Low-modulus, high-strength, high-deformability and high-beta-phase-content Ti-Ta alloy and preparation method thereof
A Ti-Ta alloy with high β-phase content and low modulus is prepared via ball milling and sintering, addressing segregation and mechanical weaknesses, resulting in uniform phase morphology and enhanced mechanical properties.
Patent Information
- Application Number
- CN202411181926.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Existing Ti-Ta alloys face issues of low strength, poor elongation, and segregation due to large density and melting point differences, leading to defects and high preparation costs, while traditional methods struggle to achieve a high β-phase content and low modulus.
A Ti-Ta alloy with a high β-phase content and low modulus is prepared through a method involving low-energy ball milling, spark plasma sintering, and quenching, ensuring uniform phase morphology and distribution, using specific particle sizes and purities of Ti and Ta powders, followed by solution treatment and quenching to enhance mechanical properties.
The resulting Ti-Ta alloy exhibits uniform phase morphology, low modulus, high strength, and high deformation capacity, overcoming segregation and achieving excellent mechanical properties.
Smart Images

Figure CN119082545A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of alloy materials, and specifically relates to a Ti-Ta alloy with a high β-phase content and low modulus, high strength and high deformation capacity. The present invention also relates to a preparation method of a Ti-Ta alloy with a high β-phase content and low modulus, high strength and high deformation capacity. Background Art
[0002] Titanium alloys have the advantages of high specific strength, good room temperature performance, good corrosion resistance, and good biocompatibility, and are widely used in the fields of biomedical metal materials. Initially, CP-Ti and Ti6Al4V were used to replace 316L stainless steel or Co-Cr alloys containing toxic elements Ni, Co, and Cr. However, further research found that when CP-Ti and Ti6Al4V are used as bone implant materials, there is a "stress shielding" phenomenon, that is, when the elastic modulus of the bone implant and the host bone is large, it is easy to cause damage to the host bone and implant failure. The elastic modulus of CP-Ti and Ti6Al4V are 110GPa and 120GPa respectively, while the elastic modulus of human compact bone is approximately 3 to 30GPa.
[0003] In addition, the study also found that although the comprehensive performance of Ti6Al4V is relatively good, it contains Al and V, which are harmful to the human body. Therefore, finding new alloys as biomedical materials has become a research hotspot. In contrast, β-titanium alloy contains almost no harmful elements. It not only has better biocompatibility but also can maintain a lower modulus while maintaining high strength. Among them, Ta, as a β-stabilizing element of β-titanium alloy, has more excellent corrosion resistance and better biocompatibility. When used as a solute element in titanium alloy, it can achieve infinite solid solution in β-Ti, retaining β-Ti with a lower elastic modulus to room temperature, and reducing the elastic modulus of titanium alloy while playing a role in solid solution strengthening.
[0004] At present, the process of preparing Ti-Ta alloy mainly adopts vacuum melting method. However, due to the large difference in melting point and density between Ti and Ta (the melting point of Ti is 1660℃, the melting point of Ta is 2996℃, and the density of Ti is 4.5g / cm 3 , the density of Ta is 16.6g / cm 3 ), which often leads to defects such as large segregation and pores in the alloy. In order to eliminate the above defects, more than 10 times of smelting are required, which will increase the preparation cost. The materials made by powder metallurgy process have the advantages of designable structure composition, fast sintering rate, high sintering temperature and high density, and are widely used.
[0005] Chinese invention patent CN 104342583 A discloses a method for preparing a Ti-Ta alloy with an inhomogeneous structure. The Ti-Ta alloy prepared by this method has obvious Ta-rich regions and Ta-rich regions in the structure due to insufficient diffusion time. This type of alloy has a low elastic modulus and a high tensile strength, but it has the problems of high porosity and low elongation; Chinese invention patent CN113750288A discloses a method for preparing a ceramic particle reinforced Ti-Ta based bone implant composite material. Although the material has a high strength, it introduces a large amount of ceramic reinforcement phase on the basis of the Ti-Ta alloy, resulting in a high elastic modulus of the composite material, which limits its application in the field of biological applications; Chinese patent CN 109732087 A discloses a Ti-Ta material with a gradient structure, which improves the problem of low interface bonding strength of metal-metal matrix composite materials, but its structure and performance have obvious anisotropy, and its use is relatively limited; Chinese invention patent CN 115109979 A published a preparation process of a Ti-Ta-Nb-Zr-Mo biomedical high entropy alloy, which has a high compressive yield strength, but has many added elements, difficult composition control, and many melting times, resulting in a high preparation cost. Zhou et al. prepared Ti-xTa alloy (x = 10 ~ 80wt.%) by vacuum melting. Their research shows that when the Ta content is 30 ~ 70wt.%, the alloy has good room temperature excellent performance (Zhou YL, Niinomi M, Akahori T, Effects of Ta content on Young's modulus and tensile properties of binary Ti-Ta alloys for biomedical applications, Materials Science and Engineering: A, 2004, 371 (1-2): 283-290,). Therefore, it is particularly important to prepare a Ti-Ta alloy with low elastic modulus, high strength and high plasticity. Summary of the invention
[0006] The purpose of the present invention is to provide a Ti-Ta alloy with a high β-phase content and low modulus, high strength and high deformation capacity, which solves the problem of low strength and poor elongation in biomedical titanium alloys due to low elastic modulus.
[0007] Another object of the present invention is to provide a method for preparing a Ti-Ta alloy with a low modulus, high strength, and high deformation capacity and a high β-phase content, thereby solving the problem that the traditional preparation method is prone to segregation and low β-phase content.
[0008] The first technical solution adopted by the present invention is: a high β-phase content Ti-Ta alloy with low modulus, high strength and high deformation capacity, which is composed of the following components by mass percentage: Ti 50-70%, Ta 30-50%, and the sum of the mass percentages of the above components is 100%.
[0009] The second technical solution adopted by the present invention is: a method for preparing a Ti-Ta alloy with a high β-phase content and low modulus, high strength and high deformation capacity, comprising the following steps:
[0010] Step 1, weigh the following components by mass percentage: 50-70% Ti powder, 30-50% Ta powder, the sum of the mass percentages of the above components is 100%, mix the Ti powder and the Ta powder, add a ball milling aid, perform low-energy ball milling to obtain a mixed slurry, and then vacuum dry the mixed slurry to obtain a Ti-Ta mixed powder;
[0011] Step 2, pre-pressing the Ti-Ta mixed powder obtained in step 1 in a mold, and then sintering and densifying the powder to obtain a Ti-Ta pre-alloyed block;
[0012] Step 3: Place the Ti-Ta pre-alloyed block obtained in step 2 into a tubular furnace for solution treatment in the β phase region, and then perform quenching treatment.
[0013] The second technical solution of the present invention is also characterized in that:
[0014] In step 1, the Ti powder is a spherical powder, the particle size distribution range is 50-150 μm, and the purity is ≥99.9%; the Ta powder is an irregular powder, the particle size distribution range is 3-5 μm, and the purity is ≥99.9%.
[0015] In step 1, the ball milling aid is anhydrous ethanol or isopropanol, the amount of the ball milling aid added during the low-energy ball milling process is 1-2 mL, the ball-to-material ratio is 5:1, the ball milling speed is 200-250 r / min, the ball milling time is 4 h, and the grinding balls are zirconium oxide.
[0016] In step 1, the vacuum drying is carried out at a drying temperature of 60° C. and a drying time of 4 h.
[0017] In step 2, spark plasma sintering is used for sintering densification treatment. The spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850-1400℃, the holding time is 20min, and the vacuum degree is maintained at ≤5Pa during the sintering process. After sintering, the furnace is cooled to room temperature.
[0018] In step 3, the heating rate in the solution treatment is 10°C / min, the solution temperature is 1400-1600°C, the holding time is 1-2h, and a protective gas is introduced during the solution treatment.
[0019] In step 3, after the holding time of the solution treatment process is completed, the temperature is lowered to above the β phase temperature point at a cooling rate of 5°C / min, and then quenching treatment is performed.
[0020] The beneficial effects of the present invention are as follows: the high β-phase content Ti-Ta alloy with low modulus, high strength and high deformation capacity and the preparation method thereof of the present invention, the high β-phase content Ti-Ta alloy has uniform phase morphology and organizational composition in microscopic terms, and has low modulus, high strength and high deformation capacity in mechanics; the preparation method can realize diversified regulation of alloy organization and performance by combining powder metallurgy with heat treatment, can make Ta evenly distributed in the alloy, and can realize uniform phase organization, avoid the occurrence of component segregation, and on this basis, quench and quickly cool to obtain a Ti-Ta alloy rich in a large amount of β phase or full β phase. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The optical metallographic micrograph, electron micrograph and elemental surface distribution diagram of the Ti-Ta alloy with uniform phase morphology and organizational composition prepared in Example 1 of the present invention;
[0022] Figure 2 The metallographic micrograph, electron micrograph and elemental surface distribution diagram of the Ti-Ta pre-alloyed block having obvious Ti-rich region and Ta-rich region prepared in Comparative Example 1 of the present invention;
[0023] Figure 3 The metallographic micrograph, electron micrograph and element surface distribution diagram of the Ti-Ta alloy with uniformly distributed microstructure components obtained in Comparative Example 2 of the present invention;
[0024] Figure 4 The tensile stress-strain curve and the compressive stress-strain curve of the materials obtained in Example 1, Comparative Example 1 and Comparative Example 2 of the present invention are shown;
[0025] Figure 5 It is the XRD spectrum characterizing the phases of the materials obtained in Example 1 and Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0026] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0027] The invention provides a Ti-Ta alloy with a high β-phase content and low modulus, high strength and high deformation capacity. The alloy is composed of the following components in mass percentage: 50-70wt.% of pure Ti powder and 30-50wt.% of pure Ta powder, the mass percentage sum of the above two components being 100%. After low-energy uniform mixing, a powder metallurgy process (spark plasma sintering or other hot pressing sintering) is used to prepare a Ti-Ta pre-alloy block with high density, and then a solid solution treatment is carried out in the β-phase region. The long-term mutual diffusion process in the solid solution treatment and the quenching and rapid cooling process are used to further homogenize the microstructure components of the alloy to obtain a Ti-Ta alloy with a large amount of or full β-phase microstructure. The alloy has the characteristics of homogenization in microstructure morphology and element distribution, and has the excellent performance of low modulus, high strength and high deformation capacity in mechanical properties.
[0028] The present invention also provides a method for preparing a Ti-Ta alloy with a high β-phase content and low modulus, high strength and high deformation capacity, which is specifically carried out according to the following steps:
[0029] Step 1: Weigh 50-70wt.% of pure Ti powder and 30-50wt.% of pure Ta powder according to mass percentage, and the sum of the mass percentages of the above components is 100%. Perform low-energy ball milling on the pure Ti powder and pure Ta powder, and the ball milling aid is anhydrous ethanol or isopropanol. After obtaining a mixed slurry, the mixed slurry is vacuum dried to obtain a uniformly mixed Ti and Ta mixed powder. Wherein: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during low-energy ball milling is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C and the drying time is 4h.
[0030] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and perform sintering and densification treatment by spark plasma sintering or other hot pressing sintering processes to obtain a pre-alloyed block with uniform macroscopic distribution of Ta powder and close combination with Ti powder particles. Wherein: the spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850~1400℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0031] Step 3: Place the Ti-Ta pre-alloyed block obtained in step 2 into a tubular furnace for homogenization treatment. Under the premise that the Ta particles are fully dissolved, a Ti-Ta alloy with homogenization in both macro and micro scales and rich in β phase is obtained after quenching, and the alloy has excellent mechanical properties of low modulus, high strength and high deformation capacity. Among them: the heating rate in the solution treatment is 10℃ / min, the solution temperature is 1400-1600℃, the holding time is 1-2h, argon is introduced as a protective gas during the heat treatment, and after the holding time is over, the temperature is reduced to 1000℃ (or above other β phase temperature points) at a cooling rate of 5℃ / min, and the sample is quickly placed in ice water for quenching.
[0032] Through the above-mentioned manner, the low modulus, high strength, high deformation capacity and high β-phase content Ti-Ta alloy of the present invention and the preparation method thereof, aiming at the problem that segregation is easily caused when traditionally preparing alloy components with large density differences and large melting point differences, a design idea of using powder metallurgy sintering combined with subsequent heat treatment regulation is proposed. The pre-prepared alloy component powder is used as the raw material, the raw material powder is evenly mixed through a suitable low-energy ball milling process, and then a rapid sintering process of spark plasma sintering (or other hot pressing sintering methods) is used to prepare a pre-alloy block with high density. Subsequently, the alloy structure and morphology can be regulated according to the required performance in combination with an appropriate heat treatment process. Through this preparation process combining powder metallurgy with heat treatment, diversified regulation of the alloy structure and performance can be achieved, so that the alloy is further homogenized in terms of structure composition. On this basis, a Ti-Ta alloy rich in a large amount of β phase or full β phase is obtained by quenching and rapid cooling, and a titanium alloy with low modulus, high strength and high elongation is obtained.
[0033] Comparative Example 1
[0034] As Comparative Example 1 of the present invention, a Ti-Ta pre-alloyed block having macro-uniform distribution of Ti powder particles and Ta powder particles and micro-uniform distribution of Ti-Ta powder particles is prepared by spark plasma sintering, which is specifically implemented according to the following steps:
[0035] Step 1: Weigh 50wt.% of pure Ti powder and 50wt.% of pure Ta powder respectively according to the mass percentage, and the sum of the mass percentages of the above components is 100%. The pure Ti powder and pure Ta powder are subjected to low-energy ball milling, and the ball milling aid is anhydrous ethanol. After obtaining a mixed slurry, the mixed slurry is vacuum dried to obtain a uniformly mixed Ti and Ta mixed powder. Among them: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during the low-energy ball milling process is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C and the drying time is 4h.
[0036] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and use spark plasma sintering to perform sintering and densification treatment to obtain a pre-alloyed block in which the Ta powder is evenly distributed macroscopically and tightly combined with the Ti powder particles. Wherein: the spark plasma sintering pressure in step 2 is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850~1400℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0037] Comparative Example 2
[0038] As Comparative Example 2 of the present invention, a Ti-Ta alloy having uniform alloy composition and a large amount of martensite phase is prepared by spark plasma sintering combined with heat treatment, which is specifically implemented according to the following steps:
[0039] Step 1: Weigh 50wt.% of pure Ti powder and 50wt.% of pure Ta powder according to mass percentage, and the sum of the mass percentages of the above components is 100%. Perform low-energy ball milling on the pure Ti powder and pure Ta powder, and the ball milling aid is anhydrous ethanol or isopropanol. After obtaining a mixed slurry, the mixed slurry is vacuum dried to obtain a uniformly mixed Ti and Ta mixed powder. Wherein: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during the low-energy ball milling process is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C and the drying time is 4h.
[0040] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and use spark plasma sintering to perform sintering and densification treatment to obtain a pre-alloyed block with uniform macroscopic distribution of Ta powder and close combination with Ti powder particles. The spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850~1400℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0041] Step 3: Put the Ti-Ta alloy obtained in step 2 into a tubular furnace for homogenization treatment. Under the premise that the Ta particles are fully dissolved, cool it to room temperature in the furnace to obtain a Ti-Ta alloy that is homogenized in both macro and micro scales. The heating rate in the solution treatment is 10°C / min, the solution temperature is 1600°C, the holding time is 1h, argon is introduced as a protective gas during the heat treatment, and the cooling rate in the furnace is 5°C / min.
[0042] Example 1
[0043] The preparation method of the low modulus, high strength, high deformation capacity and high β-phase content Ti-Ta alloy of the present invention is specifically implemented according to the following steps:
[0044] Step 1: Weigh 50wt.% of pure Ti powder and 50wt.% of pure Ta powder according to mass percentage, and the sum of the mass percentages of the above components is 100%. Perform low-energy ball milling on the pure Ti powder and pure Ta powder, and use anhydrous ethanol as a ball milling aid to obtain a mixed slurry, and then vacuum dry the mixed slurry to obtain a uniformly mixed Ti and Ta mixed powder. Wherein: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during low-energy ball milling is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C, and the drying time is 4h.
[0045] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and use spark plasma sintering to perform sintering and densification treatment to obtain a pre-alloyed block with uniform macroscopic distribution of Ta powder and close combination with Ti powder particles. Wherein: the spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0046] Step 3: Put the Ti-Ta alloy obtained in step 2 into a tubular furnace for homogenization treatment. Under the premise that the Ta particles are fully dissolved, after quenching, a Ti-Ta alloy with homogenization in both macro and micro scales and rich in β phase is obtained, and the alloy has excellent mechanical properties of low modulus, high strength and high deformation capacity. Among them: the heating rate in the solution treatment is 10℃ / min, the solution temperature is 1600℃, the holding time is 1h, and argon is introduced as a protective gas during the heat treatment. To ensure the safety of the operation, the temperature is reduced to 1000℃ (or above other β phase temperature points) at a cooling rate of 5℃ / min after the holding time is over, and the sample is quickly placed in ice water for quenching.
[0047] Example 2
[0048] The preparation method of the low modulus, high strength, high deformation capacity and high β-phase content Ti-Ta alloy of the present invention is specifically implemented according to the following steps:
[0049] Step 1: Weigh 50wt.% of pure Ti powder and 50wt.% of pure Ta powder according to mass percentage, and the sum of the mass percentages of the above components is 100%. Perform low-energy ball milling on the pure Ti powder and pure Ta powder, and use anhydrous ethanol as a ball milling aid to obtain a mixed slurry, and then vacuum dry the mixed slurry to obtain a uniformly mixed Ti and Ta mixed powder. Wherein: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during low-energy ball milling is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C, and the drying time is 4h.
[0050] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and use spark plasma sintering to perform sintering densification treatment to obtain a Ti-Ta alloy containing a large amount of martensite phase and uniform composition and structure. Wherein: the spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 1400℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0051] Step 3: Place the Ti-Ta alloy obtained in step 2 into a tube furnace for solution treatment, and after quenching, obtain a Ti-Ta alloy that is homogenized in both macro and micro scales and rich in β phase, and the alloy has excellent mechanical properties of low modulus, high strength and high deformation capacity. Wherein: the heating rate in the solution treatment is 10℃ / min, the solution temperature is 1500℃, the holding time is 1.5h, argon is introduced as a protective gas during the heat treatment, and after the holding time is over, the sample is quickly placed in ice water for quenching.
[0052] Example 3
[0053] The preparation method of the low modulus, high strength, high deformation capacity and high β-phase content Ti-Ta alloy of the present invention is specifically implemented according to the following steps:
[0054] Step 1: According to the mass percentage, 70wt.% of pure Ti powder and 30wt.% of pure Ta powder are weighed respectively, and the sum of the mass percentages of the above components is 100%. The pure Ti powder and pure Ta powder are subjected to low-energy ball milling, and the ball milling aid is anhydrous ethanol. After obtaining a mixed slurry, the mixed slurry is vacuum dried to obtain a uniformly mixed Ti and Ta mixed powder. Among them: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during the low-energy ball milling process is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C and the drying time is 4h.
[0055] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and use spark plasma sintering to perform sintering and densification treatment to obtain a pre-alloyed block with uniform macroscopic distribution of Ta powder and close combination with Ti powder particles. Wherein: the spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0056] Step 3: Put the Ti-Ta alloy obtained in step 2 into a tubular furnace for homogenization treatment. Under the premise that the Ta particles are fully dissolved, after quenching, a Ti-Ta alloy with homogenization in both macro and micro scales and rich in β phase is obtained, and the alloy has excellent mechanical properties of low modulus, high strength and high deformation capacity. Among them: the heating rate in the solution treatment is 10℃ / min, the solution temperature is 1400℃, the holding time is 2h, and argon is introduced as a protective gas during the heat treatment. To ensure the safety of the operation, the temperature is reduced to 1000℃ (or above other β phase temperature points) at a cooling rate of 5℃ / min after the holding time is over, and the sample is quickly placed in ice water for quenching.
[0057] Example 4
[0058] The preparation method of the low modulus, high strength, high deformation capacity and high β-phase content Ti-Ta alloy of the present invention is specifically implemented according to the following steps:
[0059] Step 1: Weigh 60wt.% of pure Ti powder and 40wt.% of pure Ta powder respectively according to the mass percentage, and the sum of the mass percentages of the above components is 100%. The pure Ti powder and pure Ta powder are subjected to low-energy ball milling, and the ball milling aid is anhydrous ethanol. After obtaining a mixed slurry, the mixed slurry is vacuum dried to obtain a uniformly mixed Ti and Ta mixed powder. Among them: the pure Ti powder is a spherical powder, the powder particle size distribution range is 50-150μm, and the purity is ≥99.9%; the pure Ta powder is an irregular powder, the powder particle size distribution range is 3-5μm, and the purity is ≥99.9%; the amount of ball milling aid added during the low-energy ball milling process is 1-2mL, the ball-to-material ratio is 5:1, and the ball milling speed is 200-250r / min; the ball milling time is 4h, and the grinding ball is zirconium oxide; the drying temperature during vacuum drying is 60°C and the drying time is 4h.
[0060] Step 2: Pre-press the mixed powder obtained in step 1 into a graphite mold, and perform sintering and densification treatment by vacuum hot pressing to obtain a pre-alloyed block with uniform macroscopic distribution of Ta powder and close combination with Ti powder particles. Wherein: the sintering pressure in hot pressing sintering is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 1000℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
[0061] Step 3: Put the Ti-Ta alloy obtained in step 2 into a tubular furnace for homogenization treatment. Under the premise that the Ta particles are fully dissolved, after quenching, a Ti-Ta alloy with homogenization in both macro and micro scales and rich in β phase is obtained, and the alloy has excellent mechanical properties of low modulus, high strength and high deformation capacity. Among them: the heating rate in the solution treatment is 10℃ / min, the solution temperature is 1600℃, the holding time is 1h, and argon is introduced as a protective gas during the heat treatment. To ensure the safety of the operation, the temperature is reduced to 1000℃ (or above other β phase temperature points) at a cooling rate of 5℃ / min after the holding time is over, and the sample is quickly placed in ice water for quenching.
[0062] Results Analysis
[0063] 1) Figure 1 (a) Figure 1 (b) Figure 1 (c) Figure 1 (d) are respectively an optical metallographic micrograph, an electron micrograph, a Ti element surface distribution diagram and a Ta element surface distribution diagram of the Ti-Ta alloy with uniform phase morphology and structural composition obtained in Example 1. Figure 1 It can be seen that Ta is completely dissolved in Ti, the Ti-Ta alloy material has uniform composition, the phase structure is almost composed of all β-Ti, contains a small amount of α" martensite phase, and its distribution is uniform.
[0064] 2) Figure 2 (a) Figure 2 (b) Figure 2 (c) Figure 2 (d) Metallographic micrograph, electron micrograph, Ti element surface distribution diagram and Ta element surface distribution diagram of the Ti-Ta pre-alloyed block with obvious Ti-rich region and Ta-rich region obtained in Comparative Example 1. Figure 2 It can be seen that there is a short diffusion layer between the Ti-rich area and the Ta-rich area. This is because at a lower sintering temperature, the mutual diffusion distance between Ti and Ta is very limited. However, this preparation process can ensure that the Ti and Ta particles maintain good metallurgical bonding and have a higher density.
[0065] 3) Figure 3 (a) Figure 3 (b) Figure 3 (c) Figure 3 (d) are respectively a metallographic micrograph, an electron micrograph, a Ti element surface distribution diagram and a Ta element surface distribution diagram of a Ti-Ta alloy with uniformly distributed microstructure obtained in Comparative Example 2. Figure 3It can be seen that the alloy has high uniformity of phase structure and composition. Since Ta is an isomorphous β-stabilizing element of β-Ti, its stabilizing ability for β phase is weak, and the cooling method of furnace cooling cannot effectively keep a large amount of β phase at room temperature. In addition, because a large amount of Ta added is completely dissolved in Ti, it can prevent the transformation of β-Ti to α-Ti to a certain extent, making the alloy composed of an intermediate martensite phase.
[0066] 4) The titanium alloy-based composite material with micro-structure of the present invention has excellent mechanical properties and can have high strength and high deformation capacity while having a relatively low modulus. Figure 4 (a) Figure 4 (b) are the tensile stress-strain curves of the materials obtained in Example 1 and Comparative Example 1, and the compressive stress-strain curves of the materials obtained in Example 1 and Comparative Example 2. By comparison, it can be seen that the maximum tensile strength of the Ti-Ta alloy with uniform structure and containing a large amount of β phase is 1072MPa, and the elongation is 12%. However, the macro-uniform and micro-inhomogeneous Ti-Ta pre-alloyed block has a low sintering temperature, a short Ti-Ta diffusion distance, and a limited degree of metallurgical bonding, so its strength and elongation are both low. By performing room temperature compression tests on Example 1 and Comparative Example 2, it can be seen that due to the large amount of needle-shaped martensite phase contained in Comparative Example 2, the material has a high compressive yield strength but poor plasticity, which is manifested as a low material compression rate. And Example 1, which is subjected to rapid cooling after homogenization treatment, has a more excellent compression rate without losing too much strength. This is because more β phases with better plastic deformation ability are retained in the Ti-Ta alloy after quenching, resulting in the alloy obtained in Example 1 having a better compression rate.
[0067] 5) Figure 5 The results of the physical characterization of Example 1 and Comparative Example 1. Due to the short sintering time in Comparative Example 1, the diffusion of Ti and Ta is not sufficient, and the structure in the pre-alloyed block is mainly composed of α phase and pure Ta phase. Compared with Comparative Example 1, the Ti and Ta in Example 1 achieve a uniform mutual diffusion process, and the rapid cooling technology can retain all β phases to room temperature.
[0068] Table 1 Comparison of elastic modulus of commercial TC4, comparative example and embodiment
[0069] TC4 Comparative Example 2 Example 1 Elastic modulus / GPa 120 115(±2) 94(±5)
[0070] 6) Table 1 is a comparison of the elastic moduli of commercial TC4, comparative example 2 and embodiment 1. The elastic modulus of each phase structure of the titanium alloy is ranked from high to low as follows: w>α>α'>α">β. The elastic modulus of comparative example 2 in the present invention is similar to that of TC4, while in embodiment 1, thanks to the sufficient diffusion of Ti and Ta and the rapid cooling process, a large amount of β phase is retained at room temperature, and the elastic modulus of the material is reduced.
Claims
1. A high β-phase content Ti-Ta alloy with low modulus, high strength and high deformation capacity, characterized in that: It consists of the following components by mass percentage: Ti 50-70%, Ta 30-50%, and the sum of the mass percentages of the above components is 100%.
2. The method for preparing a Ti-Ta alloy with a low modulus, high strength, high deformation capacity and high β-phase content according to claim 1, characterized in that: The following steps are involved: Step 1, weigh the following components by mass percentage: 50-70% Ti powder, 30-50% Ta powder, the sum of the mass percentages of the above components is 100%, mix the Ti powder and the Ta powder, add a ball milling aid, perform low-energy ball milling to obtain a mixed slurry, and then vacuum dry the mixed slurry to obtain a Ti-Ta mixed powder; Step 2, pre-pressing the Ti-Ta mixed powder obtained in step 1 in a mold, and then sintering and densifying the powder to obtain a Ti-Ta pre-alloyed block; Step 3: Place the Ti-Ta pre-alloyed block obtained in step 2 into a tubular furnace for solution treatment in the β phase region, and then perform quenching treatment.
3. The method for preparing a Ti-Ta alloy with a low modulus, high strength, high deformation capacity and high β-phase content as claimed in claim 2, characterized in that: In the step 1, the Ti powder is a spherical powder, the particle size distribution range is 50-150 μm, and the purity is ≥99.9%; the Ta powder is an irregular powder, the particle size distribution range is 3-5 μm, and the purity is ≥99.9%.
4. The method for preparing a Ti-Ta alloy with a low modulus, high strength, high deformation capacity and high β-phase content as claimed in claim 2, characterized in that: In the step 1, the ball milling aid is anhydrous ethanol or isopropanol, the amount of the ball milling aid added during the low-energy ball milling process is 1-2 mL, the ball-to-material ratio is 5:1, the ball milling speed is 200-250 r / min, the ball milling time is 4 h, and the grinding balls are zirconium oxide.
5. The method for preparing a Ti-Ta alloy with a low modulus, high strength, high deformation capacity and high β-phase content as claimed in claim 2, characterized in that: In the step 1, the vacuum drying temperature is 60° C. and the drying time is 4 hours.
6. The method for preparing a Ti-Ta alloy with a low modulus, high strength, high deformation capacity and high β-phase content as claimed in claim 2, characterized in that: In the step 2, spark plasma sintering is used for sintering densification treatment, the spark plasma sintering pressure is 30MPa, the heating rate is 50℃ / min, the sintering temperature is 850-1400℃, the holding time is 20min, the vacuum degree is maintained at ≤5Pa during the sintering process, and the furnace is cooled to room temperature after sintering.
7. The method for preparing a Ti-Ta alloy with a high β-phase content and low modulus, high strength, and high deformation capacity as claimed in claim 2, characterized in that: In step 3, the heating rate in the solution treatment is 10° C. / min, the solution temperature is 1400-1600° C., the holding time is 1-2 h, and a protective gas is introduced during the solution treatment.
8. The method for preparing a Ti-Ta alloy with a low modulus, high strength, high deformation capacity and high β-phase content as claimed in claim 7, characterized in that: In the step 3, after the holding time of the solution treatment process is completed, the temperature is lowered to above the temperature point of the β phase region at a cooling rate of 5°C / min, and then quenching treatment is performed.
Citation Information
Patent Citations
Method for preparing titanium niobium tantalum zirconium biomedical titanium alloys by discharge plasma sintering
CN102312128A
Ti-Ta alloy as well as preparation method and application thereof
CN104342583A
Titanium-tantalum alloy plate with negative thermal expansion characteristic and preparation method thereof
CN112322935A
TiTaMg alloy and preparation method and application thereof
CN113444917A
Spherical tantalum-titanium alloy powder, product containing same and method of making same
CN114207167A