Method for recovering molybdenum and vanadium from hydrogenation waste catalyst metal ash
By treating the hydrogenation waste catalyst under water vapor and oxygen conditions and performing aerobic roasting, the problems of low recovery rate and environmental pollution in the prior art are solved, and efficient, simple and environmentally friendly molybdenum and vanadium recycling are achieved, and high Recycled product of purity.
Patent Information
- Application Number
- CN202411198756.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing methods for recycling molybdenum vanadium from waste catalysts have problems such as low metal recovery rate, poor environmental friendliness, complex processes and high costs.
The hydrogenation waste catalyst metal ash slag is treated at high temperature in the presence of water vapor and oxygen, followed by aerobic roasting, and leaching with alkali liquid. Ammonium metavanadate and molybdate are obtained through crystallization and separation, which simplifies the process flow. Improve recovery and purity.
The recovery rate of molybdenum and vanadium components is improved, the recycling process flow is simplified, environmental pollution is reduced, process costs are reduced, and high-purity ammonium metavanadate and molybdate solids are obtained.
Smart Images

Figure BDA0005017270740000091 
Figure BDA0005017270740000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal recovery and extraction, and in particular to a method for recovering molybdenum and vanadium from metal ash residue of hydrogenation waste catalyst. Background Art
[0002] At present, the methods for recovering molybdenum and vanadium from waste catalysts are divided into chemical recovery and physical recovery. Chemical recovery includes wet recovery and pyrolysis, or a combination of the two. Pyrolysis generally involves mixing waste catalysts and salt substances in a certain proportion, and then calcining them at high temperature under aerobic conditions. High-temperature calcination has two main purposes. First, a large amount of carbon is converted into volatile gases, such as carbon dioxide, at high temperatures to achieve the purpose of carbon removal; second, the existence form and valence state of valuable metals are changed and converted into soluble metal compounds. The calcined product is then leached with a leaching solution to obtain a leaching solution containing soluble metal compounds. Although the metal recovery efficiency of the calcination-leaching process is very high, the energy consumption of the calcination process is high, and a large amount of waste liquid with high salt content is generated, causing environmental pollution. Wet recovery usually involves directly dissolving the waste catalyst with a solution when the carbon content is low. The solution leaching method, based on the difference in the solubility of different metals in acid / alkaline solutions, can achieve the gradual separation and recovery of multiple different elements. Although the wet leaching process has a high metal recovery rate, it is difficult to remove impurities and separate due to the complex composition of the leaching solution, resulting in low purity of the product. In addition, the equipment is susceptible to corrosion during the process. The physical method of recovering molybdenum from waste catalysts usually involves placing molybdenum-containing materials into a high-temperature reactor and introducing an oxidizing gas to obtain molybdenum trioxide, which is recovered using the easy sublimation characteristics of molybdenum trioxide to obtain high-purity molybdenum trioxide.
[0003] The invention patent with publication number CN114606385A discloses a method for selectively leaching molybdenum and vanadium from molybdenum-vanadium waste catalysts. The molybdenum-vanadium waste catalysts are subjected to two-stage roasting treatment to obtain a roasting material; the roasting material and the combined leaching solution are mixed and then subjected to hydrothermal treatment, and then subjected to solid-liquid separation treatment to obtain a vanadium-containing molybdenum leaching solution. This method can significantly improve the leaching effect of vanadium and achieve the coordinated leaching of molybdenum and vanadium, but the two-stage roasting treatment will cause partial sublimation of molybdenum trioxide due to excessive local temperature during the roasting process, resulting in a decrease in the molybdenum recovery rate, and the two-stage roasting process will produce huge energy consumption and harmful gases, which is not conducive to energy saving and environmental protection.
[0004] The invention patent with publication number CN113774220A discloses a method for recovering molybdenum / bismuth and vanadium from waste catalysts. The method adds alkali to the waste catalyst for oxidation roasting and water leaching to separate bismuth from molybdenum and vanadium in the waste catalyst; vanadium is separated from molybdenum by precipitation of ammonium chloride; the crude ammonium molybdate solution is subjected to acid precipitation, ammonia leaching, ion exchange, purification, and vacuum crystallization to obtain ammonium heptamolybdate; and ammonium metavanadate product is obtained by ion exchange, ammonia desorption, and recrystallization. The metal recovery rate of this method is high, but the entire process is complicated, involving a wide variety of chemical reagents, and the process cost is relatively high, which is not suitable for industrial production.
[0005] The invention patent with publication number CN101724758A discloses a method for recovering molybdenum from molybdenum-containing waste catalysts. The method comprises mixing the waste catalyst with an alkaline substance and roasting it, then leaching and filtering the roasted product with a mixed acid solution containing sulfuric acid, nitric acid and citric acid, and adding ammonia water to the filtrate for precipitation to obtain an ammonium molybdate product. The method is simple to operate and has high product purity, but the metal recovery rate is low.
[0006] In summary, the existing methods for recovering molybdenum and vanadium from spent catalysts still have defects, mainly manifested in low metal recovery rate, poor environmental friendliness, complex process, high cost and other problems. Therefore, it is of great significance to develop an efficient, simple, environmentally friendly and economical method for recovering molybdenum and vanadium from metal ash of spent catalysts in slurry bed residual oil hydrogenation. Summary of the invention
[0007] In view of the problems of low metal recovery rate, poor environmental friendliness, complex process and high cost in the above-mentioned method for recovering molybdenum and vanadium from waste catalysts, the purpose of the present invention is to provide a method for recovering molybdenum and vanadium from metal ash residue of hydrogenation waste catalysts, which uses slurry bed residual oil hydrogenation waste catalyst as raw material, and after high-temperature treatment under the conditions of water vapor and oxygen, the hydrocarbon substances in the waste catalyst are converted into usable gas resources; the waste catalyst after the removal of hydrocarbon substances is roasted and decarbonized under aerobic conditions, and then an alkali solution is used to obtain an leaching solution containing molybdenum and vanadium components, and the leaching solution is subjected to a series of operations such as crystallization and separation to obtain ammonium metavanadate and molybdic acid. The method has a simple process flow, high metal recovery rate, green environmental protection, economy, and is easy to realize industrial-scale production.
[0008] The purpose of the present invention is achieved through the following technical solutions: The present invention provides a method for recovering molybdenum and vanadium from metal ash residue of hydrogenation waste catalyst, comprising the following steps: Step 1: calcining the waste catalyst of slurry bed residual oil hydrogenation, while introducing water vapor and oxygen; after the calcination is completed, roasting is carried out under aerobic conditions to obtain metal ash; Step 2: Mix the metal ash, alkaline substance and water, heat and extract, and filter to obtain filtrate A; Step 3: Mix filtrate A and ammonium chloride, adjust the pH to 1.5-5.0 with an acidic substance, and obtain filtrate B after filtering; Step 4: Cool the filtrate B and let it stand, and obtain solid ammonium metavanadate and filtrate C after filtration; and obtain solid molybdic acid by post-treatment of filtrate C.
[0009] The waste catalyst obtained in the slurry bed residual oil hydrogenation process mainly contains vanadium and molybdenum metals, followed by metal impurities such as nickel, aluminum, silicon, iron, sodium, calcium, and hydrocarbon substances such as petroleum hydrocarbons. Through calcination under water vapor and oxygen atmosphere, oxygen is used to change the metal elements in the waste catalyst from a reduced state to an oxidized state, and water vapor is used to react with polycyclic aromatic hydrocarbons in petroleum hydrocarbons to generate hydrogen, so as to realize the secondary utilization of polycyclic petroleum hydrocarbons attached to the surface of the waste catalyst, and it is beneficial to reduce the influence of hydrocarbon impurities on the metal oxidation effect while improving the reaction efficiency. However, if air contact calcination is directly adopted, due to too many components in the air, the oxygen and water vapor content is less, if you want to achieve the same effect, you need to introduce a large amount of air, react for a long time, cause waste, and affect the recovery and extraction effect, and it is also easy to burn nickel oxides and molybdenum oxides into nickel molybdate, and nickel molybdate is difficult to separate molybdenum and nickel in the subsequent hydrometallurgical process. Therefore, the use of water vapor and oxygen atmosphere for calcination in the present invention is more conducive to the separation of vanadium and molybdenum metals, and obtains a higher recovery rate and purity.
[0010] The oxygen roasting process after calcination can better remove carbon, which is also conducive to improving the recovery rate and purity of vanadium and molybdenum metals in the subsequent hydrometallurgical process. The purpose of mixing metal ash and alkaline substances for heating and leaching is to reduce the influence of other metal impurities in the metal ash. If acidic substances are used, metal impurities such as aluminum, silicon, iron, sodium, and calcium in the metal ash will dissolve in the filtrate, increasing the difficulty of subsequent impurity removal and purification of the target product.
[0011] When alkaline substances are added, the metal oxides in the waste catalyst react with the alkali to generate metal ions present in the filtrate I. When acidic substances are added to the filtrate A, the metal ion environment in the calcined material changes, and the acidic substances can be used to better adjust the pH of the filtrate. In solutions with different pH values and temperatures, the solubility of metavanadate and molybdate is different, and the solubility difference is used to separate molybdenum and vanadium.
[0012] Preferably, in step 1, the flow rate ratio of water vapor to oxygen is 1 to 6:1; more preferably, the flow rate ratio of water vapor to oxygen is 2 to 4:1.
[0013] If the ratio of water vapor to oxygen flow is too large, the water content is high and the oxygen is low, the metal oxidation reaction is not complete, and it is difficult to extract the metal by hydrometallurgical methods. If the ratio of water vapor to oxygen flow is too small, the water content is low and the oxygen is high, it is easy to calcine to generate nickel molybdate, which will also increase the difficulty of subsequent extraction and reduce the recovery rate.
[0014] Preferably, in step 1, the calcination temperature is 1100-1300° C., and the holding time is 1-60 min; more preferably, the holding time is 2-30 min.
[0015] If the calcination time is too long, it will also easily calcine to produce nickel molybdate, which will increase the difficulty of subsequent extraction and reduce the recovery rate.
[0016] Preferably, in step 1, the calcination temperature is 500-700° C., and the holding time is 2-10 h; more preferably, the holding time is 3-5 h.
[0017] The roasting process after calcination is conducive to removing the residual carbon and water in the calcination process, greatly reducing the material volume of the subsequent hydrometallurgical process, facilitating operation and improving efficiency. In addition, the roasting process uses a temperature far lower than that of calcination, which is not easy to generate nickel molybdate and will not have a significant impact on the recovery rate of subsequent hydrometallurgy.
[0018] Preferably, in step 2, the molar amount of the vanadium component in the metal ash is V 2 O 5 The molar amount of the molybdenum component is MoO 3 The molar ratio of metal ash to alkaline substances is V 2 O 5 +MoO 3 The molar ratio of the alkaline substance is 1:1 to 3.5, and more preferably, the molar ratio is 1:2 to 2.5.
[0019] Preferably, in step 2, the molar ratio of the alkaline substance to water is 1:50-100; more preferably, the molar ratio of the alkaline substance to water is 1:40-80.
[0020] Preferably, in step 2, the alkaline substance comprises a combination of one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonium carbonate and ammonium bicarbonate; more preferably, the alkaline substance comprises a combination of one or more of ammonia water, sodium carbonate and ammonium bicarbonate.
[0021] Preferably, in step 2, the temperature of the heating leaching is 40-130° C., and the time is 1-10 h; more preferably, the temperature of the heating leaching is 80-95° C., and the time is 2-5 h.
[0022] Preferably, in step 3, the molar amount of the vanadium component in the metal ash is V 2 O 5 The molar amount of the molybdenum component is MoO 3 The molar ratio of metal ash to ammonium chloride is V 2 O 5 +MoO 3 The molar ratio of the sodium hydroxide to ammonium chloride is 1:1 to 3, and more preferably, the molar ratio is 1:1.5:2.
[0023] Preferably, in step three, the pH is adjusted to 2-4 with an acidic substance, and filtrate B is obtained after filtration.
[0024] Preferably, in step three, the acidic substance comprises a combination of one or more of hydrochloric acid, sulfuric acid, nitric acid, perchloric acid, chloric acid, hydroiodic acid and hydrobromic acid; more preferably, the acidic substance comprises a combination of one or more of hydrochloric acid, sulfuric acid, nitric acid, perchloric acid and chloric acid; further preferably, the acidic substance comprises a combination of one or more of hydrochloric acid, sulfuric acid and nitric acid.
[0025] Preferably, in step three, the cooling and standing temperature is 20-85°C, and the standing time is 3-24 hours; more preferably, the cooling and standing temperature is 25-40°C, and the standing time is 5-10 hours.
[0026] Preferably, in step 4, the post-treatment of the filtrate C comprises: adding anion exchange resin to the filtrate C for removal, filtering to obtain a molybdenum-rich filtrate, adjusting the pH to 0.4-3.5, and then obtaining molybdic acid solid by evaporation and crystallization.
[0027] Preferably, the mass ratio of the anion exchange resin to the filtrate C is 0.05-0.3:1, more preferably, the mass ratio of the anion exchange resin to the filtrate C is 0.05-0.15:1; the removal time of the anion exchange resin is 0.5-8h, more preferably, the removal time is 1-5h.
[0028] Preferably, the pH of the molybdenum-rich filtrate is adjusted to 1.5-2.5.
[0029] Preferably, the evaporation crystallization temperature is 40-95°C, more preferably, the evaporation crystallization temperature is 45-65°C.
[0030] Compared with the prior art, the present invention has the following beneficial effects: (1) The metal recovery method provided by the present invention can improve the recovery rate of molybdenum and vanadium components, simplify the recovery process, reduce environmental pollution, and reduce the cost of the recovery process.
[0031] (2) The ammonium metavanadate solid and molybdic acid solid provided by the present invention have high purity, both above 96%. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is described below with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0033] Example 1 This embodiment provides a method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst, the method comprising: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1100°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 3:1), and heat for 5 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; calcine the waste catalyst at 600°C for 3 hours under aerobic conditions (air is sufficient) to obtain metal ash.
[0034] Step 2: Take 300 g of metal ash, 400 g of sodium carbonate (AR, 99%) and 3500 g of deionized water, mix them evenly, heat and soak them in a water bath at 85° C. for 4 hours, and then filter them to obtain filtrate A.
[0035] Step 3: Add 330 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of nitric acid (AR, 96%), adjust the pH of the filtrate to 4.0, and obtain filtrate B.
[0036] Step 4: Lower the temperature of filtrate B to 35° C. and let stand for 6 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0037] Step 5: Add 250g of anion exchange resin to the filtrate C, perform ion exchange for 4h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add nitric acid (mass fraction 68%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 65°C.
[0038] Example 2 This embodiment provides a method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst, the method comprising: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1200°C, and simultaneously introduce a mixture of water vapor and oxygen (the flow ratio of water vapor to oxygen is 2:1), and heat for 3 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; the waste catalyst is calcined at 650°C under aerobic conditions for 4 hours to obtain metal ash.
[0039] Step 2: Take 300 g of metal ash, 420 g of sodium bicarbonate (AR, 99%) and 4000 g of deionized water, mix them evenly, heat and soak them in a water bath at 80° C. for 4 hours, and then filter them to obtain filtrate A.
[0040] Step 3: Add 350 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of hydrochloric acid (AR, 95%), adjust the pH of the filtrate to 2.5, and obtain filtrate B.
[0041] Step 4: Lower the temperature of filtrate B to 25°C and let stand for 7 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0042] Step 5: Add 380g of anion exchange resin to the filtrate C, perform ion exchange for 5h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add nitric acid (mass fraction 68%) to the molybdenum-rich filtrate, adjust the pH value to 2.0, and then obtain molybdic acid solid by evaporation and crystallization at 60°C.
[0043] Example 3 This embodiment provides a method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst, the method comprising: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1300°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 4:1), and heat for 2 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; the waste catalyst is calcined at 600°C for 5 hours under aerobic conditions to obtain metal ash.
[0044] Step 2: Take 300 g of metal ash, mix it evenly with 450 g of sodium bicarbonate (AR, 99%) and 4500 g of deionized water, heat it in a water bath at 80° C. for 4 hours, and then filter it to obtain filtrate A.
[0045] Step 3: Add 310 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of sulfuric acid (AR, 25-28%), adjust the pH of the filtrate to 3.5, and obtain filtrate B.
[0046] Step 4: Lower the temperature of filtrate B to 40° C. and let stand for 8 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0047] Step 5: Add 340g of anion exchange resin to the filtrate C, perform ion exchange for 4h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add sulfuric acid (5mol / L) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 55°C.
[0048] Example 4 This embodiment provides a method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst, the method comprising: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1200°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 4:1), and heat for 3 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; the waste catalyst is calcined at 650°C for 4 hours under aerobic conditions to obtain metal ash.
[0049] Step 2: Take 300 g of metal ash, 420 g of sodium hydroxide (AR, 96%) and 5000 g of deionized water, mix them evenly, heat and soak them in a water bath at 85° C. for 4 hours, and then filter them to obtain filtrate A.
[0050] Step 3: Add 350 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of nitric acid (AR, 99%), adjust the pH of the filtrate to 2.5, and obtain filtrate B.
[0051] Step 4: Lower the temperature of filtrate B to 25° C. and let stand for 8 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0052] Step 5: Add 350g of anion exchange resin to the filtrate C, perform ion exchange for 4h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add nitric acid (mass fraction 68%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 65°C.
[0053] Example 5 This embodiment provides a method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst, the method comprising: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1100°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 3:1), and heat for 3 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; the waste catalyst is calcined at 650°C for 3 hours under aerobic conditions to obtain metal ash.
[0054] Step 2: Take 300 g of metal ash, 440 g of sodium carbonate (AR, 99%) and 5200 g of deionized water, mix them evenly, heat and soak them in a water bath at 80° C. for 4 hours, and then filter them to obtain filtrate A.
[0055] Step 3: Add 360 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of hydrochloric acid (AR, 96%), adjust the pH of the filtrate to 3.5, and obtain filtrate B.
[0056] Step 4: Lower the temperature of filtrate B to 45° C. and let stand for 8 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0057] Step 5: Add 420 g of anion exchange resin to the filtrate C, perform ion exchange for 4 hours, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add hydrochloric acid (volume fraction 36%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 60°C.
[0058] Example 6 This embodiment provides a method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst, the method comprising: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1100°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 5:1), and heat it for 20 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; the waste catalyst is calcined at 650°C for 3 hours under aerobic conditions to obtain metal ash.
[0059] Step 2: Take 300 g of metal ash, 440 g of sodium carbonate (AR, 99%) and 5200 g of deionized water, mix them evenly, heat and soak them in a water bath at 70° C. for 4 hours, and then filter them to obtain filtrate A.
[0060] Step 3: Add 360 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of hydrochloric acid (AR, 96%), adjust the pH of the filtrate to 2.5, and obtain filtrate B.
[0061] Step 4: Lower the temperature of filtrate B to 45° C. and let stand for 8 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0062] Step 5: Add 420 g of anion exchange resin to the filtrate C, perform ion exchange for 4 hours, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add hydrochloric acid (volume fraction 36%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 60°C.
[0063] Comparative Example 1 The difference from Example 1 is that in step 1, the flow ratio of water vapor to oxygen is too large.
[0064] The method includes: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1100°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 10:1), and heat for 5 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; the waste catalyst is calcined at 600°C for 3 hours under aerobic conditions to obtain metal ash.
[0065] Step 2: Take 300 g of metal ash, 400 g of sodium carbonate (AR, 99%) and 3500 g of deionized water, mix them evenly, heat and soak them in a water bath at 85° C. for 4 hours, and then filter them to obtain filtrate A.
[0066] Step 3: Add 330 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of nitric acid (AR, 96%), adjust the pH of the filtrate to 4.0, and obtain filtrate B.
[0067] Step 4: Lower the temperature of filtrate B to 35° C. and let stand for 6 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0068] Step 5: Add 250g of anion exchange resin to the filtrate C, perform ion exchange for 4h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add nitric acid (mass fraction 68%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 65°C.
[0069] Comparative Example 2 The difference from Example 1 is that in step 1, the flow ratio of water vapor to oxygen is too small.
[0070] The method includes: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1100°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 0.4:1), heat it for 5 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; calcine the waste catalyst at 600°C under aerobic conditions for 3 hours to obtain metal ash.
[0071] Step 2: Take 300 g of metal ash, 400 g of sodium carbonate (AR, 99%) and 3500 g of deionized water, mix them evenly, heat and soak them in a water bath at 85° C. for 4 hours, and then filter them to obtain filtrate A.
[0072] Step 3: Add 330 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of nitric acid (AR, 96%), adjust the pH of the filtrate to 4.0, and obtain filtrate B.
[0073] Step 4: Lower the temperature of filtrate B to 35° C. and let stand for 6 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0074] Step 5: Add 250g of anion exchange resin to the filtrate C, perform ion exchange for 4h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add nitric acid (mass fraction 68%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 65°C.
[0075] Comparative Example 3 The difference from Example 1 is that in step 1, the heating treatment time is too long.
[0076] The method includes: Step 1: put 5 kg of slurry bed residual oil hydrogenation waste catalyst into a heating furnace, raise the temperature of the heating furnace to 1100°C, and simultaneously introduce a mixed gas of water vapor and oxygen (the flow ratio of water vapor to oxygen is 3:1), and heat for 120 minutes to remove hydrocarbon substances in the slurry bed residual oil hydrogenation waste catalyst to obtain the waste catalyst; calcine the waste catalyst at 600°C under aerobic conditions for 3 hours to obtain metal ash.
[0077] Step 2: Take 300 g of metal ash, 400 g of sodium carbonate (AR, 99%) and 3500 g of deionized water, mix them evenly, heat and soak them in a water bath at 85° C. for 4 hours, and then filter them to obtain filtrate A.
[0078] Step 3: Add 330 g of ammonium chloride (AR, 99.5%) to filtrate A, stir evenly, then add an appropriate amount of nitric acid (AR, 96%), adjust the pH of the filtrate to 4.0, and obtain filtrate B.
[0079] Step 4: Lower the temperature of filtrate B to 35° C. and let stand for 6 hours to allow ammonium metavanadate to precipitate in solid form. Filter to obtain ammonium metavanadate solid and filtrate C.
[0080] Step 5: Add 250g of anion exchange resin to the filtrate C, perform ion exchange for 4h, remove the remaining metavanadate ions in the filtrate C, and obtain a molybdenum-rich filtrate; add nitric acid (mass fraction 68%) to the molybdenum-rich filtrate, adjust the pH value to 1.5, and then obtain molybdic acid solid by evaporation and crystallization at 65°C.
[0081] Table 1 Composition of slurry bed residue oil hydrogenation spent catalyst (raw material) project unit Numeric Dynamic viscosity (150℃) cp 198 Carbon residue (including petroleum hydrocarbons) wt% 45.60 iron mg / kg 108.4 nickel mg / kg 619.3 Sulfur content wt% 2.54 vanadium mg / kg 2022.4 Tetrahydrofuran insoluble matter % 5.61 molybdenum mg / kg 2022.4 Initial distillation point ℃ 377 Iron + Nickel + Vanadium + Molybdenum mg / kg 5485.2 10% recovery temperature ℃ 453 Density(20℃) <![CDATA[Kg / m 3 ]]> 1149.8 Table 2 ICP analysis of metal ash composition (metal elements) Table 3 Metal recycling data Vanadium component recovery rate (%) Molybdenum component recovery rate (%) Purity of ammonium metavanadate (%) Molybdic acid purity (%) Example 1 95.5 95.7 96.4 96.4 Example 2 95.2 96.1 96.6 96.2 Example 3 96.2 95.8 96.2 96.6 Example 4 96.3 96.6 96.8 96.3 Example 5 95.9 96.3 96.6 96.7 Example 6 97.4 96.7 96.5 96.5 Comparative Example 1 75.7 70.5 96.7 95.4 Comparative Example 2 85.2 72.4 97.6 95.2 Comparative Example 3 88.6 71.7 98.3 95.8 *Calculation method: vanadium component recovery rate (%) = (mass of vanadium in product / mass of vanadium in raw material) * 100; Molybdenum component recovery rate (%) = (mass of molybdenum in product / mass of molybdenum in raw material) * 100; The purity test method of ammonium metavanadate shall be in accordance with HG / T 3445-2003; Molybdic acid purity (%) (mass fraction of molybdenum obtained by ICP method) / (mass fraction of molybdenum in theoretical molybdic acid)*100.
[0082] As shown in Table 1, the composition of the slurry bed residual oil hydrogenation waste catalyst used in Examples 1-6 and Comparative Examples 1-3 is shown in Table 2, the metal element composition of the metal ash after calcination and aerobic roasting of the slurry bed residual oil hydrogenation waste catalyst in Example 1 is shown in Table 3, and the recovery rate and purity data of the products obtained after the treatment steps in Examples 1-6 and Comparative Examples 1-3 are shown.
[0083] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst, characterized in that: The steps include: Step 1: calcining the waste catalyst of slurry bed residual oil hydrogenation, while introducing water vapor and oxygen; after the calcination is completed, roasting is carried out under aerobic conditions to obtain metal ash; Step 2: Mix the metal ash, alkaline substance and water, heat and extract, and filter to obtain filtrate A; Step 3: Mix filtrate A and ammonium chloride, adjust the pH to 1.5-5.0 with an acidic substance, and obtain filtrate B after filtering; Step 4: Cool the filtrate B and let it stand, and obtain solid ammonium metavanadate and filtrate C after filtration; and obtain solid molybdic acid by post-treatment of filtrate C.
2. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 1, characterized in that: In step 1, the flow ratio of water vapor to oxygen is 1-6:1; the calcination temperature is 1100-1300°C, and the insulation time is 1-60 min; the roasting temperature is 500-700°C, and the insulation time is 2-10 h.
3. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 1, characterized in that: In step 2, the molar amount of the vanadium component in the metal ash is calculated as V2O5, and the molar amount of the molybdenum component is calculated as MoO3. The molar ratio of the metal ash to the alkaline substance is calculated as the molar ratio of V2O5+MoO3 to the alkaline substance, and the molar ratio is 1:1~3.
5.
4. The method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst according to any one of claims 1 to 3, characterized in that: In step 2, the molar ratio of the alkaline substance to water is 1:50-100; the alkaline substance includes a combination of one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, ammonium carbonate and ammonium bicarbonate.
5. The method for recovering molybdenum and vanadium from metal ash of spent hydrogenation catalyst according to any one of claims 1 to 3, characterized in that: In step 2, the heating leaching temperature is 40-130° C. and the time is 1-10 hours.
6. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 1, characterized in that: In step 3, the molar amount of the vanadium component in the metal ash is calculated as V2O5, and the molar amount of the molybdenum component is calculated as MoO3. The molar ratio of the metal ash to ammonium chloride is calculated as the molar ratio of V2O5+MoO3 to ammonium chloride, and the molar ratio is 1:1~3.
7. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 1 or 6, characterized in that: In step three, the acidic substance includes one or more combinations of hydrochloric acid, sulfuric acid, nitric acid, perchloric acid, chloric acid, hydroiodic acid and hydrobromic acid.
8. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 1 or 6, characterized in that: In step 3, the temperature of the cooling and standing is 20-85° C., and the standing time is 3-24 hours.
9. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 1, characterized in that: In step 4, the post-treatment of the filtrate C includes: adding anion exchange resin to the filtrate C for removal, filtering to obtain a molybdenum-rich filtrate, adjusting the pH to 0.4-3.5, and then evaporating and crystallizing to obtain molybdic acid solid.
10. The method for recovering molybdenum and vanadium from metal ash of hydrogenation waste catalyst according to claim 9, characterized in that: The mass ratio of the anion exchange resin to the filtrate C is 0.05-0.3:1; the removal time of the anion exchange resin is 0.5-8 hours; and the temperature of the evaporation crystallization is 40-95°C.