Preparation method of hard alloy with high wear resistance and long service life

By modifying aluminum oxide with a vinyl silane coupling agent and carbonizing it during ball milling, the method enhances the dispersion of carbon materials in cemented carbide, resulting in improved hardness, toughness, and wear resistance, addressing the dispersion issues in traditional cemented carbide materials.

CN119082529AActive Publication Date: 2024-12-06ZHUZHOU XINDA MASCH TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411238580.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

Traditional cemented carbide materials face challenges in achieving comprehensive improvements in hardness, toughness, and wear resistance due to dispersion issues between components, particularly with carbon materials, leading to performance limitations.

Method used

A method involving the modification of aluminum oxide using a vinyl silane coupling agent, followed by a carbonization process during ball milling, to evenly distribute a carbon layer on the alumina surface, combined with WC compounds of varying sizes and rare earth elements, and optimized sintering parameters to enhance the cemented carbide's performance.

Benefits of technology

The method results in a cemented carbide with improved hardness, toughness, and wear resistance, exceeding 2000 HV 30 in hardness, 14 MPa·m 1/2 in toughness, and a wear rate below 4×10 -7 mm 3 ·N -1 ·m -1, with a longer service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention belongs to the technical field of hard alloy, and particularly relates to a preparation method of high-wear-resistance long-life hard alloy, which comprises the following steps: step 1, preparing coated aluminum oxide, step 2, weighing raw materials, step 3, carrying out ball milling, and step 4, sintering. WC of various particle sizes is used for compounding, aluminum oxide and rare earth are used for conducting comprehensive modification on the hard alloy, the optimal component formula is obtained through adjustment, the hardness, toughness and abrasion resistance of the hard alloy are synergistically improved, and the service life of the hard alloy is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cemented carbide, and in particular relates to a method for preparing a high-wear-resistant and long-life cemented carbide. Background Art

[0002] As a high-performance structural material, cemented carbide is widely used in industrial production to manufacture cutting tools, drilling equipment, molds, etc. due to its excellent hardness, wear resistance and thermal stability. Traditional cemented carbide is mainly composed of refractory metal carbides (such as tungsten carbide WC) and metal binders (such as cobalt Co). Although this material performs well in many aspects, it still has some limitations. Moreover, with the continuous deepening of industrial applications, the requirements for cemented carbide performance are getting higher and higher. Traditional cemented carbide materials are often difficult to meet performance requirements.

[0003] In order to improve the performance of cemented carbide, researchers have tried a variety of modification methods, such as adding alumina, carbon materials such as graphene, etc., which can improve the hardness and strength of cemented carbide. However, due to the dispersion problem between the components, it is difficult for the alloy material to achieve a comprehensive improvement in comprehensive performance, especially in terms of hardness, toughness and wear resistance. In view of the above problems, it is necessary to further modify cemented carbide. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for preparing a high wear-resistant and long-life cemented carbide, and the method steps are as follows:

[0005] Step 1: Preparation of coated alumina

[0006] Modifying aluminum oxide using a vinyl silane coupling agent to obtain modified aluminum oxide;

[0007] Add the modified alumina to water, add peroxide initiator, styrene and divinylbenzene, stir and disperse evenly, quickly heat to 75-95°C, react for 1-3 hours and then end the reaction, then wash with ethanol and dry for use to obtain coated alumina;

[0008] Wherein, the amount of vinyl silane coupling agent is 2-4wt% of the mass of alumina;

[0009] The mass ratio of aluminum oxide, styrene and divinylbenzene is 1:0.8-1.5:0.03-0.05;

[0010] Step 2: Weigh the raw materials

[0011] Weigh the raw materials according to the following formula: 55-85 parts of WC-1, 15-45 parts of WC-2, 6-10 parts of Co powder, 0.1-0.5 parts of Y2O3, and 0.3-0.7 parts of coated alumina;

[0012] Step 3: Ball Milling

[0013] Mix WC-1, WC-2, Co powder and Y2O3 in ethylene glycol, disperse them evenly and transfer them to a planetary ball mill for ball milling at a speed of 500-700 rpm for 1-3 h;

[0014] Stop ball milling, add coated alumina, raise the temperature to 900-1100°C, carbonize for 8-12 minutes, then start ball milling at a speed of 250-350 rpm, grind for 12-18 minutes to obtain cemented carbide composite powder;

[0015] Among them, inert gas protection is used during ball milling;

[0016] Step 4: Sintering

[0017] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1450-1500°C, the sintering pressure is 50-70MPa, the temperature is kept for 30-50min, and then the temperature is slowly lowered to room temperature.

[0018] In step 1, the vinyl silane coupling agent includes one or two of vinyl trimethoxy silane and vinyl tris (2-methoxyethoxy) silane.

[0019] The water includes one or both of deionized water and distilled water.

[0020] The peroxidation initiator includes one or more of benzoyl peroxide, dicumyl peroxide, and di-tert-butyl peroxycumene.

[0021] Preferably, the amount of the vinyl silane coupling agent is 2.5-3.5 wt % of the mass of the aluminum oxide.

[0022] Preferably, the temperature is quickly raised to 80-90° C. and the reaction is carried out for 1.5-2.5 hours.

[0023] In step 2, preferably, the raw materials are weighed according to the following formula: 60-80 parts of WC-1, 20-40 parts of WC-2, 7-9 parts of Co powder, 0.2-0.4 parts of Y2O3, and 0.4-0.6 parts of coated alumina;

[0024] Among them, the average particle size of WC-1 is 0.2-0.8μm, and the average particle size of WC-2 is 1-6μm;

[0025] Preferably, the average particle size of WC-1 is 0.4-0.6 μm, and the average particle size of WC-2 is 3-5 μm.

[0026] The average particle size of Co powder is 0.6-1μm;

[0027] The average particle size of Y2O3 is 0.4-0.6μm;

[0028] The average particle size of aluminum oxide is 0.3-0.5 μm.

[0029] In step 3, the inert gas is nitrogen or argon.

[0030] Secondly, the present invention provides a high wear-resistant and long-life cemented carbide, which is prepared using the above method.

[0031] In addition, the present invention also provides an application of a highly wear-resistant and long-life cemented carbide, which is used to prepare tunneling teeth, coal mining picks, rotary digging teeth, turning tools, milling cutters, planers, drill bits, etc.

[0032] Preferably, the cemented carbide is used to prepare tunneling teeth, coal mining picks and rotary digging teeth.

[0033] The advantages and beneficial effects of the present invention are:

[0034] (1) Aluminum oxide is added to the present invention for modification, because aluminum oxide has high hardness and high temperature stability, which can significantly improve the wear resistance of cemented carbide. In addition, the addition of aluminum oxide can also improve the fracture toughness of cemented carbide, thereby improving the impact resistance of the material.

[0035] The present invention also uses WC compound with various particle sizes, uses alumina and rare earth to comprehensively modify the cemented carbide, and adjusts to obtain the optimal component formula, thereby synergistically improving the hardness, toughness and wear resistance of the cemented carbide.

[0036] On the basis of the above formula, the present invention also optimizes the parameters of the sintering process, so that the obtained cemented carbide is denser and the performance is further improved.

[0037] (2) Previous studies have shown that carbon content has a great influence on the performance of cemented carbide. Too little or too much carbon content will lead to increased porosity and reduced density. In the prior art, carbon materials such as graphene are used to improve the mechanical properties of cemented carbide, such as strength and toughness. However, the density difference between graphene and metal matrix materials is large, and traditional mechanical mixing methods are difficult to achieve uniform dispersion, resulting in problems with the performance of the resulting cemented carbide.

[0038] Therefore, how to evenly disperse carbon materials in cemented carbide to avoid agglomeration has always been a technical problem. After many attempts and failures, the inventors creatively proposed a new modification method. This method cross-links the surface of alumina with a polymer and performs a carbonization treatment during the ball milling process. Through this innovative process, the polymer is polymerized and coated with alumina in situ, so that the carbonized network carbon chain is coated on the surface of alumina, and further evenly distributed during the ball milling process to form a carbon layer wrapped on the surface of alumina. This process solves the problem of uneven mixing of carbon materials and cemented carbide components, and can effectively improve the hardness, strength and toughness of cemented carbide, thereby improving the wear resistance and service life of the material.

[0039] (3) The present invention uses coated alumina, rare earth, etc. to modify the cemented carbide, and combines WC compounding with various particle sizes and improved process parameters to obtain cemented carbide with the best performance, with a hardness parameter exceeding 2000HV 30 , toughness parameter exceeds 14MPa·m 1 / 2 , the wear rate parameter is controlled not higher than 4×10 -7 mm 3 ·N -1 ·m -1 The obtained cemented carbide has excellent comprehensive performance.

[0040] (4) The present invention is only a simple modification with a simple process and low requirements on equipment. No new equipment needs to be introduced, the modification effect is excellent, and it has broad application prospects. DETAILED DESCRIPTION

[0041] In order to enable those skilled in the art to better understand the solutions of the present invention and to make the technical means, creative features, objectives and effects achieved by the present invention easier to understand, the technical solutions in the embodiments of the present invention are clearly and completely described below.

[0042] This embodiment is only a part of the embodiments of the present invention, and does not represent all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0043] raw material

[0044] WC-1, average particle size D50 is 0.5 μm;

[0045] WC-2, average particle size D50 is 4 μm;

[0046] Co powder, average particle size D50 is 0.8 μm;

[0047] Y2O3, average particle size D50 is 0.5 μm;

[0048] Alumina, average particle size D50 is 0.4 μm.

[0049] Example 1

[0050] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0051] Step 1: Preparation of coated alumina

[0052] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0053] Add the modified alumina to water, add benzoyl peroxide, styrene and divinylbenzene, stir and disperse evenly, quickly heat to 85°C, react for 2 hours and then end the reaction, then wash with ethanol and dry for use to obtain coated alumina;

[0054] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0055] The mass ratio of alumina, styrene and divinylbenzene is 1:1:0.04;

[0056] Step 2: Weigh the raw materials

[0057] The raw materials were weighed according to the following formula: 60 parts of WC-1, 40 parts of WC-2, 7 parts of Co powder, 0.2 parts of Y2O3, and 0.4 parts of coated alumina;

[0058] Step 3: Ball Milling

[0059] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0060] Stop the ball milling, add coated alumina, raise the temperature to 1000°C, carbonize for 10 minutes, start the ball milling at a speed of 300 rpm, and grind for 15 minutes to obtain cemented carbide composite powder;

[0061] N2 protection was used during ball milling;

[0062] Step 4: Sintering

[0063] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0064] Example 2

[0065] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0066] Step 1: Preparation of coated alumina

[0067] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0068] Add the modified alumina to water, add benzoyl peroxide, styrene and divinylbenzene, stir and disperse evenly, quickly heat to 85°C, react for 2 hours and then end the reaction, then wash with ethanol and dry for use to obtain coated alumina;

[0069] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0070] The mass ratio of alumina, styrene and divinylbenzene is 1:1:0.04;

[0071] Step 2: Weigh the raw materials

[0072] The raw materials were weighed according to the following formula: 70 parts of WC-1, 30 parts of WC-2, 8 parts of Co powder, 0.3 parts of Y2O3, and 0.5 parts of coated alumina;

[0073] Step 3: Ball Milling

[0074] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0075] Stop the ball milling, add coated alumina, raise the temperature to 1000°C, carbonize for 10 minutes, start the ball milling at a speed of 300 rpm, and grind for 15 minutes to obtain cemented carbide composite powder;

[0076] N2 protection was used during ball milling;

[0077] Step 4: Sintering

[0078] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0079] Example 3

[0080] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0081] Step 1: Preparation of coated alumina

[0082] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0083] Add the modified alumina to water, add benzoyl peroxide, styrene and divinylbenzene, stir and disperse evenly, quickly heat to 85°C, react for 2 hours and then end the reaction, then wash with ethanol and dry for use to obtain coated alumina;

[0084] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0085] The mass ratio of alumina, styrene and divinylbenzene is 1:1:0.04;

[0086] Step 2: Weigh the raw materials

[0087] The raw materials were weighed according to the following formula: 80 parts of WC-1, 20 parts of WC-2, 9 parts of Co powder, 0.4 parts of Y2O3, and 0.6 parts of coated alumina;

[0088] Step 3: Ball Milling

[0089] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0090] Stop the ball milling, add coated alumina, raise the temperature to 1000°C, carbonize for 10 minutes, start the ball milling at a speed of 300 rpm, and grind for 15 minutes to obtain cemented carbide composite powder;

[0091] N2 protection was used during ball milling;

[0092] Step 4: Sintering

[0093] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0094] Comparative Example 1

[0095] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0096] Step 1: Preparation of modified alumina

[0097] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0098] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0099] Step 2: Weigh the raw materials

[0100] The raw materials were weighed according to the following formula: 70 parts of WC-1, 30 parts of WC-2, 8 parts of Co powder, 0.3 parts of Y2O3, and 0.5 parts of modified alumina;

[0101] Step 3: Ball Milling

[0102] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0103] Stop the ball milling, add modified alumina, raise the temperature to 1000°C, heat for 10 minutes, start the ball milling at a speed of 300 rpm, and grind for 15 minutes to obtain cemented carbide composite powder;

[0104] N2 protection was used during ball milling;

[0105] Step 4: Sintering

[0106] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0107] Comparative Example 2

[0108] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0109] Step 1: Prepare the Alumina Mixture

[0110] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0111] mixing the modified alumina and polystyrene to obtain an alumina mixture;

[0112] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0113] The mass ratio of alumina to polystyrene is 1:1:0.04;

[0114] Step 2: Weigh the raw materials

[0115] The raw materials were weighed according to the following formula: 70 parts of WC-1, 30 parts of WC-2, 8 parts of Co powder, 0.3 parts of Y2O3, and 0.5 parts of alumina mixture;

[0116] Step 3: Ball Milling

[0117] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0118] Stop the ball milling, add the alumina mixture, raise the temperature to 1000°C, and start the ball milling after carbonization for 10 minutes at a speed of 300 rpm. Grind for 15 minutes to obtain the cemented carbide composite powder.

[0119] N2 protection was used during ball milling;

[0120] Step 4: Sintering

[0121] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0122] Comparative Example 3

[0123] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0124] Step 1: Prepare the Alumina Mixture

[0125] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0126] adding graphene and mixing with the modified alumina to obtain an alumina mixture;

[0127] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0128] The ratio of alumina to graphene is 1:1;

[0129] Step 2: Weigh the raw materials

[0130] The raw materials were weighed according to the following formula: 70 parts of WC-1, 30 parts of WC-2, 8 parts of Co powder, 0.3 parts of Y2O3, and 0.5 parts of alumina mixture;

[0131] Step 3: Ball Milling

[0132] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0133] Stop the ball milling, add the alumina mixture, raise the temperature to 1000°C, and start the ball milling after heating for 10 minutes at a speed of 300 rpm. After grinding for 15 minutes, obtain the cemented carbide composite powder;

[0134] N2 protection was used during ball milling;

[0135] Step 4: Sintering

[0136] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0137] Comparative Example 4

[0138] A method for preparing a high wear-resistant and long-life cemented carbide, the method steps are as follows:

[0139] Step 1: Preparation of coated alumina

[0140] Modifying aluminum oxide with vinyltrimethoxysilane to obtain modified aluminum oxide;

[0141] Add the modified alumina to water, add benzoyl peroxide, styrene and divinylbenzene, stir and disperse evenly, quickly heat to 85°C, react for 2 hours and then end the reaction, then wash with ethanol and dry for use to obtain coated alumina;

[0142] Wherein, the amount of silane coupling agent is 3wt% of the mass of alumina;

[0143] The mass ratio of alumina, styrene and divinylbenzene is 1:2.5:0.04;

[0144] Step 2: Weigh the raw materials

[0145] The raw materials were weighed according to the following formula: 70 parts of WC-1, 30 parts of WC-2, 8 parts of Co powder, 0.3 parts of Y2O3, and 0.5 parts of coated alumina;

[0146] Step 3: Ball Milling

[0147] WC-1, WC-2, Co powder and Y2O3 were mixed in ethylene glycol, dispersed evenly and then transferred to a planetary ball mill for ball milling at a speed of 600 rpm for 2 h;

[0148] Stop the ball milling, add coated alumina, raise the temperature to 1000°C, carbonize for 10 minutes, start the ball milling at a speed of 300 rpm, and grind for 15 minutes to obtain cemented carbide composite powder;

[0149] N2 protection was used during ball milling;

[0150] Step 4: Sintering

[0151] The spark plasma sintering process is adopted for sintering, the sintering temperature is 1480℃, the sintering pressure is 60MPa, the temperature is kept for 40min, and then the temperature is slowly cooled to room temperature.

[0152] test

[0153] The modified cemented carbide was tested for performance, wherein the Vickers hardness was measured by a Vickers hardness tester; the strength and fracture toughness of the alloy were measured by a three-point bending fracture test; and the friction and wear test was conducted by a ball-disc method, with a loading force of 100N, a rotation speed of 500r / min, and a time of 30min. The test was generally performed by taking the average data of three groups, and the test results are shown in Table 1 below.

[0154] Table 1: Cemented carbide properties

[0155]

[0156] As can be seen from the above, in Examples 1-3, the carbon material is uniformly cross-linked and coated on the surface of aluminum oxide, which can effectively improve the comprehensive properties of cemented carbide, such as hardness, strength, toughness and wear. In Comparative Example 1, only aluminum oxide is added. Although the cemented carbide has a higher hardness, the improvement in comprehensive performance is limited. In Comparative Example 3, graphene is added, but the dispersion effect is not good. Although the strength of the alloy material is not bad, the toughness and wear performance are average. In Comparative Example 4, the content of carbon material added is relatively high, and the hardness, strength, etc. are significantly reduced, which also leads to a shortened service life.

[0157] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a high wear-resistant and long-life cemented carbide, the technical feature of which is that the method comprises the following steps: Step 1: Preparation of coated alumina Modifying aluminum oxide using a vinyl silane coupling agent to obtain modified aluminum oxide; Add the modified alumina to water, add peroxide initiator, styrene and divinylbenzene, stir and disperse evenly, quickly heat to 75-95°C, react for 1-3 hours and then end the reaction, then wash with ethanol and dry for use to obtain coated alumina; in, The amount of vinyl silane coupling agent is 2-4wt% of the mass of alumina; The mass ratio of aluminum oxide, styrene and divinylbenzene is 1:0.8-1.5:0.03-0.05; Step 2: Weigh the raw materials Weigh the raw materials according to the following formula: WC-1 55-85 parts, WC-2 15-45 parts, Co powder 6-10 parts, Y2O3 0.1-0.5 parts, coated alumina 0.3-0.7 parts; Among them, the average particle size of WC-1 is 0.2-0.8μm, and the average particle size of WC-2 is 1-6μm; Step 3: Ball Milling Mix WC-1, WC-2, Co powder and Y2O3 in ethylene glycol, disperse them evenly and transfer them to a planetary ball mill for ball milling at a speed of 500-700 rpm for 1-3 h; Stop ball milling, add coated alumina, raise the temperature to 900-1100°C, carbonize for 8-12 minutes, then start ball milling at a speed of 250-350 rpm, grind for 12-18 minutes to obtain cemented carbide composite powder; Among them, inert gas protection is used during ball milling; Step 4: Sintering The spark plasma sintering process is adopted for sintering, the sintering temperature is 1450-1500°C, the sintering pressure is 50-70MPa, the temperature is kept for 30-50min, and then the temperature is slowly lowered to room temperature.

2. The preparation method according to claim 1, wherein in step 1, the vinyl silane coupling agent comprises one or both of vinyl trimethoxy silane and vinyl tris (2-methoxyethoxy) silane.

3. The preparation method according to claim 1, wherein in step 1, the water comprises one or both of deionized water and distilled water.

4. The preparation method according to claim 1, wherein in step 1, the peroxidation initiator comprises one or more of benzoyl peroxide, dicumyl peroxide, and di-tert-butyl peroxycumene.

5. The preparation method according to claim 1, wherein in step 1, the amount of the vinyl silane coupling agent is 2.5-3.5 wt% of the mass of the alumina.

6. The preparation method according to claim 1, wherein in step 1, the temperature is rapidly raised to 80-90°C and the reaction is carried out for 1.5-2.5 hours.

7. The preparation method according to claim 1, wherein in step 2, the raw materials are weighed according to the following formula: 60-80 parts of WC-1, 20-40 parts of WC-2, 7-9 parts of Co powder, 0.2-0.4 parts of Y2O3, and 0.4-0.6 parts of coated alumina.

8. The preparation method according to claim 1, wherein in step 2, the average particle size of WC-1 is 0.4-0.6 μm, the average particle size of WC-2 is 3-5 μm; the average particle size of Co powder is 0.6-1 μm; the average particle size of Y2O3 is 0.4-0.6 μm; and the average particle size of alumina is 0.3-0.5 μm.

9. The preparation method according to claim 1, wherein in step 3, the inert gas is nitrogen or argon.

10. A high wear-resistant and long-life cemented carbide, the technical feature of which is that it is prepared using the method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Bicrystal cemented carbide and preparation method thereof

    CN107267836A

  • Alumina-based ceramic tool material containing graphene coated alumina composite powder and preparation method of alumina-based ceramic tool material

    CN107555965A

  • WC-Co hard alloy added with graphene / nanometer Al2O3 particles and preparation method

    CN114277298A

  • Preparation method of high-hardness, high-strength and high-toughness modified hard alloy

    CN117187615A

  • METHOD FOR PRODUCING SINTERED HARD ALLOYS

    RU2013135523A