Preparation method of Ag / Ti3SiC2 / rGO electric contact material
By wrapping rGO in Ag/Ti3SiC2 electrical contact material and adopting a three-stage vacuum sintering process, the problems of material conductivity and arc corrosion resistance are solved, and the preparation of electrical contact material with high density and excellent conductivity is achieved, satisfying the silver Actual production requirements for base electrical contact materials.
Patent Information
- Application Number
- CN202411152447.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-06
AI Technical Summary
During the preparation process, the Ag/Ti3SiC2 electrical contact material is difficult to uniformly distribute due to the layered structure of Ti3SiC2, and the conductivity is degraded. During sintering, Ag and Ti3SiC2 are prone to interfacial reaction, which damages the resistance to arc erosion. The existing alternative processes are complex and costly. , not environmentally friendly.
By preparing rGO-encapsulated Ti3SiC2 composite powder, rGO is uniformly dispersed and wrapped with Ti3SiC2 surface using ascorbic acid and hydroxypropyl methylcellulose, reducing the interface reaction between Ag and Ti3SiC2, and a three-stage vacuum sintering process is used to improve the density and conductivity of the material.
It realizes uniformly enhanced phase distribution of Ag/Ti3SiC2/rGO electrical contact materials, high density, excellent conductivity and good arc corrosion resistance, simple process, low cost, green and environmentally friendly, and is suitable for industrial production.
Smart Images

Figure CN119082528A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrical contact material, in particular to an Ag / Ti 3 SiC 2 Preparation method of / rGO electrical contact material. Background Art
[0002] Electrical contact materials are responsible for switching current in high and low voltage electrical appliances. They are the core components of motors and electrical products. Their performance directly affects the quality stability and service life of these products, and they are called the "heart" of electrical appliances. Entering the new century, with increasingly stringent global environmental protection policies, the European Union has issued a series of environmental directives prohibiting the use of toxic materials such as Cd in electronic and electrical products. Subsequently, developed countries such as the United States and Japan have also begun to restrict the use of Cd. Therefore, there is an urgent need to find new silver-based electrical contact materials that can replace Ag / CdO for the preparation of low-voltage electrical contacts, medium- and high-voltage contacts and other devices. Electrical contact materials are generally required to have good electrical and thermal conductivity, low and stable contact resistance, a certain strength and easy mechanical processing. In recent years, Ti 3 SiC 2 The unique crystal structure and excellent properties have attracted much attention. A large number of studies have shown that Ti 3 SiC 2 It is expected to replace CdO and be used in electrical contact materials.
[0003] Currently, Ag / Ti 3 SiC 2 The main problems in the preparation of electrical contact materials are: 1) Ti 3 SiC 2 The layered structure makes it difficult to distribute evenly, and the conductive properties of the material are significantly reduced; 2) During the sintering process, Ag and Ti 3 SiC 2 The interface reaction is easy to occur between them, which damages the material's arc erosion resistance. At the same time, the silver matrix grains are easy to grow during high-temperature sintering, which makes the material's mechanical properties and electrical conductivity relatively reduced, limiting the Ag / Ti 3 SiC 2 Application of electrical contact materials.
[0004] In order to solve the above problems and prepare electrical contact materials with excellent comprehensive performance, some researchers have conducted corresponding research. For example, Chinese patent CN111834136A published "A MAX@M composite electrical contact reinforcement phase material, composite electrical contact material and preparation method". This method uses HF acid to 3 SiC 2 Surface sensitization forms Ti 3 C 2 , then use PbCl2 The above product is activated, and then metal nanoparticles are coated on its surface by chemical plating to prepare a composite electrical contact reinforcement phase material coated with metal nanoparticles on the surface, which is then mixed with Ag and finally sintered to prepare a composite contact material. This method can improve the conductivity of the material to a certain extent, but when using this method to prepare electrical contact materials, Ti 3 SiC 2 The surface is sensitized to form Ti 3 C 2 , Ti 3 C 2 The presence of reduces the arc erosion resistance of the material, and this method has a complicated process, high technical cost, and multiple use of toxic and harmful reagents, making it difficult to mass produce. Patent CN109797307B published "Ag / C@Ti 3 AlC 2 The preparation method of contact material is firstly to form a contact material on Ti by chemical reaction. 3 AlC 2 A layer of phenolic resin organic matter is synthesized on the powder surface, and then the organic matter is decomposed into a carbon layer by high temperature calcination under argon gas, which is coated on the Ti 3 AlC 2 The particle surface is then coated with carbon. 3 AlC 2 The powder is mixed with Ag as an Ag-based reinforcement phase to make Ag / C@Ti 3 AlC 2 Electrical contact material, the method is through the Ti 3 AlC 2 The carbon layer formed on the surface inhibits the mutual diffusion of Al and Ag atoms during the sintering densification process to a certain extent. However, the carbon layer formed in this method greatly reduces the electrical conductivity of the material, and this method is not suitable for Ti 3 AlC 2 In the process of synthesizing a layer of phenolic resin on the surface of the powder, the raw materials used are resorcinol, formaldehyde and ammonia water, which are very harmful to the environment and human body and difficult to meet the requirements of industrial production. Patent CN118221104A discloses "a method for preparing an electric contact material and an electric contact". The method first mixes graphene oxide with nano copper oxide powder, nano lanthanum oxide powder and a surfactant, then reduces some oxygen-containing functional groups in the graphene oxide by hydrothermal reaction, then removes the active agent at 900-1000°C and nitrogen, then introduces hydrogen and nitrogen to reduce copper oxide, then continues to introduce inert gas, reduces graphene oxide at high temperature and high pressure, and then ball mills and sinters the above products to obtain an electric contact material with copper oxide, lanthanum oxide and graphene as reinforcing phases and uniformly distributed on a copper matrix. This method improves the uniformity of the reinforcing phase to a certain extent, but the preparation process is complicated, the reaction conditions are high, and it is not easy to prepare in batches.
[0005] Therefore, in order to meet various usage requirements in the actual production of silver-based electrical contact materials, developing a method for preparing silver-based electrical contact materials with simple and controllable process, low cost, and green environmental protection has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0006] In view of the above problems, the present invention aims to provide a Ag / Ti 3 SiC 2 The invention discloses a method for preparing a silver-based electrical contact material having uniform distribution of a reinforcing phase, high density, and small silver matrix grains, and at the same time, has excellent electrical conductivity, arc erosion resistance, and good mechanical properties.
[0007] Specifically, the present application is implemented through the following technical solutions:
[0008] First, the present application provides an Ag / Ti 3 SiC 2 The preparation method of the rGO electrical contact material comprises the following steps:
[0009] (1) Preparation of rGO-wrapped Ti 3 SiC 2 Composite powder:
[0010] GO powder, Ti 3 SiC 2 Powder (average particle size preferably 10-12 μm), sodium dodecyl sulfate powder, and deionized water are used as raw materials to prepare a dispersion;
[0011] Using ascorbic acid powder, hydroxypropyl methylcellulose powder, anhydrous ethanol and deionized water as raw materials, a reducing solution is prepared;
[0012] The dispersion liquid and the reducing liquid were mixed in a mass ratio of 1:1, and after stirring and ultrasonication, the graphene oxide (GO) was reduced to nano-reduced graphene oxide (rGO) and wrapped with Ti. 3 SiC 2 The powder surface; then by suction filtration, the filter residue is dried to obtain rGO-wrapped Ti 3 SiC 2 Composite powder;
[0013] The stirring rate is about 500r / min, the ultrasonic power is 80W, the reaction temperature is 75-90°C, and the reaction time is 60-80min;
[0014] (2) Mixing:
[0015] The rGO obtained in step (1) is wrapped with Ti 3 SiC2 The composite powder and Ag powder are placed in a vacuum mixing tank and mixed in a three-dimensional mixer, wherein Ag and rGO in the mixture wrap Ti 3 SiC 2 The powder mass ratio is (2.3-9):1, the vacuum degree of the vacuum mixing tank is maintained at 20kPa; the mixing time is 36-48h, and the rotation speed is 60-100r / min; the average particle size of the above-mentioned Ag powder is preferably 9-10μm.
[0016] (3) Pressing molding:
[0017] The mixed powder obtained in step (2) is pressed into a green body by a bidirectional pressing method;
[0018] (4) Vacuum sintering:
[0019] The green body prepared in step (3) is sintered in a vacuum sintering furnace, and the vacuum degree is maintained at more than 10Pa. The vacuum sintering process is as follows: the first stage: heating to 500-600°C at 5°C / min, and keeping warm for 0.5-1.5h; the second stage: heating to 940-960°C at 10°C / min, without keeping warm; the third stage: cooling to 700-850°C at a rate of 30°C / min, keeping warm for 7-10h, and then cooling with the furnace to obtain the above-mentioned Ag / Ti 3 SiC 2 / rGO electrical contact materials.
[0020] Furthermore, in step (1), the components of the dispersion are as follows, by weight: GO powder: 3-6 parts, Ti 3 SiC 2 Powder: 15-18 parts, sodium lauryl sulfate powder: 1.2-1.8 parts, deionized water: 75-80 parts; the components of the reducing solution are as follows by mass: ascorbic acid powder: 18-24 parts, hydroxypropyl methylcellulose powder: 2.4-3.2 parts, anhydrous ethanol: 5-8 parts, deionized water: 70-75 parts;
[0021] Furthermore, in the step (1), the pore size of the filtration filter paper is 0.8 μm, and the powder obtained after filtration is placed in a blast drying oven for drying at a drying temperature of 100-120° C. for a drying time of 1-3 h;
[0022] Furthermore, in the step (3), the pressing pressure used in the pressing process is 150-700 MPa, and the holding time is 1-3 min.
[0023] Secondly, the present application also provides an electrical contact, which comprises the Ag / Ti prepared by the above method. 3 SiC 2 / rGO electrical contact materials.
[0024] To achieve this purpose, in the above step (1), ascorbic acid is used to reduce the hydrophilic GO to hydrophobic nano-rGO, and sodium dodecyl sulfate and hydroxypropyl methylcellulose are used to make the rGO uniformly dispersed and wrapped in the Ti 3 SiC 2 Powder surface. Nano-rGO particles are wrapped in micron-sized Ti 3 SiC 2 Particle surface to achieve dispersed Ti 3 SiC 2 The purpose is to inhibit the Ag and Ti 3 SiC 2 At the same time, rGO has high strength and electrical and thermal conductivity. As a reinforcing phase, it can also significantly improve the mechanical properties of the material while improving the electrical conductivity of the material, thereby further improving the material's resistance to arc erosion.
[0025] To achieve this purpose, the vacuum sintering in step (4) of the present invention is divided into three stages. In the first stage, the temperature is slowly raised to 500-600° C. and kept warm, in order to fully remove the low-melting-point impurities such as dispersants and alcohol mixed in during the preparation process, so that the vacuum degree in the high-temperature stage can be maintained at a high level, and at the same time, the adsorbed oxygen on the surface of the powder is removed as much as possible, the interface between the reinforcing phase and the silver matrix is purified, the bonding force between the reinforcing phase and the silver matrix is increased, and the density of the material is improved; in the second stage, the temperature is quickly raised to 940-960° C. without keeping warm. The rapid heating to a higher sintering temperature is to make the sintered body reach the critical density. At this sintering temperature and density, the pores inside the sintered body are in an unstable state; not keeping warm is to prevent the silver matrix grains from growing too much; in the third stage, the temperature is reduced to 700-850°C at a rate of 30°C / min, kept warm for 7-10 hours and then cooled with the furnace. Since the activation energy required for grain boundary migration is greater than that for grain boundary diffusion, when the temperature is kept warm at this lower temperature, the grain boundary migration is suppressed while the grain boundary diffusion still proceeds, so that when the electrical contact material is kept warm for a long time at a lower temperature in the third stage, while obtaining a higher density, the particles do not grow, and finally an electrical contact material with a higher density and fine grains is obtained.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention firstly prepares Ti with rGO coated on the surface 3 SiC 2 Composite powder solves the problem of Ti 3 SiC 2 The problem of easy agglomeration, the comprehensive mechanical properties of the prepared electrical contact material are relatively high, and at the same time, due to the Ag and Ti 3 SiC 2The presence of rGO at the interface reduces the interfacial reaction between the two and significantly improves the conductivity of the electrical contact material. In addition, the preparation process of the composite powder does not require Ti 3 SiC 2 The powder is processed, which is green and environmentally friendly and the process is simple.
[0028] 2. The sintered body of the present invention is rapidly heated to a relatively high temperature without heat preservation, and then cooled to a relatively low temperature and heat preserved for a long time, so that the densification process of the sintered body is completed through grain boundary diffusion, and the silver matrix grain growth amplitude is relatively low. The average size of the prepared grains is about 1.5 μm, which is significantly smaller than the grain size of the silver-based alloy prepared by the existing method, and the density and arc erosion resistance of the electrical contact material are significantly improved.
[0029] 3. The present invention only requires conventional equipment, and the entire process does not pollute the environment, meets the requirements of green environmental protection, and is conducive to industrial promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The rGO-wrapped Ti prepared in Example 1 3 SiC 2 Microstructure of the composite powder (SEM image).
[0031] Figure 2 The Ag / Ti prepared in Example 1 3 SiC 2 Microstructure of / rGO electrical contact material (SEM image).
[0032] Figure 3 The Ag / Ti prepared in Example 1 3 SiC 2 Actual picture of / rGO electrical contact material. DETAILED DESCRIPTION
[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0034] The average particle size of Ag powder used in the following examples is 9-10 μm, and the average particle size of Ti 3 SiC 2 The average particle size of the powder is 10-12 μm, the average particle size of the GO powder is 200 nm, the mass percentage concentration of anhydrous ethanol is ≥99.7%, sodium dodecyl sulfate (ACS, 99%), ascorbic acid powder (ACS, 99%), and hydroxypropyl methylcellulose (ACS, 99%) are all purchased from Shanghai Aladdin Reagent Co., Ltd. The actual amount of each raw material used is used in the examples.
[0035] The agitator used in the following embodiments is a DJ1C-60S power-boosting electric agitator produced by Hailichen Bangxi Instrument Technology Co., Ltd., the mixer is a SYH-5 three-dimensional mixer produced by Songtai Instrument Co., Ltd., the tablet press is a DY-40 electric powder tablet press produced by Tianjin Keqi High-tech Co., Ltd., the vacuum sintering furnace is a ZT-15-20 sintering furnace produced by Chenhua Electric Furnace Co., Ltd., and the arc erosion resistance equipment is a JF04C electrical contact material testing system produced by Kunming Guiyan Jinfeng Co., Ltd.
[0036] The silver-based electrical contact materials prepared in the following examples were tested for relative density, Vickers hardness, electrical conductivity, and arc erosion resistance at room temperature. The relative density was measured using the water displacement method, the Vickers hardness was measured according to the GB / T4340.2-2012 standard, and the electrical conductivity was measured according to the GB / T 5586-2016 standard.
[0037] The present invention is described in detail below through specific examples, but the use and purpose of these exemplary embodiments are only used to illustrate the present invention, and do not constitute any form of limitation on the actual protection scope of the present invention, nor limit the protection scope of the present invention to these.
[0038] Example 1
[0039] (1) Preparation of rGO-wrapped Ti 3 SiC 2 Composite powder:
[0040] GO powder, Ti 3 SiC 2 Powder, sodium dodecyl sulfate powder and deionized water are used as raw materials to prepare a dispersion, wherein the mass fractions of the dispersion components are: GO powder: 3, Ti 3 SiC 2 Powder: 15, sodium lauryl sulfate powder: 1.2, deionized water: 75;
[0041] Ascorbic acid powder, hydroxypropyl methylcellulose powder, anhydrous ethanol and deionized water are used as raw materials to prepare a reducing solution, wherein the weight fractions of the reducing solution components are as follows: ascorbic acid powder: 18, hydroxypropyl methylcellulose powder: 2.4, anhydrous ethanol: 5, and deionized water: 70;
[0042] The dispersion liquid and the reducing liquid were mixed in a mass ratio of 1:1; stirred at 500 rpm, ultrasonically treated at 80 W, and reacted at 75 ° C for 80 min; then the powder obtained after filtration through a filter paper with a pore size of 0.8 μm was placed in a blast drying oven and dried at a drying temperature of 100 ° C for 3 h to obtain rGO-wrapped Ti 3 SiC 2 In this embodiment, rGO-coated Ti 3SiC 2 The microstructure of the composite powder is as follows Figure 1 As shown, the average particle size is about 15-20 μm.
[0043] (2) Mixing:
[0044] The rGO obtained in step (1) is wrapped with Ti 3 SiC 2 The composite powder and Ag powder are placed in a vacuum mixing tank and mixed in a three-dimensional mixer, wherein Ag and rGO in the mixture wrap Ti 3 SiC 2 The powder mass ratio is 2.3:1, the vacuum degree of the vacuum mixing tank is maintained at 20kPa, the mixing time is 36h, and the rotation speed is 100r / min.
[0045] (3) Pressing molding:
[0046] The mixed powder obtained in step (2) is pressed into a green body by a bidirectional pressing method, with a pressing pressure of 150 MPa and a holding time of 3 minutes.
[0047] (4) Vacuum sintering:
[0048] The green body prepared in step (3) was sintered in a vacuum sintering furnace, and the vacuum degree was maintained at more than 10Pa. The vacuum sintering process was as follows: the first stage: heating to 500°C at 5°C / min and keeping warm for 1.5h; the second stage: heating to 940°C at 10°C / min without keeping warm; the third stage: cooling to 700°C at a rate of 30°C / min, keeping warm for 10h and then cooling with the furnace to obtain Ag / Ti 3 SiC 2 / rGO electrical contact materials.
[0049] The Ag / Ti prepared in this example 3 SiC 2 The microstructure of the / rGO electrical contact material is shown in Figure 2 As shown, the reinforcement phase is uniformly distributed therein, and the average grain size of the silver matrix is about 1.5 μm.
[0050] The Ag / Ti prepared in this example 3 SiC 2 / rGO electrical contact material Figure 3 shown.
[0051] Example 2
[0052] (1) Preparation of rGO-wrapped Ti 3 SiC 2 Composite powder:
[0053] GO powder, Ti3 SiC 2 Powder, sodium dodecyl sulfate powder and deionized water are used as raw materials to prepare a dispersion, wherein the mass fractions of the components of the dispersion are as follows: GO powder: 4, Ti 3 SiC 2 Powder: 17, sodium lauryl sulfate powder: 1.5, deionized water: 78; ascorbic acid powder, hydroxypropyl methylcellulose powder, anhydrous ethanol, and deionized water are used as raw materials to prepare a reducing solution, wherein the components of the reducing solution are as follows: ascorbic acid powder: 21, hydroxypropyl methylcellulose powder: 2.8, anhydrous ethanol: 6, and deionized water: 72;
[0054] The dispersion liquid and the reducing liquid were mixed in a mass ratio of 1:1, stirred and ultrasonically reacted for 70 min at a reaction temperature of 80 °C, and then filtered with a filter paper with a pore size of 0.8 μm. The obtained powder was placed in a blast drying oven and dried at a drying temperature of 110 °C for 2 h to obtain rGO-encapsulated Ti 3 SiC 2 of composite powder.
[0055] (2) Mixing:
[0056] The rGO obtained in step (1) is wrapped with Ti 3 SiC 2 The composite powder and Ag powder are placed in a vacuum mixing tank and mixed in a three-dimensional mixer, wherein Ag and rGO in the mixture wrap Ti 3 SiC 2 The powder mass ratio is 5:1, the vacuum degree of the vacuum mixing tank is maintained at 20kPa; the mixing time is 42h, and the rotation speed is 80r / min.
[0057] (3) Pressing molding:
[0058] The mixed powder obtained in step (2) is pressed into a green body by a bidirectional pressing method, the pressing pressure is 400 MPa, and the holding time is 2 minutes.
[0059] (4) Vacuum sintering:
[0060] The green body prepared in step (3) is sintered in a vacuum sintering furnace, and the vacuum degree is maintained at more than 10Pa. The vacuum sintering process is as follows: the first stage: heating to 550°C at 5°C / min and keeping warm for 1h; the second stage: heating to 950°C at 10°C / min without keeping warm; the third stage: cooling to 775°C at a rate of 30°C / min, keeping warm for 8.5h and then cooling with the furnace.
[0061] Example 3
[0062] (1) Preparation of rGO-wrapped Ti 3 SiC2 Composite powder:
[0063] GO powder, Ti 3 SiC 2 Powder, sodium dodecyl sulfate powder and deionized water are used as raw materials to prepare a dispersion, wherein the mass fractions of the components of the dispersion are as follows: GO powder: 6, Ti 3 SiC 2 Powder: 18, sodium dodecyl sulfate powder: 1.8, deionized water: 80; ascorbic acid powder, hydroxypropyl methylcellulose powder, anhydrous ethanol, and deionized water are used as raw materials to prepare a reducing solution, wherein the components of the reducing solution are as follows: ascorbic acid powder: 24, hydroxypropyl methylcellulose powder: 3.2, anhydrous ethanol: 8, and deionized water: 80; the dispersion liquid is mixed with the reducing solution, and the mass ratio of the dispersion liquid to the reducing solution is 1:1. After stirring, ultrasonication, and reaction, the reaction temperature is 90°C, the reaction time is 60min, and the powder obtained after filtration through a filter paper with a pore size of 0.8μm is placed in a blast drying oven and dried at a drying temperature of 120°C for 1h to obtain rGO-wrapped Ti 3 SiC 2 of composite powder.
[0064] (2) Mixing:
[0065] The rGO obtained in step (1) is wrapped with Ti 3 SiC 2 The composite powder and Ag powder are placed in a vacuum mixing tank and mixed in a three-dimensional mixer, wherein Ag and rGO in the mixture wrap Ti 3 SiC 2 The powder mass ratio is 9:1, the vacuum degree of the vacuum mixing tank is maintained at 20kPa; the mixing time is 36h, and the rotation speed is 100r / min.
[0066] (3) Pressing molding:
[0067] The mixed powder obtained in step (2) is pressed into a green body by a bidirectional pressing method, the pressing pressure is 700 MPa, and the holding time is 1 min.
[0068] (4) Vacuum sintering:
[0069] The green body prepared in step (3) is sintered in a vacuum sintering furnace, and the vacuum degree is maintained at more than 10Pa. The vacuum sintering process is as follows: the first stage: heating to 600°C at 5°C / min and keeping warm for 0.5h; the second stage: heating to 960°C at 10°C / min without keeping warm; the third stage: cooling to 700°C at a rate of 30°C / min, keeping warm for 7h and then cooling with the furnace.
[0070] Table 1 Performance test results of the electrical contact materials obtained in Examples 1 to 3
[0071] Experimental Group Example 1 Example 2 Example 3 Relative density (%) 97.2 98.2 99.1 Hardness (HV) 146.3 120.5 101.3 Resistivity (μΩ·cm) 3.12 2.78 2.14 Arc energy(j) 0.91 0.85 0.72 Arcing time(ms) 4.48 4.35 4.12
[0072] The test results in Table 1 show that the electrical contact materials prepared in Examples 1-3 have improved performance compared to the existing Ag / CdO(20) materials. The electrical contact materials are subsequently processed by conventional methods (such as blanking, drawing, stamping, etc.) and welded to prepare electrical contact devices.
[0073] The above embodiments are only used to illustrate the contents of the present invention rather than to limit the present invention. Therefore, any changes within the meaning and scope equivalent to the claims of the present invention should be considered to be included in the scope of the claims.
Claims
1. Ag / Ti 3 SiC 2 Preparation method of / rGO electrical contact material, It is characterized in that The specific steps are as follows: 1) Preparation of rGO-wrapped Ti 3 SiC 2 Composite powder: GO powder, Ti 3 SiC 2 The powder, sodium lauryl sulfate and deionized water are mixed to obtain a dispersion for later use; Mix ascorbic acid, hydroxypropyl methylcellulose, anhydrous ethanol and deionized water to obtain a reducing solution for later use; The dispersion liquid and the reducing liquid were mixed in a mass ratio of 1:1, stirred, ultrasonically reacted, filtered and dried to obtain rGO-wrapped Ti 3 SiC 2 Composite powder; 2) Mixing: The rGO obtained in step 1) is wrapped around Ti 3 SiC 2 The composite powder and Ag powder are put into a vacuum mixing tank to mix to obtain a mixture; in the mixture, Ag powder and rGO encapsulate Ti 3 SiC 2 The powder mass ratio is (2.3-9):1; 3) Pressing molding: Pressing the mixture obtained in step 2) into a green body; 4) Vacuum sintering: The green body prepared in step 3) is sintered in a vacuum sintering furnace. The vacuum sintering process is as follows: the first stage: heating to 500-600°C at 5°C / min and keeping the temperature for 0.5-1.5h; The second stage: heating to 940-960°C at a rate of 10°C / min without heat preservation; the third stage: cooling to 700-850°C at a rate of 30°C / min, heat preservation for 7-10h and then cooling with the furnace to obtain the Ag / Ti 3 SiC 2 / rGO electrical contact materials.
2. According to claim 1, Ag / Ti 3 SiC 2 Preparation method of / rGO electrical contact material, It is characterized in that Step 1) In the dispersion, by weight: GO powder: 3-6 parts, Ti 3 SiC 2 Powder: 15-18 parts, sodium lauryl sulfate: 1.2-1.8 parts, deionized water: 75-80 parts; The reducing solution contains, by weight, 18-24 parts of ascorbic acid, 2.4-3.2 parts of hydroxypropyl methylcellulose, 5-8 parts of anhydrous ethanol, and 70-75 parts of deionized water.
3. According to claim 1, Ag / Ti 3 SiC 2 Preparation method of / rGO electrical contact material, It is characterized in that Step 1) The pore size of the filtration paper is 0.8 µm, and the drying refers to drying at a temperature of 100-120°C.
4. The Ag / Ti according to claim 1 3 SiC 2 Preparation method of / rGO electrical contact material, It is characterized in that Step 2) The average particle size of the Ag powder is 9-10 μm.
5. The Ag / Ti according to claim 1 3 SiC 2 Preparation method of / rGO electrical contact material, It is characterized in that Step 2) The mixing means that the mixing time is 36-48h and the rotation speed is 60-100r / min.
6. The method for preparing the Ag / Ti3SiC2 / rGO electrical contact material according to claim 1, It is characterized in that Step 3) The pressing refers to a pressure of 150-700 MPa and a pressure maintenance time of 1-3 minutes.
7. An electrical contact, It is characterized in that The electrical contact comprises Ag / Ti prepared by any of the methods in claims 1-6. 3 SiC 2 / rGO electrical contact materials.
Citation Information
Patent Citations
A method for preparing Ag / C@Ti3AlC2 contact material
CN109797307B
MAX@M composite electrical contact reinforced phase material, composite electrical contact material and preparation method
CN111834136A
Preparation method of electric contact material and electric contact
CN118221104A