of boron, and thus reduces its energy release efficiency.
[0003] At present, a variety of methods have been proposed to improve the combustion characteristics of boron, including the addition of metal oxides or high calorific value metals. Studies have shown that the addition of metals such as Al, Mg, Ti, and Fe can interact with boron oxide (B2O3) and play a catalytic role in the entire oxygen transfer process, thereby increasing the oxidation rate of boron. In addition, the addition of metal oxides such as bismuth oxide, copper oxide, Fe2O3, Al2O3, etc. can also significantly improve the combustion performance of boron powder. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a boron fuel loaded with tungsten oxide and a preparation method by an equal volume impregnation method, so as to solve the technical problem that the boron powder fuel in the prior art is difficult to take into account both the ignition delay time and the combustion exothermic peak.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0006] A method for preparing a tungsten oxide-loaded boron fuel, which adopts an equal volume impregnation method to load tungsten oxide on the surface of boron powder to form the tungsten oxide-loaded boron fuel.
[0007] The equal volume impregnation method is to completely impregnate the boron powder in the tungsten-containing impregnation solution, and then dry and calcine it after ultrasonic treatment and stirring to obtain the boron fuel loaded with tungsten oxide.
[0008] The present invention also has the following technical features:
[0009] Specifically, the tungsten-containing impregnation solution is an ammonium tungstate aqueous solution or an ammonium metatungstate aqueous solution.
[0010] Specifically, the volume of the tungsten-containing impregnation solution required for the equal volume impregnation method is the saturated water absorption of the boron powder.
[0011] Specifically, drying and calcination are carried out at 60°C.
[0012] Specifically, the valence state of tungsten in the tungsten oxide is hexavalent, that is, the tungsten oxide is a WO3 species.
[0013] Specifically, the method comprises the following steps:
[0014] Step 1: Add boron powder, and then use deionized water to test the saturated water absorption of the boron powder. The saturated water absorption is the volume of the tungsten-containing impregnation solution required for the boron powder using an equal volume impregnation method.
[0015] Step 2: Weigh the boron powder into a small beaker and add a magnet.
[0016] Step 3: Use a pipette to transfer the prepared tungsten-containing impregnation solution with a concentration of 0.01 mol / L to 0.2 mol / L, and add deionized water to dilute it to the volume of tungsten-containing impregnation solution required for the boron powder, and then add it dropwise to the boron powder in step 2 to completely soak the boron powder, seal it, ultrasonicate it for 5 minutes, and then stir it for 1 hour.
[0017] Step 4: Place the mixture in an oven for drying and calcination to obtain a boron fuel loaded with tungsten oxide.
[0018] Preferably, the method specifically comprises the following steps:
[0019] Step 1: Add 1g of boron powder into a beaker, and then use deionized water to test the saturated water absorption of the boron powder. The saturated water absorption is the volume of tungsten-containing impregnation solution required for 1g of boron powder using an equal volume impregnation method.
[0020] Step 2: Weigh 1g of boron powder into a small beaker and add a magnet.
[0021] Step 3: Use a pipette to transfer the prepared tungsten-containing impregnation solution with a concentration of 0.01 mol / L to 0.2 mol / L, and add deionized water to dilute it to the volume of tungsten-containing impregnation solution required for 1 g of boron powder, and then add it dropwise to the boron powder in step 2 to completely soak the boron powder, seal the mouth of the beaker with a sealing film, ultrasonicate for 5 minutes, and then stir for 1 hour.
[0022] Step 4: Place the mixture in an oven at 60° C. for drying and calcination to obtain a tungsten oxide-loaded boron fuel.
[0023] The present invention also protects a tungsten oxide loaded boron fuel, which is prepared by the above-mentioned preparation method of the tungsten oxide loaded boron fuel. The tungsten oxide content in the tungsten oxide loaded boron fuel is 0.1wt.% to 20wt.%.
[0024] Preferably, the content of tungsten oxide in the tungsten oxide-loaded boron fuel is 1 wt.% to 20 wt.%.
[0025] Specifically, the laser ignition delay time of the boron fuel loaded with tungsten oxide is 52.0 ms to 25.1 ms.
[0026] Specifically, the temperature corresponding to the combustion exothermic peak of the boron fuel loaded with tungsten oxide is 643°C to 548°C.
[0027] Compared with the prior art, the present invention has the following technical effects:
[0028] (I) The laser ignition delay time of the boron fuel loaded with tungsten oxide compound prepared by the present invention is 52.0 ms to 25.1 ms, and the temperature corresponding to the combustion exothermic peak is 643° C. to 548° C.
[0029] (II) Compared with the prior art, the boron fuel loaded with tungsten oxide compound prepared by the present invention has the advantages of good repeatability, high cleanliness and high combustion performance.
[0030] (III) Compared with other complex preparation methods, such as nanotechnology or chemical vapor deposition, the preparation method of the present invention is easier to mass produce and has higher economic benefits. Compared with the traditional physical blending method, it can achieve uniform and effective distribution of WO3 on the surface of boron powder, and its good repeatability and consistency make it have broad application prospects and competitiveness in the field of explosives.
[0031] (IV) The preparation method of the present invention adopts the isovolumetric impregnation method, which is relatively simple in synthesis process, has low equipment requirements, and mild conditions. At the same time, the experimental drugs are all common drugs in laboratories, and the production cost is low.
[0032] (V) The preparation method of the present invention has good repeatability and low price, which greatly reduces the preparation cost of boron fuel and has good competitiveness and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 These are SEM images of WO3 / B fuel samples prepared by the equal volume impregnation method: A1 is 1wt.%-WO3 / B; A2 is 3.5wt.%-WO3 / B; A3 is 7wt.%-WO3 / B; A4 is 20wt.%-WO3 / B.
[0034] Figure 2 This is the SEM element distribution mapping (B, O, W element distribution) image of the 7wt.%-WO3 / B fuel sample prepared by the equal volume impregnation method.
[0035] Figure 3XRD data of boron powder raw material and WO3 / B fuel sample prepared by equal volume impregnation method: A0 is boron raw material; A1 is 1wt.%-WO3 / B; A2 is 3.5wt.%-WO3 / B; A3 is 7wt.%-WO3 / B; A4 is 20wt.%-WO3 / B.
[0036] Figure 4 XPS spectra of WO3 / B fuel samples prepared by equal volume impregnation method (B1s; W4f; O1s): B1 is 1wt.%-WO3 / B; B2 is 3.5wt.%-WO3 / B; B3 is 7wt.%-WO3 / B.
[0037] Figure 5 The DSC curves of boron powder raw material and WO3 / B fuel sample prepared by equal volume impregnation method: B0 is boron raw material; B1 is 1wt.%-WO3 / B; B2 is 3.5wt.%-WO3 / B; B3 is 7wt.%-WO3 / B; B4 is 20wt.%-WO3 / B.
[0038] Figure 6 TG curves of boron powder raw material and WO3 / B fuel sample prepared by equal volume impregnation method: B0 is boron raw material; B1 is 1wt.%-WO3 / B; B2 is 3.5wt.%-WO3 / B; B3 is 7wt.%-WO3 / B; B4 is 20wt.%-WO3 / B.
[0039] Figure 7 Laser ignition delay time data of boron powder raw material and WO3 / B fuel sample prepared by equal volume impregnation method.
[0040] The specific contents of the present invention are further explained in detail below in conjunction with embodiments. DETAILED DESCRIPTION
[0041] It should be noted that, unless otherwise specified, all materials and equipment in the present invention are materials and equipment known in the art. For example, the atomic layer deposition equipment is an atomic layer deposition equipment known in the prior art.
[0042] In the present invention, boron powder refers to boron particles, and the two are the same concept. The boron powder is amorphous boron powder and / or crystalline boron powder, and the particle size distribution of the boron powder is from micron to nanometer.
[0043] WO3 / B refers to boron fuel loaded with tungsten oxide.
[0044] Tungsten oxide has good catalytic properties, can promote the oxidation reaction of boron, reduce the ignition temperature of boron, improve combustion efficiency, and has the advantages of improving the cleanliness and safety of combustion. Boron-based fuels require high-temperature stable catalysts in high-temperature explosives and tungsten oxide can meet this requirement, thereby ensuring the stability and efficiency of the combustion process. Therefore, loading tungsten oxide on the surface of boron powder as an active catalyst is expected to make the application prospects of boron-based fuels in high-energy fuels and propellants broader. Therefore, the present invention adopts an impregnation method to compound with boron powder to obtain a boron fuel loaded with tungsten oxide with excellent combustion performance, which effectively promotes the application of boron-based fuels in the field of explosives and pyrotechnics.
[0045] The tungsten oxide-loaded boron fuel of the present invention is used as a boron-based fuel in the field of explosives.
[0046] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0047] Embodiment 1:
[0048] This embodiment provides a method for preparing a boron fuel loaded with tungsten oxide, the method comprising the following steps:
[0049] Step 1: Add 1g of boron powder into a beaker, and then use deionized water to test the saturated water absorption of the boron powder. The saturated water absorption is the volume of tungsten-containing impregnation solution required for 1g of boron powder using the equal volume impregnation method.
[0050] Step 2: Weigh 1g of boron powder into a small beaker and add a magnet.
[0051] Step 3: Use a pipette to transfer the prepared tungsten-containing impregnation solution, which is (NH4)6H2W 12 O 40 xH2O aqueous solution; add deionized water to dilute to the volume of tungsten-containing impregnation solution required for 1g of boron powder, and then add it dropwise to the boron powder in step 2 to completely soak the boron powder, seal the beaker with a sealing film, ultrasonicate for 5min, and then stir for 1h.
[0052] Step 4: Place the mixture in an oven at 60° C. for drying and calcination to obtain a tungsten oxide-loaded boron fuel.
[0053] In this embodiment, the reaction equation of the equal volume impregnation method is:
[0054]
[0055] In this embodiment, the concentration of the tungsten-containing impregnation solution is adjusted within the range of 0.01 mol / L to 0.2 mol / L, so that the contents of tungsten oxide in the boron fuel loaded with tungsten oxide are 1 wt.%, 3.5 wt.%, 7 wt.% and 20 wt.%, respectively.
[0056] Figure 1 The SEM images of WO3 / B fuel samples prepared by equal volume impregnation method: A1 is 1wt.%-WO3 / B; A2 is 3.5wt.%-WO3 / B; A3 is 7wt.%-WO3 / B; A4 is 20wt.%-WO3 / B. From the SEM images, the morphology of 1%-20% WO3 / B is similar, and there is little change compared with the morphology of B raw material, indicating that WO3 is highly dispersed on B raw material, and the deposition of WO3 does not significantly change the morphology of boron raw material.
[0057] Figure 2 This is the SEM element distribution mapping (B, O, W element distribution) picture of the 7wt.%-WO3 / B fuel sample prepared by the equal volume impregnation method. The distribution range of W and O elements is completely consistent with that of B element, indicating that the deposited WO3 is highly dispersed on the surface of the boron fuel, and also indicating that the preparation of WO3 / B by the equal volume impregnation method is successful.
[0058] Figure 3 XRD data of boron powder raw material and WO3 / B fuel sample prepared by equal volume impregnation method: A0 is boron raw material; A1 is 1wt.%-WO3 / B; A2 is 3.5wt.%-WO3 / B; A3 is 7wt.%-WO3 / B; A4 is 20wt.%-WO3 / B. The diffraction peaks of 1%-7% WO3 / B samples are similar to those of boron raw materials, which also shows that WO3 is highly dispersed on the surface of boron powder and is amorphous. When the WO3 content increases to 20%, a new diffraction peak appears, which belongs to the diffraction peak of WO3. This is because when the content is 20%, the size or thickness of the deposited particles becomes larger, so the diffraction peak appears.
[0059] Figure 4 The XPS spectra of WO3 / B fuel samples prepared by equal volume impregnation method (B1s; W4f; O1s): B1 is 1wt.%-WO3 / B; B2 is 3.5wt.%-WO3 / B; B3 is 7wt.%-WO3 / B. From the B1s spectrum, the peak with a binding energy of 187.7eV is attributed to zero-valent boron, and the peak intensity decreases significantly with the increase of WO3 content. This is because the number of WO3 species on the surface of the boron powder increases, and the particles cover part of B, resulting in a decrease in surface exposed B, so the corresponding peak decreases. The peak at 35.9eV in the W4f spectrum is attributed to W 6+,Combined with the O1s spectrum, it can be determined that the species deposited on the surface of the boron powder is WO3.With the increase of WO3 content in the sample, the peak area of W4f increases, and the change of O1s with the increase of WO3 content is not obvious.
[0060] Embodiment 2:
[0061] This embodiment provides a tungsten oxide loaded boron fuel, which is prepared by the preparation method of the tungsten oxide loaded boron fuel given in Example 1, wherein the content of tungsten oxide in the tungsten oxide loaded boron fuel is 1wt.%, 3.5wt.%, 7wt.% and 20wt.%, respectively.
[0062] This embodiment provides a TG-DSC test of a boron fuel loaded with a tungsten oxide compound. The method of the TG-DSC test is: weigh an appropriate amount of the boron fuel loaded with a tungsten oxide compound and place it on the sample stage of the TG-DSC instrument, set the instrument's heating rate to 10°C / min, the test temperature range to room temperature-900°C, and the test atmosphere to air atmosphere, so that the TG and DSC curves of the boron fuel loaded with a tungsten oxide compound can be obtained.
[0063] Figure 5 The DSC curves of the boron powder raw material and the WO3 / B fuel sample prepared by the equal volume impregnation method are shown below: B0 is the boron raw material; B1 is 1wt.%-WO3 / B; B2 is 3.5wt.%-WO3 / B; B3 is 7wt.%-WO3 / B; B4 is 20wt.%-WO3 / B. The temperature corresponding to the oxidation peak (i.e., the combustion exothermic peak) of the boron raw material is 660°C, the temperature corresponding to the oxidation peak of the 1wt.%-WO3 / B sample is 643°C, the temperature corresponding to the oxidation peak of the 3.5wt.%-WO3 / B sample is 557°C, the temperature corresponding to the oxidation peak of the 7wt.%-WO3 / B sample is 555°C, and the temperature corresponding to the oxidation peak of the 20wt.%-WO3 / B sample is 548°C. When the WO3 content increases to 3.5%, the oxidation exothermic peak temperature of the sample will decrease significantly. At this time, as the WO3 content continues to increase, the temperature corresponding to the oxidation exothermic peak of the sample decreases very slowly.
[0064] Figure 6 The TG curves of boron powder raw materials and WO3 / B fuel samples prepared by equal volume impregnation method are shown in Figure 2: B0 is boron raw material; B1 is 1wt.%-WO3 / B; B2 is 3.5wt.%-WO3 / B; B3 is 7wt.%-WO3 / B; B4 is 20wt.%-WO3 / B. Figure 5 This is consistent with the DSC results in .
[0065] Embodiment 3:
[0066] This embodiment provides a tungsten oxide loaded boron fuel, which is prepared by the preparation method of the tungsten oxide loaded boron fuel given in Example 1, wherein the content of tungsten oxide in the tungsten oxide loaded boron fuel is 1wt.%, 3.5wt.%, 7wt.% and 20wt.%, respectively.
[0067] This example provides an ignition delay time test of boron fuel loaded with tungsten oxide compounds. The method of the ignition delay time test is: weigh an appropriate amount of boron fuel loaded with tungsten oxide compounds and place it on the sample stage of the laser ignition instrument, and set the instrument parameters to frequency Hz: 1000; duty cycle (1-40%): 3; number of pulses: 1000; pulse train light; power: 40W; pulse energy: 40mJ; pulse width: 30μs. In this way, the ignition delay time data of the WO3 / B fuel sample can be obtained.
[0068] Figure 7 The laser ignition delay time data of boron powder raw material and WO3 / B fuel sample prepared by equal volume impregnation method. The ignition delay time of boron powder is 51.8ms, the ignition delay time of 1wt.%-WO3 / B is 52.0ms, the ignition delay time of 3.5wt.%-WO3 / B is shortened to 46.0ms, the ignition delay time of 7wt.%-WO3 / B is shortened to 35.0ms, and the ignition delay time of 20wt.%-WO3 / B is shortened to 25.1ms. Compared with boron powder, 1% WO3 has little effect on the ignition delay time of the sample, and its ignition delay time is significantly shortened with the increase of WO3 content.
Claims
1. A method for preparing a boron fuel loaded with tungsten oxide, characterized in that: The method adopts an equal volume impregnation method to load tungsten oxide on the surface of boron powder to form a boron fuel loaded with tungsten oxide; The equal volume impregnation method is to completely soak the boron powder in the tungsten-containing impregnation solution, and after ultrasonication and stirring, dry and calcine to obtain the boron fuel loaded with tungsten oxide.
2. The method for preparing the tungsten oxide-loaded boron fuel according to claim 1, characterized in that: The tungsten-containing impregnation solution is an ammonium tungstate aqueous solution or an ammonium metatungstate aqueous solution.
3. The method for preparing the tungsten oxide-loaded boron fuel according to claim 1, characterized in that: The volume of the tungsten-containing impregnation solution required for the equal volume impregnation method is the saturated water absorption of the boron powder.
4. The method for preparing the tungsten oxide-loaded boron fuel according to claim 1, characterized in that: The drying and calcination were carried out at 60°C.
5. The method for preparing the tungsten oxide-loaded boron fuel according to claim 1, characterized in that: The valence state of tungsten in the tungsten oxide is hexavalent.
6. The method for preparing the tungsten oxide-loaded boron fuel according to claim 1, characterized in that: The method specifically comprises the following steps: Step 1, adding boron powder, and then testing the saturated water absorption of the boron powder with deionized water, wherein the saturated water absorption is the volume of the tungsten-containing impregnation solution required for the boron powder using an equal volume impregnation method; Step 2: weigh boron powder and pour it into a small beaker, and add a magnet; Step 3: Use a pipette to transfer the prepared tungsten-containing impregnation solution with a concentration of 0.01 mol / L to 0.2 mol / L, add deionized water to dilute it to the volume of the tungsten-containing impregnation solution required by the boron powder, and then add it dropwise to the boron powder in step 2 to completely infiltrate the boron powder, seal, sonicate, and then stir; Step 4: Place the mixture in an oven for drying and calcination to obtain a boron fuel loaded with tungsten oxide.
7. A boron fuel loaded with tungsten oxide, characterized in that: The boron fuel is prepared by the preparation method of the tungsten oxide-loaded boron fuel according to any one of claims 1 to 6; the content of tungsten oxide in the tungsten oxide-loaded boron fuel is 0.1wt.% to 20wt.%.
8. The tungsten oxide-loaded boron fuel according to claim 7, characterized in that: The content of tungsten oxide in the tungsten oxide-loaded boron fuel is 1wt.% to 20wt.%.
9. The tungsten oxide-loaded boron fuel according to claim 7, characterized in that: The laser ignition delay time of the boron fuel loaded with tungsten oxide is 52.0ms to 25.1ms.
10. The tungsten oxide-loaded boron fuel according to claim 7, characterized in that: The temperature corresponding to the combustion exothermic peak of the boron fuel loaded with tungsten oxide is 643°C to 548°C.