Preparation method of vanadium-aluminum alloy for aerospace titanium alloy
By adopting vacuum magnetic levitation smelting and sandblasting processes in the production of vanadium aluminum alloys for aerospace titanium alloys, the problems of long production cycle, high cost and unstable product quality are solved, and efficient and stable vanadium aluminum alloy preparation is achieved, which is significantly Improved production capacity and yield rate.
Patent Information
- Application Number
- CN202411235128.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
The existing vanadium aluminum alloy production methods for aerospace titanium alloys have problems such as long production cycle, small production capacity, high cost and unstable product quality, especially long-term and shrinkage defects caused by vacuum induction smelting, as well as electric aluminum thermal method. The problem of incomplete separation of oxide film and residue liquid.
Vanadium pentoxide and slag-making agent are dried and mixed with air atomized aluminum powder to perform self-propagation reaction to obtain vanadium aluminum alloy ingots, and refine them in a vacuum magnetic levitation smelting furnace, combining sandblasting, grinding and magnetic levitation smelting processes. Control process parameters to reduce impurity content and the occurrence of shrinkage areas.
It significantly shortens the production cycle, improves production capacity and product quality, reduces costs, minimizes impurity content, and improves yield and economic benefits.
Smart Images

Figure CN119082520A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of vanadium-aluminum alloy preparation, and in particular relates to a method for preparing vanadium-aluminum alloy for aerospace titanium alloy. Background Art
[0002] Vanadium aluminum alloy is an element additive for the production of titanium alloys, high-temperature alloys and certain special alloys. It is most widely used in the titanium alloy field. Vanadium aluminum alloy used in aerospace titanium alloys has extremely high requirements on the uniformity of the alloy's chemical composition and the level of impurities.
[0003] At present, the production methods of vanadium aluminum alloy for aerospace titanium alloy at home and abroad mainly include two-step method and electric aluminothermic method. The two-step method refers to the vanadium aluminum alloy ingot produced by the one-step method (aluminothermic reduction method) is processed by sandblasting, grinding and other methods, and broken into suitable sizes and aluminum beans for refining in medium and high frequency vacuum induction melting furnaces. Through vacuum melting, the chemical composition of the main elements of the vanadium aluminum alloy is further uniform (the extreme difference of Al and V elements is less than 2%), and the content of impurity elements such as O and N in the ingot is reduced (O: not more than 0.18%, N: not more than 0.04%). The obtained ingot is crushed, magnetically separated, and sorted. The vanadium-aluminum alloy for aerospace titanium alloy can be obtained by the two-step method; however, in actual production, the two-step method has two significant disadvantages. First, the method has a long production cycle and a small production capacity, which is mainly caused by the process characteristics of vacuum induction melting. Taking a 200kg feed amount as an example, it takes at least 3.5 hours from feeding to cooling of the ingot to take out of the furnace for the secondary melting of a furnace of vanadium-aluminum alloy in a medium-frequency induction furnace, which is time-consuming and inefficient. Second, affected by the cooling rate, the ingot produced by this method has a deeper shrinkage cavity in the upper area, and the chemical composition deviation near the shrinkage cavity area is large. Removing the shrinkage cavity area will cause a certain loss, resulting in a reduction in the yield.
[0004] The electric aluminothermic method refers to the use of electrodes to ignite the raw materials (vanadium pentoxide, aluminum powder, calcium fluoride) in an electric arc furnace to carry out aluminothermic reduction reaction, and then conduct electric heating after the reaction is completed. The purpose of electric heating is to increase the temperature of the molten pool system, make the alloy liquid phase fully homogenized, and obtain a vanadium aluminum alloy with high uniformity of the main element chemical composition (the extreme difference of Al and V elements is less than 2.0%). There are also some obvious defects in the production of vanadium aluminum alloy by the electric aluminothermic method. On the one hand, there is a large amount of oxide film inside the vanadium aluminum alloy produced by the electric aluminothermic method, and the subsequent processing procedures are cumbersome, resulting in high economic costs and difficulty in industrial production; on the other hand, there is an incomplete separation of slag and liquid, which poses a serious product quality risk.
[0005] In view of this, it is necessary to provide a new production process to solve the problems of unstable quality, high production cost, long cycle and low production capacity of vanadium-aluminum alloys used in aerospace titanium alloys. Summary of the invention
[0006] In order to solve the above problems existing in the prior art, the present invention provides a method for preparing vanadium aluminum alloy for aerospace titanium alloy. The technical problem to be solved by the present invention is achieved by the following technical solutions:
[0007] A method for preparing a vanadium aluminum alloy for aerospace titanium alloy, comprising:
[0008] Step 1: Drying vanadium pentoxide and slag-forming agent at a drying temperature of 85 to 115° C. for a drying time of 10 to 20 hours;
[0009] Step 2: Mix the dried vanadium pentoxide, slag-forming agent and air atomized aluminum powder according to the following weight percentages: air atomized aluminum powder: 45.88-46.45%, vanadium pentoxide: 50.75-51.07%, slag-forming agent: 2.80-3.06%;
[0010] Step 3: putting the uniformly mixed powder into a reaction container and pressing it, then igniting the powder to make it undergo a self-propagating reaction to obtain a vanadium-aluminum alloy ingot;
[0011] Step 4: performing surface treatment on the vanadium-aluminum alloy ingot and then crushing it into vanadium-aluminum alloy blocks;
[0012] Step 5: Load the vanadium-aluminum alloy block into a vacuum magnetic suspension melting furnace, evacuate the furnace until the pressure inside the furnace is less than 1.0 Pa, and then fill the furnace with argon gas until the vacuum degree is -300 to -600 Pa;
[0013] Step 6: increasing the power of the vacuum magnetic levitation melting furnace at a rate of 50-100 kW / min, so that the vanadium-aluminum alloy block begins to melt, and after the vanadium-aluminum alloy block is completely melted, continuing to refine for 5-10 minutes while stirring to obtain vanadium-aluminum alloy liquid, wherein the refining power is 300-400 kW;
[0014] Step 7: After the refining is completed, the power of the vacuum magnetic levitation melting furnace is reduced to 0 kW at a rate of 100 to 150 kW / min, and the vanadium-aluminum alloy liquid is cooled for 30 to 60 minutes, and the vanadium-aluminum alloy is obtained after treatment, wherein the vanadium-aluminum alloy comprises the following components in weight percentage: vanadium: 57.5% to 58.5%, the remainder being aluminum and unavoidable impurities, wherein iron: ≤0.10%, silicon: ≤0.10%, carbon: ≤0.02%, oxygen: ≤0.08%, and nitrogen: ≤0.02%.
[0015] Furthermore, the slag-forming agent is fluorite powder, wherein the content of silicon dioxide in the fluorite powder is ≤1.0%.
[0016] Furthermore, in step 4, surface treatment of the vanadium-aluminum alloy ingot includes: sandblasting and grinding the vanadium-aluminum alloy ingot to remove sticky slag and sticky carbon.
[0017] Furthermore, in step 4, the maximum size of the crushed vanadium-aluminum alloy block is 50 to 70 mm.
[0018] Beneficial effects of the present invention:
[0019] 1. The present invention adopts the aluminothermic method and magnetic suspension smelting method to produce high-quality vanadium-aluminum alloy ingots, which greatly shortens the product production cycle, thereby increasing production capacity and reducing production costs;
[0020] 2. The magnetic suspension smelting process is used in combination with the parameters provided by the present invention to minimize the entry of carbon, oxygen, nitrogen and other elements in the air into the vanadium aluminum alloy, thereby reducing the impurity content in the alloy, eliminating segregation and chemical ingot defects, and achieving better and more stable product quality;
[0021] 3. The shrinkage area of the vanadium-aluminum alloy ingot prepared by the two-step method is about one-third of that of the two-step method, with small processing loss and high yield, which effectively reduces the production cost and has good economic benefits.
[0022] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The test report at the sampling point 1 in the upper layer in Example 1;
[0024] Figure 2 This is the test report at the sampling point 2 in the lower layer in Example 2. DETAILED DESCRIPTION
[0025] Combine the following Figure 1-2 The present invention is further described in detail with reference to the specific embodiments, but the embodiments of the present invention are not limited thereto.
[0026] Example 1
[0027] The embodiment of the present invention provides a method for preparing a vanadium aluminum alloy for aerospace titanium alloy, which specifically comprises the following steps:
[0028] Step 1: Dry the vanadium pentoxide and slag-forming agent at a drying temperature of 85 to 115° C. for 18 hours.
[0029] Step 2: Weigh the dried vanadium pentoxide, slag-forming agent and air-atomized aluminum powder according to the following weights: air-atomized aluminum powder: 185.80 kg, vanadium pentoxide: 203.00 kg, slag-forming agent: 11.20 kg, and mix them thoroughly. The slag-forming agent is fluorite fine powder, and the silicon dioxide content in the fluorite fine powder is ≤1.0%.
[0030] Step 3: Load the evenly mixed powder into a graphite crucible and press it tightly. Then ignite the magnesium chips and put them into the crucible to ignite the powder for a self-propagating reaction. After the reaction is completed, transport the crucible to a cooling area and cool it for 48 hours to fully separate the slag and the molten metal to obtain a vanadium-aluminum alloy ingot.
[0031] Step 4: sandblasting and grinding the vanadium-aluminum alloy ingot to remove sticky slag and sticky carbon, and breaking it into vanadium-aluminum alloy blocks with a maximum size of 50 to 70 mm.
[0032] Step 5: Load the vanadium-aluminum alloy block into a vacuum magnetic levitation melting furnace, evacuate the furnace to a pressure of 0.7Pa, reduce the air content in the furnace, and prevent the oxygen and nitrogen in the air from reacting with the metal to form oxides and nitrides during the smelting process. Then, fill the furnace with argon to a vacuum degree of -300Pa to increase the pressure in the furnace to ensure that the ingot can be quickly exhausted during subsequent smelting and cooling, thereby controlling the looseness ratio of the ingot.
[0033] Step 6: Increase the power of the vacuum magnetic levitation melting furnace at a rate of 60kw / min. Under continuous electromagnetic induction heating, the vanadium-aluminum alloy block begins to melt and is in a completely suspended state as a melt. After the vanadium-aluminum alloy block is completely melted, continue to refine at a power of 300kw for 6 minutes while performing electromagnetic stirring to improve the uniformity of the chemical composition of the main elements of the alloy and to enrich the impurities in the ingot to the inner wall of the crucible for easy processing and removal, thereby finally obtaining a vanadium-aluminum alloy liquid.
[0034] Step 7: After the refining is completed, the power of the vacuum magnetic suspension melting furnace is reduced to 0 kW at a rate of 120 kW / min, and the vanadium aluminum alloy liquid is cooled in a water-cooled copper crucible for 40 minutes, and then the vanadium aluminum alloy is refined, crushed, magnetically separated, color-sorted, and manually selected to obtain a high-quality vanadium aluminum alloy for aerospace titanium alloy with uniform composition, low impurity content, no oxidation, and no nitridation defects. The vanadium aluminum alloy includes the following components by weight percentage: vanadium: 57.5% to 58.5%, the balance is aluminum and unavoidable impurities, wherein iron: ≤0.10%, silicon: ≤0.10%, carbon: ≤0.02%, oxygen: ≤0.08%, nitrogen: ≤0.02%.
[0035] The vanadium-aluminum alloy ingot after cooling in step 7 and before treatment was sampled and analyzed. The center of the bottom of the ingot was used as the base point and divided into three equal parts according to the thickness direction of the ingot. Three samples were uniformly taken from the center to the edge of three different thickness layers of the ingot, for a total of nine samples. The components of the nine samples were analyzed, and the analysis results are as follows:
[0036] Table 1 Chemical composition of the vanadium aluminum alloy prepared in Example 1
[0037]
[0038] In addition, the specific production data of Example 1 is shown in Table 2.
[0039] Table 2 Production data of vanadium aluminum alloy prepared in Example 1
[0040]
[0041] Control group 1
[0042] This control group 1 provides a conventional preparation method of vanadium aluminum alloy, which specifically includes the following steps:
[0043] Step 1: Dry the vanadium pentoxide and slag-forming agent at a drying temperature of 85 to 115° C. for 15 hours.
[0044] Step 2: Weigh the dried vanadium pentoxide, slag-forming agent and air-atomized aluminum powder according to the following weights: air-atomized aluminum powder: 185.80 kg, vanadium pentoxide: 203.00 kg, slag-forming agent: 11.20 kg, and mix them thoroughly. The slag-forming agent is fluorite fine powder.
[0045] Step 3: Load the evenly mixed powder into a graphite crucible and press it, ignite the powder to carry out a self-propagating reaction, and after the reaction is completed, naturally cool the alloy liquid in an atmospheric environment for 48 hours to obtain a vanadium-aluminum alloy ingot semi-finished product.
[0046] Step 4: The vanadium-aluminum alloy ingot semi-finished product is finely crushed, and a medium-frequency induction furnace is used for secondary smelting. The furnace is evacuated to a pressure of 2.0 Pa, and the refining time is 6 minutes. It is then poured into a mold, cooled in the furnace for 2.5 hours, and then removed from the furnace. The shrinkage holes and loose parts of the ingot are removed, and the vanadium-aluminum alloy is obtained after crushing.
[0047] The ingot after being taken out of the furnace and before being crushed in step 4 was sampled and analyzed. The center of the bottom of the ingot was taken as the base point, and the ingot was divided into three equal parts in the thickness direction. Three points of samples were uniformly taken from the center to the edge of the three different thickness layers of the ingot, for a total of nine samples. The components of the nine samples were analyzed, and the analysis results are as follows:
[0048] Table 3 Chemical composition of vanadium aluminum alloy prepared in control group 1
[0049]
[0050]
[0051] In addition, the specific production data of the control group 1 is shown in Table 4.
[0052] Table 4 Production data of vanadium aluminum alloy prepared in control group 1
[0053]
[0054] Example 2
[0055] The embodiment of the present invention provides a method for preparing a vanadium aluminum alloy for aerospace titanium alloy, which specifically comprises the following steps:
[0056] Step 1: Dry the vanadium pentoxide and slag-forming agent at a drying temperature of 85 to 115° C. for 18 hours.
[0057] Step 2: Weigh the dried vanadium pentoxide, slag-forming agent and air-atomized aluminum powder according to the following weights: air-atomized aluminum powder: 183.50 kg, vanadium pentoxide: 204.26 kg, slag-forming agent: 12.24 kg, and mix them thoroughly. The slag-forming agent is fluorite fine powder, and the content of silicon dioxide in the fluorite fine powder is ≤1.0%.
[0058] Step 3: Load the evenly mixed powder into a graphite crucible and press it tightly. Then ignite the magnesium chips and put them into the crucible to ignite the powder for a self-propagating reaction. After the reaction is completed, transport the crucible to a cooling area and cool it for 48 hours to fully separate the slag and the molten metal to obtain a vanadium-aluminum alloy ingot.
[0059] Step 4: sandblasting and grinding the vanadium-aluminum alloy ingot to remove sticky slag and sticky carbon, and breaking it into vanadium-aluminum alloy blocks with a maximum size of 50 to 70 mm.
[0060] Step 5: Load the vanadium-aluminum alloy block into a vacuum magnetic levitation melting furnace, evacuate the furnace to a pressure of 1.0Pa, reduce the air content in the furnace, and prevent the oxygen and nitrogen in the air from reacting with the metal to form oxides and nitrides during the smelting process. Then, fill the furnace with argon to a vacuum degree of -500Pa to increase the pressure in the furnace to ensure that the ingot can be quickly exhausted during the subsequent smelting and cooling process, thereby controlling the looseness ratio of the ingot.
[0061] Step 6: Increase the power of the vacuum magnetic levitation melting furnace at a rate of 80kw / min. Under continuous electromagnetic induction heating, the vanadium-aluminum alloy block begins to melt and is in a completely suspended state as a melt. After the vanadium-aluminum alloy block is completely melted, continue to refine at a power of 400kw for 8min while performing electromagnetic stirring to improve the uniformity of the chemical composition of the main elements of the alloy and to enrich the impurities in the ingot to the inner wall of the crucible for easy processing and removal, thereby finally obtaining a vanadium-aluminum alloy liquid.
[0062] Step 7: After the refining is completed, the power of the vacuum magnetic suspension melting furnace is reduced to 0 kW at a rate of 140 kW / min, and the vanadium aluminum alloy liquid is cooled in a water-cooled copper crucible for 60 minutes, and then the vanadium aluminum alloy is refined, crushed, magnetically separated, color-sorted, and manually selected to obtain a high-quality vanadium aluminum alloy for aerospace titanium alloy with uniform composition, low impurity content, no oxidation, and no nitridation defects. The vanadium aluminum alloy includes the following components by weight percentage: vanadium: 57.5% to 58.5%, the balance is aluminum and unavoidable impurities, wherein iron: ≤0.10%, silicon: ≤0.10%, carbon: ≤0.02%, oxygen: ≤0.08%, nitrogen: ≤0.02%.
[0063] The vanadium-aluminum alloy ingot after cooling in step 7 and before treatment was sampled and analyzed. The center of the bottom of the ingot was used as the base point and divided into three equal parts according to the thickness direction of the ingot. Three samples were uniformly taken from the center to the edge of three different thickness layers of the ingot, for a total of nine samples. The components of the nine samples were analyzed, and the analysis results are as follows:
[0064] Table 5 Chemical composition of the vanadium aluminum alloy prepared in Example 2
[0065]
[0066]
[0067] In addition, the specific production data of Example 2 is shown in Table 6.
[0068] Table 6 Production data of vanadium aluminum alloy prepared in Example 2
[0069]
[0070] Control group 2
[0071] This control group 2 provides a conventional preparation method of vanadium aluminum alloy, which specifically includes the following steps:
[0072] Step 1: Dry the vanadium pentoxide and slag-forming agent at a drying temperature of 85 to 115° C. for 18 hours.
[0073] Step 2: Weigh the dried vanadium pentoxide, slag-forming agent and air-atomized aluminum powder according to the following weights: air-atomized aluminum powder: 183.50 kg, vanadium pentoxide: 204.26 kg, slag-forming agent: 12.24 kg, and mix them thoroughly. The slag-forming agent is fluorite fine powder.
[0074] Step 3: Put the evenly mixed powder into a graphite crucible and press it, ignite the powder to carry out a self-propagating reaction, and after the reaction is completed, naturally cool the alloy liquid in an atmospheric environment for 48 hours to obtain a vanadium-aluminum alloy ingot.
[0075] Step 4: The vanadium-aluminum alloy ingot is finely crushed and subjected to secondary smelting in a medium frequency induction furnace. The furnace is evacuated to a pressure of 1.0 Pa for 10 minutes. The ingot is then poured into a mold and cooled for 3 hours before being taken out of the furnace. Shrinkage cavities and loose parts of the ingot are removed and crushed to obtain a vanadium-aluminum alloy.
[0076] The ingot after being taken out of the furnace and before being crushed in step 4 was sampled and analyzed. The center of the bottom of the ingot was taken as the base point, and the ingot was divided into three equal parts in the thickness direction of the ingot. Three points of samples were uniformly taken from the center to the edge of the three different thickness layers of the ingot, for a total of nine samples. The nine samples were analyzed for composition, and the analysis results are as follows: Table 7 Chemical composition of the vanadium aluminum alloy prepared in control group 2
[0077]
[0078] In addition, the specific production data of the control group 1 is shown in Table 8.
[0079] Table 8 Production data of vanadium aluminum alloy prepared in control group 2
[0080]
[0081] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing vanadium aluminum alloy for aerospace titanium alloy, characterized in that: include: Step 1: Drying vanadium pentoxide and slag-forming agent at a drying temperature of 85 to 115° C. for a drying time of 10 to 20 hours; Step 2: Mix the dried vanadium pentoxide, slag-forming agent and air atomized aluminum powder according to the following weight percentages: air atomized aluminum powder: 45.88-46.45%, vanadium pentoxide: 50.75-51.07%, slag-forming agent: 2.80-3.06%; Step 3: putting the uniformly mixed powder into a reaction container and pressing it, then igniting the powder to make it undergo a self-propagating reaction to obtain a vanadium-aluminum alloy ingot; Step 4: performing surface treatment on the vanadium-aluminum alloy ingot and then crushing it into vanadium-aluminum alloy blocks; Step 5: Load the vanadium-aluminum alloy block into a vacuum magnetic suspension melting furnace, evacuate the furnace until the pressure inside the furnace is less than 1.0 Pa, and then fill the furnace with argon gas until the vacuum degree is -300 to -600 Pa; Step 6: increasing the power of the vacuum magnetic levitation melting furnace at a rate of 50-100 kW / min, so that the vanadium-aluminum alloy block begins to melt, and after the vanadium-aluminum alloy block is completely melted, continuing to refine for 5-10 minutes while stirring to obtain vanadium-aluminum alloy liquid, wherein the refining power is 300-400 kW; Step 7: After the refining is completed, the power of the vacuum magnetic levitation melting furnace is reduced to 0 kW at a rate of 100 to 150 kW / min, and the vanadium-aluminum alloy liquid is cooled for 30 to 60 minutes, and the vanadium-aluminum alloy is obtained after treatment, wherein the vanadium-aluminum alloy comprises the following components in weight percentage: vanadium: 57.5% to 58.5%, the remainder being aluminum and unavoidable impurities, wherein iron: ≤0.10%, silicon: ≤0.10%, carbon: ≤0.02%, oxygen: ≤0.08%, and nitrogen: ≤0.02%.
2. The method for preparing vanadium aluminum alloy for aerospace titanium alloy according to claim 1, characterized in that: The slag-making agent is fluorite powder, wherein the content of silicon dioxide in the fluorite powder is ≤1.0%.
3. The method for preparing vanadium aluminum alloy for aerospace titanium alloy according to claim 1, characterized in that: In step 4, surface treatment of the vanadium-aluminum alloy ingot comprises: The vanadium-aluminum alloy ingot is sandblasted and polished to remove sticky slag and sticky carbon.
4. The method for preparing vanadium aluminum alloy for aerospace titanium alloy according to claim 1, characterized in that: In step 4, the maximum size of the crushed vanadium-aluminum alloy block is 50-70 mm.