Aluminum alloy iron removal agent, aluminum alloy iron removal method and aluminum alloy

By using iron removers with manganese, boron and beryllium elements in aluminum alloys, the problems of low iron removal rate and complex process in the prior art are solved, and the iron impurities are efficiently removed and the casting temperature range of the aluminum liquid is broadened, thereby improving the The mechanical properties of aluminum alloys.

CN119082530APending Publication Date: 2024-12-06CHONGQING CHANGAN AUTOMOBILE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411222283.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing aluminum alloy iron removal technology has problems such as low iron removal rate, complex process operation, high energy consumption and high requirements for iron removal temperature control, especially the poor removal effect of small amounts of iron impurities.

Method used

Using an aluminum alloy iron removal agent containing manganese, boron and beryllium elements, Fe2B precipitation is formed through manganese and iron, boron element deteriorates and enriches iron phase, and beryllium element improves the morphology of iron intermetallic compounds, thereby achieving efficient removal of iron impurities, and Broaden the iron removal insulation temperature range.

Benefits of technology

A high iron removal rate (39%~56%) is achieved, which reduces the complexity of process operation and energy consumption, broadens the casting temperature range of aluminum liquid, and improves the mechanical properties of aluminum alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082530A_ABST
    Figure CN119082530A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy iron removal, and discloses an aluminum alloy iron removal agent which comprises a substance containing a manganese element, a substance containing a boron element and a substance containing a beryllium element, and the mass ratio of the manganese element to the boron element is (2: 1)-(20: 1); the mass ratio of the boron element to the beryllium element is (0.8: 1)-(1.2: 1). The manganese element, the boron element and the beryllium element have a synergistic effect, iron element impurities in the aluminum alloy are effectively removed, all the elements only react with the iron element, meanwhile, the elements do not react with other elements, the phenomenon that a matrix is damaged due to the generated impurities is avoided, and the iron removal effect is stable. The invention further discloses an aluminum alloy iron removal method and an aluminum alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of aluminum alloy iron removal, for example, to an aluminum alloy iron removal agent, an aluminum alloy iron removal method and an aluminum alloy. Background Art

[0003] Among the impurity elements in recycled aluminum, iron is the most important element. Iron-containing impurities usually have a significant impact on the mechanical properties and casting properties of aluminum alloys. The effects of iron-containing impurities on mechanical properties are mainly manifested in: promoting crack initiation and propagation, reducing fatigue life, and reducing wear resistance. As a hard and brittle phase in aluminum alloys, iron-rich intermetallic compounds have no plasticity themselves and are generally considered to reduce mechanical properties. Under stress, stress concentration will occur around iron-rich intermetallic compounds, leading to crack initiation and accelerated crack propagation, reducing the effective load-bearing area in recycled aluminum alloys, resulting in a gradual decrease in its tensile strength, yield strength, and elongation, and its influence on elongation is much higher than that on tensile strength and yield strength. In addition, during the solidification process, the needle-like iron-rich phase will block the flow of aluminum melt between dendrites, resulting in defects such as shrinkage cavities and looseness in the ingot.

[0004] There are two common methods to eliminate the influence of iron phase: one is to add modifiers such as Mn, Cr, Co, V and Ce to transform the originally harmful needle-shaped iron-rich phase into a less harmful Chinese character or block-shaped phase; the other is to remove iron from aluminum alloys by physical or chemical methods, such as centrifugation, gravity sedimentation, electromagnetic separation and filtration. However, among the physical or chemical methods, the centrifugal separation method is difficult to operate and is only suitable for small-scale iron removal in the laboratory; the electromagnetic separation method has extremely high energy consumption, which greatly increases the cost of iron removal; the filtration method can only be applied to larger impurities, and has a poor effect on smaller impurities, and has extremely high requirements for the filter.

[0005] It can be seen that the existing modifiers or methods for eliminating the iron phase have their own advantages and disadvantages. While achieving iron removal, there are problems such as high process operation requirements.

[0006] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present application, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0007] In order to provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. The summary is not an extensive review, nor is it intended to identify key / critical components or delineate the scope of protection of these embodiments, but rather serves as a prelude to the detailed description that follows.

[0008] The embodiments of the present disclosure provide an aluminum alloy iron removal agent, an aluminum alloy iron removal method, and an aluminum alloy, which can ensure a reliable iron removal rate without introducing other impurities, and can widen the iron removal insulation temperature, thereby widening the pouring temperature of the aluminum liquid after iron removal, reducing the control accuracy of the iron removal method on the iron removal temperature and the subsequent pouring temperature, and reducing the process requirements.

[0009] In some embodiments, the aluminum alloy iron remover includes: a substance containing manganese, a substance containing boron, and a substance containing beryllium, wherein the mass ratio of manganese to boron is (2:1) to (20:1); the mass ratio of boron to beryllium is (0.8:1) to (1.2:1).

[0010] In some embodiments, the aluminum alloy iron removal method includes: obtaining aluminum liquid A to be iron removed; adjusting the temperature of aluminum liquid A to 700-710°C, and then adding the aforementioned aluminum alloy iron remover to the aluminum liquid A to remove iron to obtain aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 0.1%-5%, the mass percentage of boron element is 0.05%-1.5%, and the mass percentage of beryllium element is 0.05%-1.5%; refining the aluminum liquid B to obtain aluminum liquid C; allowing the aluminum liquid C to stand at 630-720°C, and then filtering.

[0011] In some embodiments, the aluminum alloy is obtained by casting the deironing aluminum liquid obtained by the aforementioned aluminum alloy deironing method.

[0012] The aluminum alloy iron removal agent, aluminum alloy iron removal method and aluminum alloy provided in the embodiments of the present disclosure can achieve the following technical effects:

[0013] In the aluminum alloy deironing agent of the disclosed embodiment, the basic principle of introducing B element to remove iron is that B element and iron element form Fe2B, and then sink in the form of precipitation to form slag, thereby reducing the content of Fe element. The basic principle of introducing Mn element to remove iron is that Mn element serves the purpose of modifying the iron-rich phase, thereby causing the needle-shaped β-AlFeSi phase to be unable to form, and excessive Mn will cause the needle-shaped iron phase morphology to change into Chinese character shape or hexagon; the basic principle of introducing Be element to remove iron is that Be element makes the brittle iron metal compound crystals in Al alloy change from coarse needle shape and layer shape to fine equiaxed shape, thereby improving the strength and plasticity of the casting. The elements in the aluminum alloy deironing agent of the disclosed embodiment not only satisfy the reaction with iron element only, but also will not react with other elements to produce impurities that damage the matrix. In summary, manganese, boron and beryllium work synergistically to effectively remove iron impurities in aluminum alloys, with a high iron removal rate; moreover, the iron removal insulation temperature range of molten aluminum is effectively widened, thereby widening the casting temperature range of aluminum alloys, reducing process requirements, and ensuring a high removal rate of impurity iron within the iron removal insulation temperature range of 630 to 720°C (or casting temperature), with an iron removal rate of 39% to 56%.

[0014] The aluminum alloy deironing method of the disclosed embodiment is simple in process and easy to operate. Moreover, the insulation temperature range of the aluminum liquid C is wide (630-720°C), which reduces the control requirements for the deironing insulation temperature during the deironing process, thereby making the pouring temperature range of the aluminum liquid C wide, effectively broadening the pouring temperature range of the aluminum alloy and reducing the process requirements.

[0015] The aluminum alloy of the disclosed embodiment is obtained by pouring aluminum liquid after iron removal using the aforementioned iron removal method, and the Fe content is significantly reduced, thereby improving the mechanical properties.

[0016] The above general description and the following description are exemplary and explanatory only and are not intended to limit the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] One or more embodiments are exemplarily described by corresponding drawings, which do not limit the embodiments. Elements with the same reference numerals in the drawings are shown as similar elements, and the drawings do not constitute a scale limitation, and wherein:

[0018] Figure 1 It is a flowchart of a method for removing iron from aluminum alloy provided by an embodiment of the present disclosure;

[0019] Figure 2 is a metallographic micrograph of an aluminum-silicon alloy having an iron content of 1 wt % used in Example 1 provided in the embodiments of the present disclosure;

[0020] Figure 3is a metallographic micrograph of the iron-removed aluminum alloy obtained in Example 1 after iron removal provided in the embodiments of the present disclosure;

[0021] Figure 4 It is a metallographic micrograph of the iron-removed aluminum alloy obtained in Example 2 provided in the embodiments of the present disclosure after iron removal. DETAILED DESCRIPTION

[0022] In order to be able to understand the features and technical contents of the embodiments of the present disclosure in more detail, the implementation of the embodiments of the present disclosure is described in detail below in conjunction with the accompanying drawings. The attached drawings are for reference only and are not used to limit the embodiments of the present disclosure. In the following technical description, for the convenience of explanation, a full understanding of the disclosed embodiments is provided through multiple details. However, one or more embodiments can still be implemented without these details. In other cases, to simplify the drawings, well-known structures and devices can be simplified for display.

[0023] The terms "first", "second", etc. in the specification and claims of the embodiments of the present disclosure and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchanged where appropriate, so that the embodiments of the embodiments of the present disclosure described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions.

[0024] Unless otherwise stated, the term "plurality" means two or more.

[0025] In the embodiment of the present disclosure, the character " / " indicates that the preceding and following objects are in an "or" relationship. For example, A / B indicates: A or B.

[0026] The term "and / or" is a description of the association relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A or B, or, A and B.

[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present disclosure may be combined with each other.

[0028] An embodiment of the present disclosure provides an aluminum alloy iron remover, characterized in that it includes a substance containing manganese element, a substance containing boron element and a substance containing beryllium element, wherein the mass ratio of manganese element to boron element is (2:1) to (20:1); the mass ratio of boron element to beryllium element is (0.8:1) to (1.2:1).

[0029] The aluminum alloy deironing agent of the disclosed embodiment has a substance containing manganese element, a substance containing boron element and a substance containing beryllium element as main components, wherein the B element reacts chemically with the iron element to form an Fe-B compound (e.g., Fe2B), which then sinks in the form of precipitation to form slag, and is captured and discharged in the form of slag, thereby reducing the content of the Fe element. The Mn element serves the purpose of modifying the iron-rich phase, thereby causing the needle-like β-AlFeSi phase to be unable to form, and excessive Mn can transform the needle-like iron phase morphology into a Chinese character shape or a hexagon. The Be element transforms the brittle iron intermetallic compound crystals in the Al alloy from coarse needles and layers into fine equiaxed shapes, thereby improving the strength and plasticity of the casting. The introduced element not only satisfies the reaction with the iron element only, but also does not react with other elements to produce impurities that damage the matrix. In summary, manganese, boron and beryllium work synergistically to effectively remove iron impurities in aluminum alloys. Moreover, the casting temperature range of aluminum alloys is effectively widened. A high removal rate of impure iron can be guaranteed within the casting temperature range of 630 to 720°C, and the iron removal rate reaches 39% to 56%.

[0030] The aluminum alloy iron remover of the disclosed embodiment is suitable for Al-Si alloys. Mn and Fe have similar atomic radii. The addition of elemental Mn and its compounds prompts Fe atoms to preferentially replace Mn atoms in the AlMnSi phase, so that the Fe element preferentially forms the Chinese character-shaped α-Al(Fe,Mn)Si phase, which has less harm to the alloy performance, and serves the purpose of modifying the iron-rich phase, thereby preventing the needle-shaped β-AlFeSi phase from forming. Excessive Mn will cause the needle-shaped iron phase morphology to be transformed into a Chinese character shape or hexagon.

[0031] The aluminum alloy iron remover of the embodiment of the present disclosure is suitable for removing iron from aluminum alloys with an iron content of 0.5% to 1%.

[0032] In the aluminum alloy iron remover of the embodiment of the present disclosure, the substance containing the manganese element includes elemental manganese and / or manganese-containing compounds.

[0033] Optionally, the manganese-containing compound includes an aluminum-manganese alloy. In the aluminum-manganese alloy, the mass percentage of manganese is not limited, and optionally, the mass percentage of manganese is 5% to 15%, for example, the mass percentage of manganese is 5%, 10%, 11%, 12%, 13%, 14%, 15% or any other value within the range of 5% to 15%.

[0034] In the aluminum alloy iron remover of the embodiment of the present disclosure, the substance containing the boron element includes elemental boron and / or boron-containing compounds.

[0035] Optionally, the boron-containing compound includes an aluminum-boron alloy. In the aluminum-boron alloy, the mass percentage of boron is not limited, and optionally, the mass percentage of boron is 1% to 10%, for example, the mass percentage of boron is 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any other value within the range of 1% to 10%.

[0036] In the aluminum alloy iron remover of the embodiment of the present disclosure, the substance containing the beryllium element includes elemental beryllium and / or beryllium-containing compounds.

[0037] Optionally, the beryllium-containing compound includes an aluminum-beryllium alloy. In the aluminum-beryllium alloy, the mass percentage of beryllium is not limited, and optionally, the mass percentage of beryllium is 1% to 10%, for example, the mass percentage of boron is 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any other value within the range of 1% to 10%.

[0038] In some embodiments, in the aluminum alloy iron remover, the mass ratio of manganese element to boron element is (2.5:1) to (15:1); and / or, the mass ratio of boron element to beryllium element is 1:1.

[0039] Combination Figure 1 As shown, a method for removing iron from aluminum alloy according to an embodiment of the present disclosure includes:

[0040] S10, obtaining aluminum liquid A to be deironed.

[0041] S20, adjusting the temperature of the aluminum liquid A to 700-710° C., then adding the aforementioned aluminum alloy iron remover to the aluminum liquid A to remove iron, thereby obtaining aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 0.1%-5%, the mass percentage of boron element is 0.05%-1.5%, and the mass percentage of beryllium element is 0.05%-1.5%;

[0042] S30, refining the aluminum liquid B to obtain aluminum liquid C;

[0043] S40, allowing the aluminum liquid C to stand at 630-720° C., and then filtering.

[0044] The aluminum alloy deironing method of the disclosed embodiment is simple in process and easy to operate. Moreover, the insulation temperature range of the aluminum liquid C is wide (630-720°C), which broadens the deironing temperature and reduces the control requirements for the deironing temperature; and the pouring temperature range of the filtered aluminum liquid C is broadened, which effectively broadens the pouring temperature range of the aluminum alloy and reduces the process requirements.

[0045] In the disclosed embodiment, in step S10, the aluminum liquid A can be obtained by heating and melting an aluminum alloy block (e.g., an aluminum alloy ingot) from which iron needs to be removed at a high temperature, or can be obtained by heating and melting raw materials measured according to the target aluminum alloy composition.

[0046] In one example, in step S10, obtaining aluminum liquid A to be de-ironized includes: placing an aluminum-silicon alloy containing iron in a crucible, heating and melting it, and obtaining aluminum liquid A to be de-ironized. The crucible may be a crucible with an inner wall coated with a coating, and the coating is not limited, for example, a commercially available product, Mabel coating agent.

[0047] In another example, in step S10, obtaining the aluminum liquid A to be de-ironized includes: preparing various raw materials according to the stoichiometric ratio of various metal components in the aluminum-silicon alloy, placing the raw materials in a crucible, and then heating and melting the raw materials to obtain the aluminum liquid A to be de-ironized. The crucible can be a crucible with an inner wall coated with a coating, and the coating is not limited, for example, a commercially available product, Mabao coating agent.

[0048] The method of obtaining a crucible with an inner wall coated with the coating comprises: preheating the crucible to 150° C., then uniformly coating the coating on the inner wall of the crucible, and then heating and drying to obtain a crucible with an inner wall coated with the coating. The heating and drying temperature can be determined according to the coating used.

[0049] In some embodiments, in step S20, in the aluminum liquid B, the mass percentage of manganese element is 1% to 5%, the mass percentage of boron element is 0.1% to 1%, and the mass percentage of beryllium element is 0.1% to 1%. In this embodiment, the iron removal effect is improved by further controlling the amount of each metal element added to the iron removal agent.

[0050] Optionally, in step S20, in the aluminum liquid B, the mass percentage of manganese element is 1% to 3%, the mass percentage of boron element is 0.1% to 0.8%, and the mass percentage of beryllium element is 0.1% to 0.8%.

[0051] In some embodiments, in step S20, in the aluminum liquid B, the mass ratio of manganese element to iron element is (0.1:1) to (6:1); and / or, the mass ratio of boron element to iron element is (0.05:1) to (1.5:1); and / or, the mass ratio of beryllium element to iron element is (0.05:1) to (1.5:1). In this embodiment, by controlling the mass ratio of each metal element to Fe element in the deironing agent, the deironing effect can be closer to the ideal one, thereby improving the deironing rate.

[0052] Optionally, in step S20, in the aluminum liquid B, the mass ratio of manganese element to iron element is (1.5﹕1) to (6﹕1); and / or, the mass ratio of boron element to iron element is (0.1﹕1) to (1﹕1); and / or, the mass ratio of beryllium element to iron element is (0.1﹕1) to (1﹕1).

[0053] Optionally, in step S20, in the aluminum liquid B, the mass ratio of manganese element to iron element is (1.9﹕1) to (5.5﹕1); and / or, the mass ratio of boron element to iron element is (0.2﹕1) to (0.8﹕1); and / or, the mass ratio of beryllium element to iron element is (0.2﹕1) to (0.8﹕1).

[0054] In some embodiments, in step S30, the aluminum liquid B is subjected to a refining treatment, including: controlling the temperature of the aluminum liquid B at 720-740° C., and introducing an inert gas carrying a refining agent powder into the aluminum liquid B to perform a powder spraying refining and slag removal treatment.

[0055] Optionally, the refining agent is a salt solvent that does not contain sodium ions.

[0056] Optionally, the refining agent includes a sodium-free chloride salt or fluoride salt, such as a commercially available sodium-free refining agent such as the refining agent model HNJK-J101 produced by Henan Jingkang Industrial Co., Ltd.

[0057] Optionally, the amount of the refining agent added is 0.3% to 1.2% of the weight of the aluminum liquid B.

[0058] Optionally, the amount of the refining agent added is 0.5% of the weight of the aluminum liquid B.

[0059] In some embodiments, in step S40, the aluminum liquid C is kept at 630-720° C. for 20-60 minutes. Optionally, the standing time is 20-50 minutes. Optionally, the standing time is 30 minutes.

[0060] In some embodiments, after step S40, the method further includes: pouring the iron-removed aluminum liquid obtained after step S40 at a temperature of 630 to 720° C. to obtain an iron-removed aluminum alloy.

[0061] In some embodiments, in step S20, before adding the aluminum alloy iron remover as claimed in any one of claims 1 to 4 to the aluminum liquid A, the step further includes: preheating and drying the aluminum alloy iron remover to dry the aluminum alloy iron remover to avoid the introduction of moisture.

[0062] Optionally, the aluminum alloy iron remover is preheated and dried, including: preheating the aluminum alloy iron remover to 180° C. to 240° C., and preheating and drying.

[0063] It is understandable that in some steps, such as step S20 and step S30, the composition of the molten aluminum (liquid aluminum B and liquid aluminum C) can also be analyzed before the furnace to detect the component content of the molten aluminum, and the melt with a deviation in content can be supplemented or diluted to make its composition reach an acceptable range.

[0064] Specific examples are provided below to more specifically illustrate the aluminum alloy iron removal agent and aluminum alloy iron removal method according to the embodiments of the present disclosure.

[0065] Example 1

[0066] An aluminum alloy iron remover I comprises an aluminum-manganese alloy, an aluminum-boron alloy and an aluminum-beryllium alloy, wherein the mass ratio of manganese element to boron element is 5:1; and the mass ratio of boron element to beryllium element is 1:1.

[0067] A method for removing iron from an aluminum alloy using the aluminum alloy iron remover I of Example 1 comprises:

[0068] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.53%.

[0069] The temperature of the aluminum liquid A is adjusted to 710°C, and then the aluminum alloy iron remover I is added to the aluminum liquid A to remove iron to obtain aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 1%, the mass percentage of boron element is 0.2%, and the mass percentage of beryllium element is 0.2%; that is, in the aluminum liquid B, the mass ratio of manganese element to iron element is 1.9:1, the mass ratio of boron element to iron element is 0.4:1, and the mass ratio of beryllium element to iron element is 0.4:1.

[0070] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added, and after the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C. The Al-Si special refining agent was dispersed in the inert gas, and the inert gas carrying the Al-Si special refining agent was added to the aluminum liquid B by powder spraying to perform slag removal.

[0071] The aluminum liquid C was kept at 630-720°C for 30 minutes, and then filtered to remove the surface scum; and the iron-removed aluminum liquid I was obtained.

[0072] In this embodiment 1, the obtained aluminum liquid after iron removal is poured to obtain the corresponding aluminum alloy I after iron removal. It can be understood that the pouring temperature is the heat preservation and standing temperature (iron removal temperature) of the aluminum liquid C.

[0073] In this Example 1, the aluminum liquid C is kept at 630°C, 680°C and 720°C for 30 minutes, respectively, to obtain deironized aluminum liquid Ⅰ-1, deironized aluminum liquid Ⅰ-2 and deironized aluminum liquid Ⅰ-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring each deironized aluminum liquid at the corresponding holding temperature are recorded as deironized aluminum alloy Ⅰ-1, deironized aluminum alloy Ⅰ-2 and deironized aluminum alloy Ⅰ-3, respectively.

[0074] In this Example 1, the original Fe content of the aluminum liquid A and the Fe content after iron removal in each aluminum liquid I after iron removal were detected, and the tensile strength and elongation of each iron-removed aluminum alloy I obtained by casting were detected, and the test results are shown in Table 1. Among them, the original Fe content of the aluminum liquid A is 0.53%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0075] Table 1

[0076]

[0077] It can be seen from Table 1 that the iron removal rate is between 39.5% and 47.8% when Mn:B=5:1 and B:Be=1:1. When the iron removal insulation temperature is 680℃, the iron removal rate is better.

[0078] Figure 2 This is a metallographic micrograph of the aluminum-silicon alloy with an iron content of 1 wt% used in Example 1. Figure 3 This is a metallographic micrograph of the iron-removed aluminum alloy I-2 obtained in Example 1, compared with Figure 2 and Figure 3 It can be seen that the addition of the iron remover gradually reduces the content of the needle-shaped iron-rich phase in the alloy, while the short rod-shaped iron phase structure increases.

[0079] Example 2

[0080] An aluminum alloy iron remover II comprises an aluminum-manganese alloy, an aluminum-boron alloy and an aluminum-beryllium alloy, wherein the mass ratio of manganese element to boron element is 15:1; the mass ratio of boron element to beryllium element is 1:1.

[0081] The method for removing iron from aluminum alloy using the aluminum alloy iron remover II of Example 2 comprises:

[0082] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.55%.

[0083] The temperature of the aluminum liquid A is adjusted to 710°C, and then aluminum alloy iron remover II is added to the aluminum liquid A to remove iron to obtain aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 3%, the mass percentage of boron element is 0.2%, and the mass percentage of beryllium element is 0.2%; that is, in the aluminum liquid B, the mass ratio of manganese element to iron element is 5.5:1, the mass ratio of boron element to iron element is 0.4:1, and the mass ratio of beryllium element to iron element is 0.4:1.

[0084] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added. After the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C;

[0085] The aluminum liquid C was kept at 630-720°C for 30 minutes, and then filtered to remove the surface scum; and the iron-removed aluminum liquid II was obtained.

[0086] In this embodiment 2, the obtained aluminum liquid II after iron removal is poured to obtain the corresponding aluminum alloy II after iron removal. It can be understood that the pouring temperature is the insulation and standing temperature of the aluminum liquid C.

[0087] In this Example 1, the aluminum liquid C is kept at 630°C, 680°C and 720°C for 30 minutes, respectively, to obtain deironized aluminum liquid Ⅱ-1, deironized aluminum liquid Ⅱ-2 and deironized aluminum liquid Ⅱ-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring the deironized aluminum liquids at the corresponding holding temperatures are recorded as deironized aluminum alloy Ⅱ-1, deironized aluminum alloy Ⅱ-2 and deironized aluminum alloy Ⅱ-3, respectively.

[0088] In this Example 2, the original Fe content of the aluminum liquid A and the Fe content after iron removal in each aluminum liquid II after iron removal were detected, and the tensile strength and elongation of each iron-removed aluminum alloy II obtained by casting were detected, and the test results are shown in Table 2. Among them, the original Fe content of the aluminum liquid A is 0.55%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0089] Table 2

[0090]

[0091] It can be seen from Table 2 that when Mn:B=15:1, B:Be=1:1, the iron removal rate is between 42.8% and 55.6%. When the iron removal insulation temperature is 680℃, the iron removal rate is better.

[0092] Figure 4 This is the metallographic micrograph of the iron-removed aluminum alloy II-2 obtained in Example 2. It can be seen that the addition of excessive Mn promotes the change of the iron phase morphology, transforming the needle-shaped iron phase morphology into a Chinese character shape or hexagon.

[0093] Example 3

[0094] An aluminum alloy iron remover III comprises an aluminum-manganese alloy, an aluminum-boron alloy and an aluminum-beryllium alloy, wherein the mass ratio of manganese element to boron element is 10:1; and the mass ratio of boron element to beryllium element is 1:1.

[0095] The method for removing iron from aluminum alloy using the aluminum alloy iron remover III of Example 3 comprises:

[0096] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.52%.

[0097] The temperature of the aluminum liquid A is adjusted to 710°C, and then the aluminum alloy iron remover I is added to the aluminum liquid A to remove iron to obtain aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 1%, the mass percentage of boron element is 0.1%, and the mass percentage of beryllium element is 0.1%; that is, in the aluminum liquid B, the mass ratio of manganese element to iron element is 1.9:1, the mass ratio of boron element to iron element is 0.2:1, and the mass ratio of beryllium element to iron element is 0.2:1.

[0098] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added. After the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C;

[0099] The aluminum liquid C was kept at 630-720°C for 30 minutes, and then filtered to remove the surface scum; and the iron-removed aluminum liquid III was obtained.

[0100] In this embodiment 3, the obtained aluminum liquid III after iron removal is poured to obtain the corresponding aluminum alloy III after iron removal. It can be understood that the pouring temperature is the insulation and standing temperature of the aluminum liquid C.

[0101] In this Example 3, the aluminum liquid C is kept at 630°C, 680°C and 720°C for 30 minutes, respectively, to obtain deironized aluminum liquid III-1, deironized aluminum liquid III-2 and deironized aluminum liquid III-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring each deironized aluminum liquid at the corresponding holding temperature are recorded as deironized aluminum alloy III-1, deironized aluminum alloy III-2 and deironized aluminum alloy III-3, respectively.

[0102] In this embodiment 3, the original Fe content of the aluminum liquid A and the Fe content after iron removal in each aluminum liquid III after iron removal were detected, and the tensile strength and elongation of each iron-removed aluminum alloy III obtained by casting were detected, and the test results are shown in Table 3. Among them, the original Fe content of the aluminum liquid A is 0.52%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0103] It can be seen from Table 3 that when Mn:B=10:1, B:Be=1:1, the iron removal rate is between 41.2% and 53.1%. When the iron removal insulation temperature is 680℃, the iron removal rate is better and the iron removal effect is good; the tensile strength and elongation both reach the peak value, the tensile strength reaches 281MPa, and the elongation reaches 12.8%.

[0104] Table 3

[0105]

[0106] Example 4

[0107] An aluminum alloy iron remover IV comprises an aluminum-manganese alloy, an aluminum-boron alloy and an aluminum-beryllium alloy, wherein the mass ratio of manganese element to boron element is 2.5:1; the mass ratio of boron element to beryllium element is 1:1.

[0108] The method for removing iron from aluminum alloy using the aluminum alloy iron remover IV of Example 4 comprises:

[0109] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.52%.

[0110] The temperature of the aluminum liquid A is adjusted to 710°C, and then the aluminum alloy iron remover I is added to the aluminum liquid A to remove iron to obtain aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 1%, the mass percentage of boron element is 0.4%, and the mass percentage of beryllium element is 0.4%; that is, in the aluminum liquid B, the mass ratio of manganese element to iron element is 1.9:1, the mass ratio of boron element to iron element is 0.8:1, and the mass ratio of beryllium element to iron element is 0.8:1.

[0111] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added. After the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C;

[0112] The aluminum liquid C was kept at 630-720°C for 30 minutes, and then filtered to remove the surface scum; and the iron-removed aluminum liquid IV was obtained.

[0113] In this embodiment 4, the obtained aluminum liquid IV after iron removal is poured to obtain the corresponding aluminum alloy IV after iron removal. It can be understood that the pouring temperature is the insulation and standing temperature of the aluminum liquid C.

[0114] In this Example 4, the aluminum liquid C is kept at 630°C, 680°C and 720°C for 30 minutes, respectively, to obtain deironized aluminum liquid IV-1, deironized aluminum liquid IV-2 and deironized aluminum liquid IV-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring the deironized aluminum liquids at the corresponding holding temperatures are recorded as deironized aluminum alloy IV-1, deironized aluminum alloy IV-2 and deironized aluminum alloy IV-3, respectively.

[0115] In this Example 4, the original Fe content of the aluminum liquid A and the Fe content after iron removal in each aluminum liquid IV after iron removal were detected, and the tensile strength and elongation of each iron-removed aluminum alloy IV obtained by casting were detected, and the test results are shown in Table 4. Among them, the original Fe content of the aluminum liquid A is 0.52%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0116] Table 4

[0117]

[0118] It can be seen from Table 4 that when Mn:B=2.5:1, B:Be=1:1, the iron removal rate is between 39.3% and 45.1%. When the iron removal insulation temperature is 680℃, the iron removal rate is better.

[0119] Comparative Example 1

[0120] Comparison of aluminum alloy iron removers I, including aluminum-manganese alloy and aluminum-boron alloy, in which the mass ratio of manganese element to boron element is 5:1.

[0121] The method for removing iron from aluminum alloy using the aluminum alloy iron remover of Comparative Example 1 is as follows:

[0122] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.54%.

[0123] The temperature of the aluminum liquid A is adjusted to 710° C., and then the aluminum alloy iron remover comparative I is added to the aluminum liquid A to remove iron, thereby obtaining aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 1%, and the mass percentage of boron element is 0.2%;

[0124] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added. After the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C;

[0125] The aluminum liquid C was kept at 630-720°C for 30 minutes and then filtered to remove the surface scum; the aluminum liquid comparison I after iron removal was obtained.

[0126] In this comparative example 1, the obtained aluminum liquid after iron removal comparative example I is poured to obtain the corresponding aluminum alloy comparative example I after iron removal. It can be understood that the pouring temperature is the insulation and standing temperature of the aluminum liquid C.

[0127] In this comparative example 1, the aluminum liquid C was kept at 630°C, 680°C and 720°C for 30 min, respectively, to obtain deironized aluminum liquid comparison Ⅰ-1, deironized aluminum liquid comparison Ⅰ-2 and deironized aluminum liquid comparison Ⅰ-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring the deironized aluminum liquids at the corresponding holding temperatures were recorded as deironized aluminum alloy comparison Ⅰ-1, deironized aluminum alloy comparison Ⅰ-2 and deironized aluminum alloy comparison Ⅰ-3, respectively.

[0128] In this comparative example 1, the original Fe content of aluminum liquid A and the Fe content after iron removal in each aluminum liquid comparison Ⅰ after iron removal were detected, and the tensile strength and elongation of each iron removal aluminum alloy comparison Ⅰ obtained by casting were detected, and the test results are shown in Table 5. Among them, the original Fe content of aluminum liquid A is 0.54%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0129] Table 5

[0130]

[0131] It can be seen from Table 5 that when Be element is not added, the iron removal rate is significantly reduced, and the tensile strength and elongation are also significantly reduced.

[0132] Comparative Example 2

[0133] Comparison of aluminum alloy iron removers II, including aluminum-boron alloy and aluminum-beryllium alloy, in which the mass ratio of boron element to beryllium element is 1:1.

[0134] The method for removing iron from aluminum alloy using the aluminum alloy iron remover of Comparative Example 2, Comparative Example II, comprises:

[0135] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.51%.

[0136] The temperature of the aluminum liquid A is adjusted to 710° C., and then the aluminum alloy iron remover comparative II is added to the aluminum liquid A to remove iron, thereby obtaining aluminum liquid B; wherein the mass percentage of boron element in the aluminum liquid B is 0.2%;

[0137] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added. After the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C;

[0138] The aluminum liquid C was kept at 630-720°C for 30 minutes and then filtered to remove the surface scum; the aluminum liquid comparison II after iron removal was obtained.

[0139] In this comparative example 2, the obtained aluminum liquid after iron removal comparative II is cast to obtain the corresponding aluminum alloy comparative II after iron removal. It can be understood that the casting temperature is the insulation and standing temperature of the aluminum liquid C.

[0140] In this comparative example 2, the aluminum liquid C was kept at 630°C, 680°C and 720°C for 30 min, respectively, to obtain deironized aluminum liquid comparison Ⅱ-1, deironized aluminum liquid comparison Ⅱ-2, and deironized aluminum liquid comparison Ⅱ-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring the deironized aluminum liquids at the corresponding holding temperatures were recorded as deironized aluminum alloy comparison Ⅱ-1, deironized aluminum alloy comparison Ⅱ-2, and deironized aluminum alloy comparison Ⅱ-3, respectively.

[0141] In this comparative example 2, the original Fe content of aluminum liquid A and the Fe content after iron removal in each aluminum liquid comparison II after iron removal were detected, and the tensile strength and elongation of each iron removal aluminum alloy comparison II obtained by casting were detected, and the test results are shown in Table 6. Among them, the original Fe content of aluminum liquid A is 0.51%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0142] Table 6

[0143]

[0144] It can be seen from Table 6 that when the iron remover only includes B element and Be element, the iron removal rate is significantly reduced, and the tensile strength and elongation are also significantly reduced.

[0145] Comparative Example 3

[0146] Comparison of aluminum alloy iron removers III, including aluminum-manganese alloy and aluminum-beryllium alloy, in which the mass ratio of manganese element to beryllium element is 5:1.

[0147] The method for removing iron from aluminum alloy using the aluminum alloy iron remover of Comparative Example 3 Comparative Example III comprises:

[0148] An aluminum-silicon alloy is placed in a crucible whose inner wall is coated with a coating, and heated to melt to obtain aluminum liquid A to be deironed; wherein the mass content of Fe element in the aluminum liquid A is 0.52%.

[0149] The temperature of the aluminum liquid A is adjusted to 710° C., and then the aluminum alloy iron remover comparative III is added to the aluminum liquid A to remove iron, thereby obtaining aluminum liquid B; wherein the mass percentage of boron element in the aluminum liquid B is 0.2%;

[0150] The temperature of aluminum liquid B was adjusted to 730°C, and then 0.5wt% Al-Si special refining agent was added. After the reaction was completed, the melt was stirred for 5 minutes to obtain aluminum liquid C;

[0151] The aluminum liquid C was kept at 630-720°C for 30 minutes and then filtered to remove the surface scum; the aluminum liquid comparison III after iron removal was obtained.

[0152] In this comparative example 3, the obtained iron-removed aluminum liquid comparative III is poured to obtain the corresponding iron-removed aluminum alloy comparative III. It can be understood that the pouring temperature is the heat preservation and standing temperature of the aluminum liquid C.

[0153] In this comparative example 3, the aluminum liquid C was kept at 630°C, 680°C and 720°C for 30 minutes, respectively, to obtain deironized aluminum liquid comparison III-1, deironized aluminum liquid comparison III-2 and deironized aluminum liquid comparison III-3, respectively. Accordingly, the deironized aluminum alloys obtained by pouring the deironized aluminum liquids at the corresponding holding temperatures were recorded as deironized aluminum alloy comparison III-1, deironized aluminum alloy comparison III-2 and deironized aluminum alloy comparison III-3, respectively.

[0154] In this comparative example 3, the original Fe content of aluminum liquid A and the Fe content after iron removal in each aluminum liquid comparison III after iron removal were detected, and the tensile strength and elongation of each iron removal aluminum alloy comparison III obtained by casting were detected, and the test results are shown in Table 7. Among them, the original Fe content of aluminum liquid A is 0.52%, and the iron removal rate = (original Fe content-Fe content after iron removal) / original Fe content × 100%.

[0155] Table 7

[0156]

[0157] It can be seen from Table 7 that when the iron remover only includes Mn and Be elements, the iron removal rate is significantly reduced, and the tensile strength and elongation are also significantly reduced.

[0158] In the embodiments of the present disclosure, the Fe content is detected by a SPECTRO spectrometer. The tensile strength of the aluminum alloy is obtained by a Zwick tensile machine test. The elongation of the aluminum alloy is obtained by a Zwick tensile machine and a 25 mm extensometer test.

[0159] In Examples 1 to 4 of the embodiments of the present disclosure, and Comparative Examples 1 to 3, the aluminum-manganese alloy uses an Al-10Mn master alloy, the aluminum-boron alloy uses an Al-5B master alloy, and the aluminum-beryllium alloy uses an Al-5Be master alloy. Of course, the embodiments of the present disclosure are not limited to the master alloys with the above specific proportions.

[0160] The present application is not limited to the structures that have been described above and shown in the drawings, and various modifications and changes may be made without departing from the scope thereof. The scope of the present application is limited only by the appended claims.

[0161] In the present application, each embodiment may focus on the differences from other embodiments, and the same or similar parts between the embodiments may refer to each other.

Claims

1. An aluminum alloy iron remover, characterized in that: It includes substances containing manganese, substances containing boron and substances containing beryllium, wherein the mass ratio of manganese to boron is (2:1) to (20:1); the mass ratio of boron to beryllium is (0.8:1) to (1.2:1).

2. The aluminum alloy iron remover according to claim 1, characterized in that: The mass ratio of manganese to boron is (2.5:1) to (15:1); and / or The mass ratio of boron to beryllium is 1:

1.

3. The aluminum alloy iron remover according to claim 1, characterized in that: Manganese-containing substances include elemental manganese and / or manganese-containing compounds; and / or The substance containing the boron element includes elemental boron and / or a boron-containing compound; and / or The substance containing beryllium element includes single substance beryllium and / or beryllium-containing compound.

4. The aluminum alloy iron remover according to claim 3, characterized in that: Manganese-containing compounds include aluminum-manganese alloys; and / or Boron-containing compounds include aluminum-boron alloys; and / or Beryllium-containing compounds include aluminum-beryllium alloys.

5. A method for removing iron from aluminum alloy, characterized in that: include: Obtaining aluminum liquid A to be deironed; The temperature of the aluminum liquid A is adjusted to 700-710° C., and then the aluminum alloy iron remover according to any one of claims 1 to 4 is added to the aluminum liquid A to remove iron, thereby obtaining an aluminum liquid B; wherein, in the aluminum liquid B, the mass percentage of manganese element is 0.1%-5%, the mass percentage of boron element is 0.05%-1.5%, and the mass percentage of beryllium element is 0.05%-1.5%; Refining the aluminum liquid B to obtain aluminum liquid C; The aluminum liquid C is kept at 630-720°C and then filtered.

6. The method for removing iron from aluminum alloy according to claim 5, characterized in that: In the aluminum liquid B, the mass ratio of manganese element to iron element is (0.1﹕1) to (6﹕1); and / or, the mass ratio of boron element to iron element is (0.05﹕1) to (1.5﹕1); and / or, the mass ratio of beryllium element to iron element is (0.05﹕1) to (1.5﹕1).

7. The method for removing iron from aluminum alloy according to claim 6, characterized in that: In the aluminum liquid B, the mass ratio of manganese element to iron element is (1.5﹕1) to (6﹕1); and / or, the mass ratio of boron element to iron element is (0.1﹕1) to (1﹕1); and / or, the mass ratio of beryllium element to iron element is (0.1﹕1) to (1﹕1).

8. The method for removing iron from aluminum alloy according to claim 5, characterized in that: The aluminum liquid B is subjected to a refining treatment, including: The temperature of the aluminum liquid B is controlled at 720-740° C., and an inert gas carrying a refining agent powder is introduced into the aluminum liquid B for powder spraying, refining and slag removal treatment.

9. The method for removing iron from aluminum alloy according to claim 8, characterized in that: The refining agent is a salt solvent that does not contain sodium ions; and / or The amount of refining agent added is 0.3% to 1.2% of the weight of the aluminum liquid B.

10. The method for removing iron from aluminum alloy according to claim 5, characterized in that: The aluminum liquid C is kept at 630-720° C. and allowed to stand for 20-60 minutes.

11. The method for removing iron from aluminum alloy according to claim 5, characterized in that: Before adding the aluminum alloy iron remover according to any one of claims 1 to 4 to the aluminum liquid A, the method further comprises: Preheat and dry the aluminum alloy iron remover.

12. An aluminum alloy, characterized in that: It is obtained by pouring the deironing aluminum liquid obtained by the aluminum alloy deironing method as described in any one of claims 5 to 11.