Preparation process of aluminum alloy material for sports equipment
By using graphene and nickel in aluminum alloy materials for sports equipment, melting and kneading of rare earth lanthanum and chemical conversion treatment, the corrosion resistance and mechanical properties of existing aluminum alloy materials are solved, and a higher level of Comprehensive performance and wider application scenarios.
Patent Information
- Application Number
- CN202411578680.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-11-07
AI Technical Summary
The existing aluminum alloy materials for sports equipment have insufficient corrosion resistance and mechanical properties, which are difficult to meet the increasingly diverse use occasions.
The graphene-aluminum intermediate alloy was prepared by pressure permeation process, and nickel elements were loaded through in-situ co-reduction method, combined with rare earth lanthanum and aluminum blocks to melt and mix, and then cast and mold, and finally chemical conversion was used. The treatment solution is chemically converted to produce an aluminum alloy material for sports equipment with excellent corrosion resistance and mechanical properties.
It significantly improves the corrosion resistance and mechanical properties of aluminum alloy materials, expands its application in sports equipment, and meets personalized and customized needs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloys, and in particular to a preparation process of an aluminum alloy material for sports equipment. Background Art
[0002] In recent years, people have paid more attention to health and sports activities, and the demand for sports equipment has grown and become more diversified. In addition to traditional fitness equipment, people's demand for outdoor sports equipment, team sports equipment and children's sports equipment is increasing, and personalized needs and customized products have thus occupied a place in the sports equipment market. With the advancement of technology and changes in user needs, sports equipment not only needs to meet basic functional requirements, but also needs to have higher performance and innovative design. The characteristics of metal materials, such as strength, durability, stability and plasticity, provide reliable structure and support for sports equipment.
[0003] Aluminum alloy is a material made of a mixture of aluminum and other alloying elements. Aluminum alloy has a lower density and is lighter than other metal materials. Therefore, aluminum alloy equipment is easier to carry and operate. Aluminum alloy also has good processing properties and can be processed into various shapes and structures through a variety of processes such as extrusion, casting, and welding to meet the design requirements of different sports equipment. When aluminum alloy is used as sports equipment, it also has defects such as easy corrosion and insufficient strength, which makes it difficult to meet the increasingly diverse use occasions of sports equipment. Therefore, a preparation process for aluminum alloy materials for sports equipment is proposed. The aluminum alloy material prepared by this process has excellent corrosion resistance and mechanical properties, which greatly improves the comprehensive performance of aluminum alloys and expands the use occasions of aluminum alloys as sports equipment. It has great prospects and value. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation process of aluminum alloy material for sports equipment to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A preparation process of an aluminum alloy material for sports equipment, the preparation process of the aluminum alloy material for sports equipment comprising: preparing a graphene-aluminum master alloy by a pressure infiltration process with nickel-plated graphene and aluminum powder; casting and molding A380 aluminum alloy, graphene-aluminum master alloy, and rare earth-aluminum master alloy to prepare a modified aluminum alloy; and chemically converting the modified aluminum alloy with a chemical conversion treatment liquid to prepare the aluminum alloy material for sports equipment; The nickel-plated graphene is prepared by loading nickel onto graphene oxide through an in-situ co-reduction method; The rare earth-aluminum master alloy is prepared by melting and mixing rare earth lanthanum and aluminum blocks; The chemical conversion treatment liquid is prepared by mixing acrylamide, sodium silicate, an oxidizing agent and a reducing agent; The oxidant is one of potassium persulfate and ammonium persulfate; The reducing agent is one of sodium sulfite, sodium bisulfite and ammonium ferrous sulfate.
[0006] As an optimization, the preparation process of the aluminum alloy material for sports equipment includes the following preparation steps: (1) The mixed reaction liquid was stirred at 80-90°C and 300-500 r / min. The pH value of the mixed solution was tested with pH test paper every 5 minutes, and ammonia water was added to stabilize the pH value of the mixed solution at 9-10. After 15 minutes, no more ammonia water was added. After stirring for 30 minutes, heating was stopped, and the mixture was cooled to room temperature, filtered, and washed with deionized water for 3-5 times. Under vacuum conditions, it was dried at 50-60°C for 10-12 hours, placed in a ball mill, and spun at 500- The nickel-plated graphene was obtained by ball milling at 600 rpm for 20 to 24 hours; the nickel-plated graphene and aluminum powder were mixed evenly at a mass ratio of 1: (20 to 30), placed in a powder mixer, stirred and mixed at 300 to 500 r / min for 14 to 16 hours, cold-pressed at 10 to 20 MPa, placed in a high-temperature electric furnace, kept at 600 to 700° C. for 4 to 6 hours, poured at 700 to 800° C., kept at pressure for 10 to 20 minutes, and demolded to obtain a graphene-aluminum intermediate alloy; (2) Under argon protection, the A380 aluminum alloy is placed in a graphite crucible and heated to 730-750°C. After the A380 aluminum alloy is completely melted, 0.2-0.3 times the mass of the A380 aluminum alloy is added with a graphene-aluminum master alloy and 0.06-0.07 times the mass of the A380 aluminum alloy is added. The mixture is stirred at 730-750°C and 300-500 r / min for 30-40 min and kept warm for 50-60 min. The melt temperature is lowered to 690-710°C. The melt is refined and deslagging is performed, and then poured into a metal mold to obtain a modified aluminum alloy. (3) The modified aluminum alloy is immersed in a chemical conversion treatment solution, ultrasonically shaken at 70-80°C for 30-36 hours, taken out, washed with anhydrous ethanol and deionized water for 3-5 times respectively, and dried at 50-60°C for 10-12 hours under vacuum conditions to obtain an aluminum alloy material for sports equipment.
[0007] As an optimization, the preparation method of the mixed reaction liquid in step (1) is: nickel sulfate, trisodium citrate hexahydrate, ammonium chloride, sodium hypophosphite, and deionized water are uniformly mixed in a mass ratio of 1:(2.5~2.6):(1.5~1.6):(0.5~0.6):(20~30), a graphene aqueous solution with a mass of 4~5 times that of nickel sulfate is added, and the pH is adjusted to 9~10 with ammonia water to obtain a mixed reaction liquid.
[0008] As an optimization, the preparation method of the graphene aqueous solution is: graphene oxide and deionized water are evenly mixed in a mass ratio of 1:(20~30), and ultrasonically dispersed for 1~2h to obtain a graphene aqueous solution.
[0009] As an optimization, the preparation method of the rare earth-aluminum master alloy in step (2) is as follows: rare earth lanthanum and aluminum block are mixed in a mass ratio of 1:(10-12), the temperature is raised to 730-750°C to melt the rare earth lanthanum and the aluminum block, the mixture is stirred at 730-750°C and 300-500 r / min for 20-30 min, and the mixture is kept warm for 50-60 min, the temperature of the melt is reduced to 690-710°C, the melt is refined and deslagging is performed, the melt is poured into a metal mold, and the mixture is cooled to room temperature to obtain a rare earth-aluminum master alloy.
[0010] As an optimization, the preparation method of the chemical conversion treatment liquid in step (3) is: under nitrogen protection, acrylamide, oxidant, reductant, and deionized water are mixed uniformly in a mass ratio of 1: (0.03-0.05): (0.004-0.006): (90-100), and sodium silicate in an amount of 0.2-0.3 times the mass of acrylamide is added, and the mixture is mixed uniformly to obtain a chemical conversion treatment liquid.
[0011] As an optimization, the oxidant is one of potassium persulfate and ammonium persulfate.
[0012] As an optimization, the reducing agent is one of sodium sulfite, sodium bisulfite, and ammonium ferrous sulfate.
[0013] Compared with the prior art, the beneficial effects achieved by the present invention are: When preparing the aluminum alloy material for sports equipment, the present invention loads nickel onto graphene oxide through an in-situ co-reduction method to obtain nickel-plated graphene; the nickel-plated graphene and aluminum powder are subjected to a pressure infiltration process to obtain a graphene-aluminum master alloy; rare earth lanthanum and aluminum blocks are melted and mixed to obtain a rare earth-aluminum master alloy; A380 aluminum alloy, graphene-aluminum master alloy and rare earth-aluminum master alloy are cast to obtain a modified aluminum alloy; acrylamide, sodium silicate, an oxidant and a reducing agent are prepared into a chemical conversion treatment liquid; the modified aluminum alloy is subjected to chemical conversion treatment using the chemical conversion treatment liquid to obtain the aluminum alloy material for sports equipment.
[0014] First, nickel was loaded onto graphene oxide through an in-situ co-reduction method to obtain nickel-plated graphene; the nickel-plated graphene and aluminum powder were subjected to a pressure infiltration process to obtain a graphene-aluminum master alloy; graphene can strengthen aluminum alloy materials for sports equipment from three aspects: first, fine grain strengthening, the thermal expansion coefficient of graphene nanosheets is lower than that of the metal matrix, so the graphene nanosheets can effectively hinder the grain growth of the metal matrix; second, dislocation pinning, during the plastic deformation of aluminum alloy materials for sports equipment, graphite will pin dislocations at the grain boundaries, thereby hindering dislocation movement; third, load strengthening, during the plastic deformation of aluminum alloy materials for sports equipment, due to the special wrinkled structure of graphene, it can help the metal matrix bear a certain load. Part of the load, thereby improving the mechanical properties of aluminum alloy materials for sports equipment; although graphene has excellent strengthening effects on aluminum alloy materials in theory, a large number of research results show that there are problems such as weak interface bonding and non-wetting between graphene and metallic aluminum, resulting in low interface bonding between graphene and aluminum, and the strengthening effect of graphene cannot be fully exerted; nickel has a strong bonding force with graphene, therefore, the in-situ co-reduction method is used to load nickel on the surface of graphene, which can effectively improve the interface wettability between graphene and aluminum, and reduce the thermal expansion of the interface, thereby forming a stable interface bonding, giving full play to the strengthening effect of graphene on aluminum alloy, and giving aluminum alloy materials for sports equipment excellent mechanical properties.
[0015] Secondly, rare earth lanthanum and aluminum blocks are melted and mixed to obtain rare earth-aluminum master alloy; A380 aluminum alloy, graphene-aluminum master alloy, and rare earth-aluminum master alloy are cast to obtain modified aluminum alloy; A380 alloy is composed of α-A1, Si, β-Al 5 FeSi and Al 2 Cu is the main phase. Related studies have shown that the higher the Si content, the worse the corrosion resistance of the aluminum alloy material. During the corrosion process, the large-sized eutectic Si phase and β-Al in the A380 aluminum alloy 5 The FeSi phase will form a corrosion microbattery with the anode phase α-A1, and after corrosion, corrosion holes will be formed near the second phase. When the Si phase exists in the aluminum-silicon alloy matrix in the form of thick and long needles, it is not only not conducive to its mechanical properties, but also its larger area of the cathode phase will suffer more serious corrosion. The addition of rare earth lanthanum hinders the diffusion of elements (Si, Fe, etc.), and the long needle-shaped eutectic Si phase becomes short rods or granules. 5 The morphology and size of the FeSi phase also changed significantly, becoming a smaller, short rod-like shape. After adding rare earth lanthanum to the aluminum alloy, the average grain size decreased, reducing the occurrence of micro-galvanic corrosion and improving the corrosion resistance of aluminum alloy materials used in sports equipment. At the same time, the generated Al 11 La 3 Rare earth phases with high melting point and high strength further improve the mechanical properties of aluminum alloy materials used in sports equipment.
[0016] Finally, acrylamide, sodium silicate, an oxidant and a reductant are prepared into a chemical conversion treatment liquid; the modified aluminum alloy is subjected to chemical conversion treatment with the chemical conversion treatment liquid to obtain an aluminum alloy material for sports equipment; sodium silicate can form a precipitation film on the surface of the aluminum alloy, and polyacrylamide, as an organic matter, can be adsorbed on the surface of the aluminum alloy in the gaps of the precipitation film generated by sodium silicate to form an adsorption film, making the film layer denser; at the same time, polyacrylamide can also be coated on the surface of the sodium silicate precipitation film and wrap part of the sodium silicate that has not formed a film. When pitting corrosion causes the film layer to rupture, these sodium silicates can be released and precipitate with the metal cations enriched in the pitting pits, thereby playing a role of self-repair; the two different film-forming substances complement each other to generate a chemical conversion film with better corrosion resistance than single sodium silicate or acrylamide, showing better long-term corrosion resistance, and giving the aluminum alloy material for sports equipment excellent corrosion resistance. DETAILED DESCRIPTION
[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example
[0018] A preparation process of an aluminum alloy material for sports equipment, the preparation process of the aluminum alloy material for sports equipment comprising the following preparation steps: (1) Graphene oxide and deionized water were mixed at a mass ratio of 1:20, and ultrasonically dispersed for 1 hour to obtain a graphene aqueous solution; nickel sulfate, trisodium citrate hexahydrate, ammonium chloride, sodium hypophosphite, and deionized water were mixed at a mass ratio of 1:2.5:1.5:0.5:20, and the graphene aqueous solution with a mass ratio of 4 times that of nickel sulfate was added, and the pH was adjusted to 9 with ammonia water to obtain a mixed reaction solution; the mixed reaction solution was stirred at 80°C and 300 r / min, and the pH value of the mixed solution was detected with a pH test paper every 5 minutes, and ammonia water was added to stabilize the pH value of the mixed solution at 9. , after 15 minutes, no more ammonia water was added, and heating was stopped after stirring for 30 minutes. The mixture was cooled to room temperature, filtered, washed with deionized water for 3 times, dried at 50°C for 12 hours under vacuum conditions, placed in a ball mill, and ball-milled at 500rpm for 24 hours to obtain nickel-plated graphene; the nickel-plated graphene and aluminum powder were evenly mixed at a mass ratio of 1:20, placed in a powder mixer, stirred and mixed at 300r / min for 16 hours, cold-pressed at 10MPa, placed in a high-temperature electric furnace, kept warm at 600°C for 6 hours, cast at 700°C, kept under pressure for 10 minutes, and demolded to obtain a graphene-aluminum intermediate alloy; (2) Mixing rare earth lanthanum and aluminum block in a mass ratio of 1:10, heating to 730°C to melt the rare earth lanthanum and aluminum block, stirring at 730°C and 300 r / min for 30 minutes, and keeping warm for 60 minutes, reducing the melt temperature to 690°C, refining and deslagging the melt, pouring it into a metal mold, and cooling it to room temperature to obtain a rare earth-aluminum master alloy; placing A380 aluminum alloy in a graphite crucible under argon protection, heating to 730°C, after the A380 aluminum alloy is completely melted, adding 0.2 times the mass of the A380 aluminum alloy of graphene-aluminum master alloy and 0.06 times the mass of the A380 aluminum alloy of rare earth-aluminum master alloy, stirring at 730°C and 300 r / min for 40 minutes and keeping warm for 60 minutes, reducing the melt temperature to 690°C, refining and deslagging the melt, and pouring it into a metal mold to obtain a modified aluminum alloy; (3) Under nitrogen protection, acrylamide, potassium persulfate, sodium sulfite and deionized water are mixed in a mass ratio of 1:0.03:0.004:90, and sodium silicate with a mass of 0.2 times that of acrylamide is added and mixed to obtain a chemical conversion treatment solution; the modified aluminum alloy is immersed in the chemical conversion treatment solution, ultrasonically shaken at 70°C for 36 h, taken out, washed with anhydrous ethanol and deionized water for 3 times each, and dried at 50°C for 12 h under vacuum conditions to obtain an aluminum alloy material for sports equipment. Example
[0019] A preparation process of an aluminum alloy material for sports equipment, the preparation process of the aluminum alloy material for sports equipment comprising the following preparation steps: (1) Graphene oxide and deionized water were mixed at a mass ratio of 1:25, and ultrasonically dispersed for 1.5 hours to obtain a graphene aqueous solution; nickel sulfate, trisodium citrate hexahydrate, ammonium chloride, sodium hypophosphite, and deionized water were mixed at a mass ratio of 1:2.55:1.55:0.55:25, and 4.5 times the mass of nickel sulfate was added to the graphene aqueous solution, and the pH was adjusted to 9.5 with ammonia water to obtain a mixed reaction solution; the mixed reaction solution was stirred at 85°C and 400 r / min, and the pH value of the mixed solution was detected with a pH test paper every 5 minutes, and ammonia water was added to stabilize the pH value of the mixed solution. The temperature was set at 9.5, and no ammonia water was added after 15 minutes. After stirring for 30 minutes, the heating was stopped, the mixture was cooled to room temperature, filtered, washed with deionized water for 4 times, dried at 55°C for 11 hours under vacuum conditions, placed in a ball mill, and ball milled at 550 rpm for 22 hours to obtain nickel-plated graphene; the nickel-plated graphene and aluminum powder were evenly mixed at a mass ratio of 1:25, placed in a powder mixer, stirred and mixed at 400 r / min for 15 hours, cold-pressed at 15 MPa, placed in a high-temperature electric furnace, kept warm at 650°C for 5 hours, poured at 750°C, kept under pressure for 15 minutes, and demolded to obtain a graphene-aluminum intermediate alloy; (2) Mixing rare earth lanthanum and aluminum block in a mass ratio of 1:11, heating to 740°C to melt the rare earth lanthanum and aluminum block, stirring at 740°C and 400 r / min for 25 minutes, and keeping warm for 55 minutes, reducing the temperature of the melt to 700°C, refining and deslagging the melt, pouring it into a metal mold, and cooling it to room temperature to obtain a rare earth-aluminum master alloy; placing A380 aluminum alloy in a graphite crucible under argon protection, heating it to 740°C, after the A380 aluminum alloy is completely melted, adding 0.25 times the mass of the A380 aluminum alloy of graphene-aluminum master alloy and 0.065 times the mass of the A380 aluminum alloy of rare earth-aluminum master alloy, stirring at 740°C and 400 r / min for 35 minutes and keeping warm for 55 minutes, reducing the temperature of the melt to 700°C, refining and deslagging the melt, and pouring it into a metal mold to obtain a modified aluminum alloy; (3) Under nitrogen protection, acrylamide, potassium persulfate, sodium sulfite and deionized water are mixed in a mass ratio of 1:0.04:0.005:95, and sodium silicate with a mass of 0.25 times that of acrylamide is added and mixed to obtain a chemical conversion treatment liquid; the modified aluminum alloy is immersed in the chemical conversion treatment liquid, ultrasonically shaken at 75°C for 33 h, taken out, washed with anhydrous ethanol and deionized water for 4 times respectively, and dried at 55°C for 11 h under vacuum conditions to obtain an aluminum alloy material for sports equipment. Example
[0020] A preparation process of an aluminum alloy material for sports equipment, the preparation process of the aluminum alloy material for sports equipment comprising the following preparation steps: (1) Graphene oxide and deionized water were mixed at a mass ratio of 1:30, and ultrasonically dispersed for 2 hours to obtain a graphene aqueous solution; nickel sulfate, trisodium citrate hexahydrate, ammonium chloride, sodium hypophosphite, and deionized water were mixed at a mass ratio of 1:2.6:1.6:0.6:30, and the graphene aqueous solution with a mass ratio of 5 times that of nickel sulfate was added, and the pH was adjusted to 10 with ammonia water to obtain a mixed reaction solution; the mixed reaction solution was stirred at 90°C and 500 r / min, and the pH value of the mixed solution was detected with a pH test paper every 5 minutes, and ammonia water was added to stabilize the pH value of the mixed solution at 1. After 0, 15min, no more ammonia water is added, heating is stopped after stirring for 30min, the mixture is cooled to room temperature, filtered, washed with deionized water for 5 times, dried at 60°C for 10h under vacuum conditions, placed in a ball mill, and ball milled at 600rpm for 20h to obtain nickel-plated graphene; the nickel-plated graphene and aluminum powder are evenly mixed at a mass ratio of 1:30, placed in a powder mixer, stirred and mixed at 500r / min for 14h, cold-pressed at 20MPa, placed in a high-temperature electric furnace, kept warm at 700°C for 4h, cast at 800°C, kept under pressure for 20min, and demolded to obtain a graphene-aluminum intermediate alloy; (2) Mixing rare earth lanthanum and aluminum block in a mass ratio of 1:12, heating to 750°C to melt the rare earth lanthanum and aluminum block, stirring at 750°C and 500 r / min for 20 minutes, and keeping warm for 50 minutes, reducing the temperature of the melt to 710°C, refining and deslagging the melt, pouring it into a metal mold, and cooling it to room temperature to obtain a rare earth-aluminum master alloy; placing A380 aluminum alloy in a graphite crucible under argon protection, heating to 750°C, after the A380 aluminum alloy is completely melted, adding 0.3 times the mass of the A380 aluminum alloy of graphene-aluminum master alloy and 0.07 times the mass of the A380 aluminum alloy of rare earth-aluminum master alloy, stirring at 750°C and 500 r / min for 30 minutes and keeping warm for 50 minutes, reducing the temperature of the melt to 710°C, refining and deslagging the melt, and pouring it into a metal mold to obtain a modified aluminum alloy; (3) Under nitrogen protection, acrylamide, potassium persulfate, sodium sulfite and deionized water were mixed in a mass ratio of 1:0.05:(0.006:100, and sodium silicate with a mass of 0.3 times that of acrylamide was added and mixed to obtain a chemical conversion treatment solution; the modified aluminum alloy was immersed in the chemical conversion treatment solution, ultrasonically vibrated at 80°C for 30 hours, taken out, washed with anhydrous ethanol and deionized water for 5 times respectively, and dried at 60°C for 10 hours under vacuum conditions to obtain an aluminum alloy material for sports equipment.
[0021] Comparative Example 1 The difference between the preparation process of the aluminum alloy material for sports equipment in Comparative Example 1 and Example 2 lies in the difference in step (1), where step (1) is modified as follows: graphene oxide and aluminum powder are mixed evenly at a mass ratio of 1:25, placed in a powder mixer, stirred and mixed at 400 r / min for 15 h, cold pressed at 15 MPa, placed in a high-temperature electric furnace, kept at 650° C. for 5 h, poured at 750° C., kept at pressure for 15 min, and demolded to obtain a graphene-aluminum intermediate alloy. The remaining steps are the same as in Example 2.
[0022] Comparative Example 2 The difference between the preparation process of the aluminum alloy material for sports equipment in Comparative Example 2 and Example 2 lies in the difference in step (2), which is modified as follows: under the protection of argon, the A380 aluminum alloy is placed in a graphite crucible and heated to 740° C. After the A380 aluminum alloy is completely melted, a graphene-aluminum master alloy with a mass of 0.25 times that of the A380 aluminum alloy is added, and the mixture is stirred at 740° C. and 400 r / min for 35 min and kept warm for 55 min, the melt temperature is reduced to 700° C., the melt is refined and deslagging, and poured into a metal mold to obtain a modified aluminum alloy. The remaining steps are the same as those in Example 2.
[0023] Comparative Example 3 The preparation process of the aluminum alloy material for sports equipment in Comparative Example 3 is different from that in Example 2 in that step (3) is not performed, and step (2) is modified as follows: rare earth lanthanum and aluminum block are mixed in a mass ratio of 1:11, the temperature is raised to 740°C to melt the rare earth lanthanum and aluminum block, stirred at 740°C and 400 r / min for 25 minutes, and kept warm for 55 minutes, the melt temperature is lowered to 700°C, the melt is refined and deslagging is performed, poured into a metal mold, and cooled to room temperature to obtain a rare earth-aluminum master alloy; in argon Under the protection of gas, the A380 aluminum alloy is placed in a graphite crucible and heated to 740°C. After the A380 aluminum alloy is completely melted, 0.25 times the mass of the A380 aluminum alloy is added with a graphene-aluminum master alloy and 0.065 times the mass of the A380 aluminum alloy is added. The mixture is stirred at 740°C and 400r / min for 35min and kept warm for 55min. The melt temperature is reduced to 700°C, the melt is refined and deslagging, and poured into a metal mold to obtain an aluminum alloy material for sports equipment. The remaining steps are the same as those in Example 2.
[0024] Test Example 1 Mechanical properties testing Test method: The examples and comparative examples were prepared into standard specimens according to GB / T228, and the tensile strength of the examples and comparative examples was tested using a universal electronic tensile testing machine, with the tensile rate set to 0.05 mm / min. The results are shown in Table 1.
[0025] Table 1 Tensile strength (MPa) Tensile strength (MPa) Example 1 379.23 Comparative Example 1 244.17 Example 2 384.52 Comparative Example 2 257.83 Example 3 381.15 Comparative Example 3 375.92 From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be found that the aluminum alloy material for sports equipment prepared by the present invention has good mechanical properties.
[0026] By comparison, the tensile strength of Examples 1 to 3 is greater than that of Comparative Example 1, indicating that nickel-plated graphene is obtained by loading nickel onto graphene oxide through an in-situ co-reduction method; the graphene-aluminum intermediate alloy is obtained by pressure infiltration process using nickel-plated graphene and aluminum powder; graphene can strengthen the aluminum alloy material for sports equipment from three aspects: first, fine grain strengthening, the thermal expansion coefficient of graphene nanosheets is lower than that of the metal matrix, so the graphene nanosheets can effectively hinder the grain growth of the metal matrix; second, dislocation pinning, during the plastic deformation of the aluminum alloy material for sports equipment, graphite will pin the dislocations at the grain boundaries, thereby hindering the movement of dislocations; third, load strengthening, during the plastic deformation of the aluminum alloy material for sports equipment, due to the special wrinkles of graphene structure, which can help the metal matrix bear part of the load, thereby improving the mechanical properties of aluminum alloy materials for sports equipment; although graphene has excellent strengthening effects on aluminum alloy materials in theory, a large number of research results show that there are problems such as weak interface bonding and non-wetting between graphene and metal aluminum, resulting in low interface bonding between graphene and aluminum, and the strengthening effect of graphene cannot be fully exerted; nickel has a strong bonding force with graphene, therefore, the in-situ co-reduction method is used to load nickel on the surface of graphene, which can effectively improve the interface wettability between graphene and aluminum, and reduce the thermal expansion of the interface, thereby forming a stable interface bonding, giving full play to the strengthening effect of graphene on aluminum alloy, and giving aluminum alloy materials for sports equipment excellent mechanical properties.
[0027] By comparison, the tensile strength of Examples 1 to 3 is greater than that of Comparative Example 2, indicating that rare earth lanthanum and aluminum blocks are melted and mixed to obtain rare earth-aluminum master alloys; A380 aluminum alloy, graphene-aluminum master alloy, and rare earth-aluminum master alloy are cast to obtain modified aluminum alloys; A380 alloy is composed of α-A1, Si, β-Al 5 FeSi and Al 2 Cu is the main phase. The addition of rare earth lanthanum hinders the diffusion of elements (Si, Fe, etc.). The long needle-shaped eutectic Si phase becomes short rods or particles. 5 The morphology and size of FeSi phase also changed significantly, becoming smaller and shorter rods. After adding rare earth lanthanum to aluminum alloy, the average grain size decreased, and the generated Al 11 La 3 Rare earth phases with high melting point and high strength further improve the mechanical properties of aluminum alloy materials used in sports equipment.
[0028] Test Example 2 Corrosion resistance test Test method: The corrosion resistance of the embodiment and the comparative example was tested by electrochemical impedance spectroscopy. A Gamry Interface 1000 electrochemical workstation was used, with the embodiment and the comparative example as the working electrode and a working area of 1 cm 2 The platinum electrode was used as the counter electrode, and the saturated calomel electrode was used as the reference electrode. The open circuit potential was measured in a 3.5% NaCl solution using this three-electrode system. The test time was 1800s. After the open circuit potential stabilized, it indicated that the system reached a steady state. Then the electrochemical impedance was measured. The parameters were set to an amplitude of 10mV and a frequency range of 100kHz to 0.01Hz. The results are shown in Table 2.
[0029] Table 2
[0030] From the comparison of the experimental data of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 2, it can be found that the aluminum alloy material for sports equipment prepared by the present invention has good corrosion resistance.
[0031] By comparison, the charge transfer resistance of Examples 1 to 3 is greater than that of Comparative Example 2, indicating that rare earth lanthanum and aluminum blocks are melted and mixed to obtain rare earth-aluminum master alloys; A380 aluminum alloy, graphene-aluminum master alloy, and rare earth-aluminum master alloy are cast to obtain modified aluminum alloys; A380 alloy is composed of α-A1, Si, β-Al 5 FeSi and Al 2 Cu is the main phase. Related studies have shown that the higher the Si content, the worse the corrosion resistance of the aluminum alloy material. During the corrosion process, the large-sized eutectic Si phase and β-Al in the A380 aluminum alloy 5 The FeSi phase will form a corrosion microbattery with the anode phase α-A1, and after corrosion, corrosion holes will be formed near the second phase. When the Si phase exists in the aluminum-silicon alloy matrix in the form of thick and long needles, it is not only not conducive to its mechanical properties, but also its larger area of the cathode phase will suffer more serious corrosion. The addition of rare earth lanthanum hinders the diffusion of elements (Si, Fe, etc.), and the long needle-shaped eutectic Si phase becomes short rods or granules. 5 The morphology and size of the FeSi phase also changed significantly, becoming smaller and shorter rods; after adding rare earth lanthanum to the aluminum alloy, the average grain size decreased, reducing the occurrence of microgalvanic corrosion and improving the corrosion resistance of aluminum alloy materials used in sports equipment.
[0032] By comparison, the charge transfer resistance of Examples 1 to 3 is greater than that of Comparative Example 3, indicating that acrylamide, sodium silicate, an oxidant, and a reductant are prepared into a chemical conversion treatment liquid; the modified aluminum alloy is subjected to chemical conversion treatment with the chemical conversion treatment liquid to obtain an aluminum alloy material for sports equipment; sodium silicate can form a precipitation film on the surface of the aluminum alloy, and polyacrylamide, as an organic matter, can be adsorbed on the surface of the aluminum alloy in the gaps of the precipitation film generated by sodium silicate to form an adsorption film, making the film layer denser; at the same time, polyacrylamide can also be coated on the surface of the sodium silicate precipitation film and wrap part of the sodium silicate that has not formed a film. When pitting corrosion causes the film layer to rupture, these sodium silicates can be released and precipitate with the metal cations enriched in the pitting pits, thereby playing a self-repairing role; the two different film-forming substances complement each other to generate a chemical conversion film with better corrosion resistance than single sodium silicate or acrylamide, showing better long-term corrosion resistance, and giving the aluminum alloy material for sports equipment excellent corrosion resistance.
[0033] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A process for preparing an aluminum alloy material for sports equipment, characterized in that: The preparation process of the aluminum alloy material for sports equipment is to prepare a graphene-aluminum master alloy by a pressure infiltration process with nickel-plated graphene and aluminum powder; to prepare a modified aluminum alloy by casting A380 aluminum alloy, graphene-aluminum master alloy and rare earth-aluminum master alloy; to prepare an aluminum alloy material for sports equipment by chemical conversion treatment liquid; The nickel-plated graphene is prepared by loading nickel onto graphene oxide through an in-situ co-reduction method; The rare earth-aluminum master alloy is prepared by melting and mixing rare earth lanthanum and aluminum blocks; The chemical conversion treatment liquid is prepared by mixing acrylamide, sodium silicate, an oxidizing agent and a reducing agent; The oxidant is one of potassium persulfate and ammonium persulfate; The reducing agent is one of sodium sulfite, sodium bisulfite and ammonium ferrous sulfate; The preparation process of the aluminum alloy material for sports equipment comprises the following preparation steps: (1) The mixed reaction liquid was stirred at 80-90°C and 300-500 r / min. The pH value of the mixed solution was tested with pH test paper every 5 minutes, and ammonia water was added to stabilize the pH value of the mixed solution at 9-10. After 15 minutes, no more ammonia water was added. After stirring for 30 minutes, heating was stopped, and the mixture was cooled to room temperature, filtered, and washed with deionized water for 3-5 times. Under vacuum conditions, it was dried at 50-60°C for 10-12 hours, placed in a ball mill, and spun at 500- The nickel-plated graphene was obtained by ball milling at 600 rpm for 20 to 24 hours; the nickel-plated graphene and aluminum powder were mixed evenly at a mass ratio of 1: (20 to 30), placed in a powder mixer, stirred and mixed at 300 to 500 r / min for 14 to 16 hours, cold-pressed at 10 to 20 MPa, placed in a high-temperature electric furnace, kept at 600 to 700° C. for 4 to 6 hours, poured at 700 to 800° C., kept at pressure for 10 to 20 minutes, and demolded to obtain a graphene-aluminum intermediate alloy; (2) Under argon protection, the A380 aluminum alloy is placed in a graphite crucible and heated to 730-750°C. After the A380 aluminum alloy is completely melted, 0.2-0.3 times the mass of the A380 aluminum alloy is added with a graphene-aluminum master alloy and 0.06-0.07 times the mass of the A380 aluminum alloy is added. The mixture is stirred at 730-750°C and 300-500 r / min for 30-40 min and kept warm for 50-60 min. The melt temperature is lowered to 690-710°C. The melt is refined and deslagging is performed, and then poured into a metal mold to obtain a modified aluminum alloy. (3) The modified aluminum alloy is immersed in a chemical conversion treatment solution, ultrasonically shaken at 70-80°C for 30-36 hours, taken out, washed with anhydrous ethanol and deionized water for 3-5 times respectively, and dried at 50-60°C for 10-12 hours under vacuum conditions to obtain an aluminum alloy material for sports equipment.
2. The process for preparing an aluminum alloy material for sports equipment according to claim 1, characterized in that: The preparation method of the mixed reaction liquid in step (1) is as follows: nickel sulfate, trisodium citrate hexahydrate, ammonium chloride, sodium hypophosphite, and deionized water are uniformly mixed in a mass ratio of 1:(2.5~2.6):(1.5~1.6):(0.5~0.6):(20~30), a graphene aqueous solution with a mass of 4~5 times that of nickel sulfate is added, and the pH is adjusted to 9~10 with ammonia water to obtain a mixed reaction liquid.
3. The process for preparing an aluminum alloy material for sports equipment according to claim 2, characterized in that: The preparation method of the graphene aqueous solution is as follows: graphene oxide and deionized water are uniformly mixed in a mass ratio of 1:(20-30), and ultrasonically dispersed for 1-2 hours to obtain the graphene aqueous solution.
4. The process for preparing an aluminum alloy material for sports equipment according to claim 1, characterized in that: The preparation method of the rare earth-aluminum master alloy in step (2) is as follows: rare earth lanthanum and aluminum block are mixed in a mass ratio of 1:(10-12), the temperature is raised to 730-750°C to melt the rare earth lanthanum and the aluminum block, the mixture is stirred at 730-750°C and 300-500 r / min for 20-30 min, and the mixture is kept warm for 50-60 min, the temperature of the melt is reduced to 690-710°C, the melt is refined and deslagging is performed, the melt is poured into a metal mold, and the mixture is cooled to room temperature to obtain a rare earth-aluminum master alloy.
5. The process for preparing an aluminum alloy material for sports equipment according to claim 1, characterized in that: The preparation method of the chemical conversion treatment liquid in step (3) is as follows: under nitrogen protection, acrylamide, an oxidant, a reducing agent, and deionized water are mixed uniformly in a mass ratio of 1:(0.03-0.05):(0.004-0.006):(90-100), and sodium silicate in an amount of 0.2-0.3 times the mass of acrylamide is added, and the mixture is mixed uniformly to obtain a chemical conversion treatment liquid.
6. The process for preparing an aluminum alloy material for sports equipment according to claim 5, characterized in that: The oxidant is one of potassium persulfate and ammonium persulfate.
7. The process for preparing an aluminum alloy material for sports equipment according to claim 5, characterized in that: The reducing agent is one of sodium sulfite, sodium bisulfite and ammonium ferrous sulfate.
Citation Information
Patent Citations
Preparation method of graphene / aluminium composite
CN106702193A
Preparation method of nickel-plated graphene reinforced tin-based soldering paste
CN114952073A
High-strength foam aluminum alloy casting method
CN116083761A
Rare earth modified aluminum alloy and preparation method thereof
CN118389912A