Preparation method of potassium-containing metal spheroidizing agent core-spun yarn

By rationally preparing and treating elements such as magnesium, calcium, rare earths and other elements in the core wire, and using potassium fluoride powder and cover agent, the operation risk of high magnesium core wire in the spheroidization reaction and the low magnesium absorption rate are solved. , the absorption rate of magnesium and graphite spheroidization rate are improved, and the spheroidization effect and structure of the casting are improved.

CN119082401APending Publication Date: 2024-12-06YUZHOU HENGLILAI ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411200052.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The core wire with high magnesium content causes operational hazards, carbide formation, magnesium gas escape and low absorption rate during spheroidization reaction, affecting the spheroidization effect, and potassium is easy to oxidize and volatilize, making it difficult to disperse evenly in the metal solution, reducing Its effectiveness.

Method used

It consists of 48.0-52.0% ferrosilicon, 6.5-7.5% silicon calcium, 6.5-7.5% rare earth silicon, 0.7-1.0% pure lanthanum rare earth, 11.0-13.0% magnesium ingots, and 19.0-27.3% scrap steel The core-encapsulated wire is formed by smelting, casting, crushing, mixing and rolling steps, and the covering agent and potassium fluoride powder are added. The nitrogen protection and alternating filling feeding technology are used to form a core-encapsulated wire containing potassium metal spheroidizer to improve magnesium dissolution. and distribution, reduce oxidation, enhance potassium deoxygenation and desulfurization capabilities.

Benefits of technology

The absorption rate of magnesium and graphite spheroidization rate are improved, the operation risk and reaction instability are reduced, the spheroidization effect and tissue structure of the casting are significantly improved, and the white mouth defects and casting distortion are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017617030000061
    Figure BDA0005017617030000061
  • Figure BDA0005017617030000071
    Figure BDA0005017617030000071
  • Figure BDA0005017617030000072
    Figure BDA0005017617030000072
Patent Text Reader

Abstract

The invention discloses a preparation method of a potassium-containing metal spheroidizing agent core-spun yarn, and relates to the technical field of core-spun yarns, the potassium-containing metal spheroidizing agent core-spun yarn is composed of 48.0%-52.0% of silicon iron, 6.5%-7.5% of silicon calcium, 6.5%-7.5% of rare earth silicon, 0.7%-1.0% of pure lanthanum rare earth, 11.0%-13.0% of magnesium ingots and 19.0%-27.3% of waste steel. According to the preparation method of the potassium-containing metal spheroidizing agent cored wire, dissolution and distribution of magnesium in molten steel can be improved by filling and adding the covering agent and the potassium fluoride powder, magnesium is helped to be absorbed more effectively, and therefore the utilization rate of magnesium is increased, the covering agent added in the smelting process can improve the slagging capacity, meanwhile, reducing gas is formed, and the magnesium is prevented from being smelted. When the cored wire is fed into high-temperature molten metal, the content of effective magnesium in residual magnesium in the molten iron is increased, generated sulfide can serve as a heterogeneous nucleation core of graphite nodules, the graphite spheroidization rate can be remarkably increased, and spheroidization recession and graphite distortion and anti-white defect of large-section ductile iron can be effectively simulated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cored wires, and more particularly to a method for preparing a cored wire containing a potassium metal spheroidizer. Background Art

[0002] The wire feeding process is to crush the various additives and spheroidizing agents that need to be added to the molten iron into a certain particle size, and then wrap it with a cold-rolled steel strip to form a composite additive material of any length (commonly known as alloy cored wire). Then, with the help of a special wire feeding machine for casting, the alloy cored wire is continuously fed into the bottom of the molten iron in the processing bag. Due to the action of the high-temperature molten iron, the steel strip is melted, and the alloy elements immediately come into contact with the molten iron to achieve the purpose of desulfurization, spheroidization, and composition adjustment.

[0003] The cored wire contains alloy magnesium (Mg), and its main function is to improve the performance of the final product by utilizing the characteristics of magnesium. However, due to the high magnesium content in the cored wire, the spheroidization reaction will be fierce, which not only increases the danger of operation, but also the high magnesium content will lead to the formation of carbides and increase the tendency of white cast iron. At the same time, the solubility of magnesium in molten iron is limited, so that a large amount of magnesium escapes in the form of gas, thereby reducing the absorption rate of magnesium and affecting the spheroidization effect. In order to improve the absorption rate of magnesium and reduce the degree of reaction, potassium is added to the cored wire. Potassium can improve the dissolution and distribution of magnesium in molten steel, help magnesium to be absorbed more effectively, and at the same time, it can significantly improve the graphite spheroidization rate and eliminate the irregular graphite of rare earth ductile iron. However, because potassium is very active and easily oxidized and volatilized, potassium can react quickly with oxygen in the air to form potassium oxide. This oxide layer prevents potassium from further reacting with the metal solution. At the same time, due to its low density, when added to the metal solution, potassium tends to float on the surface instead of being evenly dispersed throughout the solution, which affects its effectiveness as an alloying component.

[0004] Therefore, it is necessary to propose a method for preparing a cored wire containing a potassium metal spheroidizer to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to solve the problems raised in the above background technology and provide a method for preparing a cored wire containing a potassium metal spheroidizer.

[0006] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0007] A method for preparing a potassium-containing metal nodulizer cored wire, comprising 48.0-52.0% ferrosilicon, 6.5-7.5% calcium silicon, 6.5-7.5% rare earth silicon, 0.7-1.0% pure lanthanum rare earth, 11.0-13.0% magnesium ingot, and 19.0-27.3% scrap steel;

[0008] The method for preparing a potassium metal spheroidizing agent cored wire comprises the following steps:

[0009] S1. Melting: The magnesium ingot and ferrosilicon are placed in a medium frequency furnace for melting, and calcium silicon, rare earth silicon and scrap steel are added in sequence. During the melting, a covering agent is added to the furnace, and nitrogen is introduced into the medium frequency furnace as a protective gas. The melting temperature is 1210-1260° C., and the melting time is 0.4-0.5 hours. After melting, an alloy melt is obtained;

[0010] S2, casting: pouring the alloy melt into a metal ingot mold to obtain an alloy ingot;

[0011] S3, crushing: crush the alloy ingot into 4mm-8mm alloy blocks using a jaw crusher, and then crush the alloy blocks using a granulator, and then pass through a 6-8 mesh sieve to obtain alloy powder;

[0012] S4, mixing: the alloy powder is divided into two parts, the first part of the alloy powder and potassium fluoride powder are placed in a three-dimensional mixer for uniform mixing, and the cored wire mixture is obtained after the mixing time is 0.2-0.5 hours, and the second part of the alloy powder is reserved;

[0013] S5. Inspection: Test the cored wire mixture and the second batch of alloy powder, and keep them for later use after they pass the test;

[0014] S6. Coiling: Use Q195 cold-rolled steel strip to weigh the first mixed material and the second alloy powder separately on the cored wire machine, feed them into the cored wire machine for coating by alternating feeding, then use a winding machine to roll the cored wire into a coil, finally inspect and package the coil to obtain the finished cored wire.

[0015] Preferably, the amount of the covering agent added in step S1 is 0.5%-1.0% of the total mass of the raw materials, and the composition of the covering agent is 50-60% potassium fluoride and 40-50% graphite powder.

[0016] Preferably, during the casting in step S2, the distance between the medium frequency furnace mouth and the ingot mold is 100-400 mm.

[0017] Preferably, the crushing and screening in step S3 are performed in an argon protection environment.

[0018] Preferably, the diameter of the potassium fluoride powder in the mixed material in step S4 is 0.1-0.2 mm, and the particle size of the alloy powder is less than 2.5 mm.

[0019] Preferably, when the steel strip is wrapped around the core wire mixture in step S7, the interface of the steel strip is mechanically engaged.

[0020] Preferably, the composition of the alloy powder obtained by crushing in step S3 is silicon: 40.0%-46.0%, calcium: 2.0%-3.0%, lanthanum: 0.8%-1.0%, cerium: 1.6%-2.0%, magnesium: 10.0%-12.0%, aluminum: 0.5%-0.8%, and the rest is 33%-43% iron and less than 2.0% unavoidable impurities.

[0021] Preferably, the amount of potassium fluoride powder added to the mixed material in step S4 is 4.6-5.6% of the mass of the first alloy powder.

[0022] Preferably, the distance of alternating filling and feeding during S6 rolling is 5 mm.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. By filling and adding covering agent and potassium fluoride powder, the dissolution and distribution of magnesium in molten steel can be improved, and magnesium can be absorbed more effectively, thereby improving the utilization rate of magnesium. The covering agent added during smelting can enhance the slag-making ability and form reducing gas to reduce the oxidation of magnesium. When the cored wire is sent into the high-temperature molten metal, according to the principle of thermal reduction, potassium fluoride reacts with silicon in the molten iron at high temperature to reduce potassium. By utilizing the strong deoxidation and desulfurization ability of potassium, the content of oxygen and sulfur in the molten metal is significantly reduced, and the effective magnesium content in the residual magnesium in the molten iron is increased. Moreover, the generated sulfide can be used as the heterogeneous nucleation core of graphite nodules, which can significantly improve the graphite spheroidization rate, greatly increase the graphite number and refine the matrix structure of the casting, and effectively simulate the spheroidization recession and the graphite distortion and anti-white defects of large-section ductile iron.

[0025] 2. The setting of alternating filling and feeding of cored wire mixture and alloy powder can avoid the situation where continuous addition of potassium will cause a sudden increase in local concentration and trigger an unstable reaction. Adding in batches can avoid this risk and improve the safety of operation. At the same time, it can achieve more precise control of the total amount of potassium and the timing of addition, avoiding uncontrollable reactions or waste caused by excessive addition at one time. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] 20 Examples of Embodiments:

[0028] The composition is composed of 49.3% ferrosilicon, 6.9% calcium silicon, 7.0% rare earth silicon, 0.8% pure lanthanum rare earth, 12.4% magnesium ingot, and 23.6% scrap steel;

[0029] The amount of covering agent added is 0.6% of the total mass of the raw materials, and the composition of the covering agent is a mixture of 55% potassium fluoride and 45% graphite powder;

[0030] The amount of potassium fluoride powder added is 5.0% of the mass of the first alloy powder;

[0031] The method for preparing a potassium metal spheroidizing agent cored wire comprises the following steps:

[0032] S1. Smelting: the magnesium ingot and ferrosilicon are placed in a medium frequency furnace for melting, and calcium silicon, rare earth silicon and scrap steel are added in sequence. During smelting, a covering agent is added to the furnace, and nitrogen is introduced into the medium frequency furnace as a protective gas. The smelting temperature is 1250° C. and the smelting time is 0.45 hours. After smelting, an alloy melt is obtained;

[0033] S2, casting: pouring the alloy melt into a metal ingot mold to obtain an alloy ingot. During casting, the distance between the medium frequency furnace mouth and the ingot mold is 150 mm;

[0034] S3, crushing: crushing the alloy ingot into alloy blocks less than 6 mm by using a jaw crusher, and then crushing the alloy blocks by using a granulator. After crushing, the alloy powder is obtained by passing through a 6-mesh sieve. The composition of the alloy powder is 43.0% silicon, 2.5% calcium, 0.9% lanthanum, 1.8% cerium, 11.5% magnesium, 0.6% aluminum, and the rest is 38% iron and 1.7% inevitable impurities;

[0035] S4, mixing: the alloy powder is divided into two parts, the first part of the alloy powder and potassium fluoride powder are placed in a three-dimensional mixer for uniform mixing, and the cored wire mixture is obtained after the mixing time is 0.4 hours, and the second part of the alloy powder is reserved;

[0036] S5. Inspection: Test the cored wire mixture and the second batch of alloy powder, and keep them for later use after they pass the test;

[0037] S6. Coiling: Use Q195 cold-rolled steel strip to weigh the first mixed material and the second alloy powder separately on the cored wire machine, feed them into the cored wire machine for coating by alternating feeding, then use a winding machine to roll the cored wire into a coil, finally inspect and package the coil to obtain the finished cored wire.

[0038] Twenty rolls of the same QX-10K new potassium-containing spheroidized cored wire were produced according to the same production steps and parameters and were applied to the bottom of the molten iron in the same type of treatment ladle.

[0039] 20 cases of comparative example:

[0040] The composition is composed of 53.6% ferrosilicon, 7.4% calcium silicon, 1.9% rare earth silicon, 0.8% pure lanthanum rare earth, 30.8% magnesium ingot, and 5.4% scrap steel;

[0041] The cored wire preparation method comprises the following steps:

[0042] S1. Melting: Place the magnesium ingot and ferrosilicon in a medium frequency furnace for melting, add silicon calcium, rare earth silicon and scrap steel in sequence, and introduce nitrogen into the medium frequency furnace as a protective gas. The melting temperature is 1250° C. and the melting time is 0.45 hours. After melting, an alloy melt is obtained;

[0043] S2, casting: pouring the alloy melt into a metal ingot mold to obtain an alloy ingot. During casting, the distance between the medium frequency furnace mouth and the ingot mold is 150 mm;

[0044] S3, crushing: crushing the alloy ingot into alloy blocks less than 6 mm by using a jaw crusher, and then crushing the alloy blocks by using a granulator. After crushing, the alloy powder is passed through a 6-mesh sieve to obtain the alloy powder, and the composition of the obtained alloy powder is 43.0% silicon, 2.5% calcium, 0.8% lanthanum, 1.9% cerium, 30.8% magnesium, 0.7% aluminum, and the rest is 17.35% iron and 2.5% inevitable impurities;

[0045] S4. Inspection: Test the alloy powder and keep it ready for use after it passes the test;

[0046] S5. Coiling: Use Q195 cold-rolled steel strip to coat the alloy powder on a cored wire machine and make cored wire, then use a wire winding machine to roll the cored wire into a coil, and finally inspect and package the coil to obtain the finished cored wire.

[0047] Twenty rolls of the same QX-30 common spheroidized cored wire were produced according to the same production steps and parameters as 20 comparative cases, and were applied to the bottom of the molten iron in the same treatment ladle as in the embodiment.

[0048] Under the same parameters, 20 rolls of QX-30 common spheroidized cored wire of the comparative example and 20 rolls of QX-10K new potassium-containing spheroidized cored wire of the embodiment were used in the same batch of the same type of treatment packages to compare various performance parameters. The performance parameters compared were spheroidized wire length, residual magnesium content, magnesium absorption rate and spheroidization rate:

[0049] Table 1, data of 20 rolls of comparative ratio applied to the same batch of processing packages are as follows:

[0050]

[0051]

[0052] Table 2, data of 20 volumes of the embodiment applied to the same batch of processing packages are as follows:

[0053]

[0054] Referring to Table 1 and Table 2, when the two groups of cored wires are applied to the same treatment package, the absorption rate of magnesium in Table 2 is 38.66%, which is higher than the absorption rate of 30.55% in Table 1, and is 26.55% higher than the original absorption rate; the length of the spheroidizing wire is reduced by an average of 2.2 meters, and the length of the spheroidizing wire directly affects the production cost. The shorter the length of the spheroidizing wire, the lower the cost; the spheroidizing rate is increased from 88.38% to 90.75%, an average increase of 2.37%.

[0055] It can be seen that the preparation method can not only reduce the magnesium content in the core material of the cored wire, reduce the amount of coated wire added, and improve the absorption rate of magnesium, but also improve the quality of the molten iron during spheroidization, increase the spheroidization rate of the casting by 2.37 percentage points, and ensure the quality of the casting.

Claims

1. A method for preparing a cored wire containing a potassium metal nodulizer, characterized in that: It is composed of 48.0-52.0% ferrosilicon, 6.5-7.5% calcium silicon, 6.5-7.5% rare earth silicon, 0.7-1.0% pure lanthanum rare earth, 11.0-13.0% magnesium ingot, and 19.0-27.3% scrap steel; The method for preparing a potassium metal spheroidizing agent cored wire comprises the following steps: S1. Melting: The magnesium ingot and ferrosilicon are placed in a medium frequency furnace for melting, and calcium silicon, rare earth silicon and scrap steel are added in sequence. During the melting, a covering agent is added to the furnace, and nitrogen is introduced into the medium frequency furnace as a protective gas. The melting temperature is 1210-1260° C., and the melting time is 0.4-0.5 hours. After melting, an alloy melt is obtained; S2, casting: pouring the alloy melt into a metal ingot mold to obtain an alloy ingot; S3, crushing: crush the alloy ingot into 4mm-8mm alloy blocks using a jaw crusher, and then crush the alloy blocks using a granulator, and then pass through a 6-8 mesh sieve to obtain alloy powder; S4, mixing: the alloy powder is divided into two parts, the first part of the alloy powder and potassium fluoride powder are placed in a three-dimensional mixer for uniform mixing, and the cored wire mixture is obtained after the mixing time is 0.2-0.5 hours, and the second part of the alloy powder is reserved; S5. Inspection: Test the cored wire mixture and the second batch of alloy powder, and keep them for later use after they pass the test; S6. Coiling: Use Q195 cold-rolled steel strip to weigh the first mixed material and the second alloy powder separately on the cored wire machine, feed them into the cored wire machine for coating by alternating feeding, then use a winding machine to roll the cored wire into a coil, finally inspect and package the coil to obtain the finished cored wire.

2. The method for preparing a potassium-containing metal spheroidizer cored wire according to claim 1, characterized in that: The amount of covering agent added in step S1 is 0.5%-1.0% of the total mass of the raw materials, and the composition of the covering agent is 50-60% potassium fluoride and 40-50% graphite powder.

3. The method for preparing a potassium-containing metal spheroidizing agent cored wire according to claim 1, characterized in that: During the casting in step S2, the distance between the medium frequency furnace mouth and the ingot mold is 100-400 mm.

4. The method for preparing a potassium-containing metal spheroidizer cored wire according to claim 1, characterized in that: The crushing and screening in step S3 are performed in an argon protection environment.

5. The method for preparing a potassium-containing metal spheroidizer cored wire according to claim 1, characterized in that: The diameter of the potassium fluoride powder in the mixed material of step S4 is 0.1-0.2 mm, and the particle size of the alloy powder is less than 2.5 mm.

6. The method for preparing a potassium-containing metal spheroidizer cored wire according to claim 1, characterized in that: When the steel strip is wrapped around the core wire mixture in step S7, the interface of the steel strip is mechanically engaged.

7. The method for preparing a potassium-containing metal spheroidizer cored wire according to claim 1, characterized in that: The alloy powder obtained by the pulverization in step S3 has the following components: silicon: 40.0%-46.0%, calcium: 2.0%-3.0%, lanthanum: 0.8%-1.0%, cerium: 1.6%-2.0%, magnesium: 10.0%-12.0%, aluminum: 0.5%-0.8%, and the rest is 33%-43% iron and less than 2.0% inevitable impurities.

8. The method for preparing a potassium-containing metal spheroidizer cored wire according to claim 1, characterized in that: The amount of potassium fluoride powder added to the mixed material in step S4 is 4.6-5.6% of the mass of the first batch of alloy powder.