Corrosion-resistant high-entropy alloy coating and preparation method thereof
Through the ball milling and laser cladding process of equiatomic ratio Co, Fe, Mo, Ni, V high-entropy alloys, a single-phase body-center cubic structure coating with high hardness and high corrosion resistance was prepared, which solved the single performance of traditional coating materials. and the problem of defects in high entropy alloy coatings achieve good corrosion resistance and high hardness in complex environments.
Patent Information
- Application Number
- CN202410980512.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional coating materials cannot have the comprehensive properties of wear resistance, corrosion resistance, high temperature resistance, high strength and toughness, and cannot adapt to complex working environments. They are prone to defects of pores, cracks and uneven tissue when preparing high-entropy alloy coatings. .
Co, Fe, Mo, Ni, V high-entropy alloys with equal atomic ratio were mixed by ball mill and stirred with ethyl cellulose ethanol solution, coated on the surface of the substrate, and laser cladding was prepared. The process parameters include laser power 1000- 1300W, scanning speed 6-7mm/s, overlap distance 1.5-1.9mm, forming a high-entropy alloy coating with a single-center cubic solid solution structure.
A single-phase body-center cubic structure NiFeCoMoV high-entropy alloy coating with uniform tissue, high hardness and high corrosion resistance without subsequent heat treatment was obtained. The microhardness reached 340HV0.05, and the corrosion resistance was better than arc smelting and 45 steel matrix. Good corrosion resistance is shown in different corrosion environments.
Smart Images

Figure CN119082582A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an alloy coating and a preparation method thereof, and in particular to a corrosion-resistant high-entropy alloy coating and a preparation method thereof. Background Art
[0002] At present, the service environment of materials used in aerospace, national defense, deep sea and other fields is becoming more and more demanding. The performance of traditional engineering materials is increasingly difficult to meet the increasingly demanding use environment. Surface modification technology can form WC wear-resistant coatings, NiCr anti-corrosion coatings, MCrAlY high-temperature alloy coatings, etc. on the surface of materials. However, the performance of traditional coating materials is relatively single, and it is impossible to have comprehensive properties such as wear resistance, corrosion resistance, high temperature resistance, high strength and toughness at the same time, and it cannot adapt to more complex working environments. Therefore, the development of new alloy coating materials is imminent.
[0003] The unique crystal structure and organizational characteristics of high-entropy alloys make them have higher strength, hardness, better corrosion resistance, wear resistance, good thermal stability and other excellent properties than common metal materials. They have broad industrial application prospects in wear-resistant alloys, high-temperature alloys, corrosion-resistant alloys, etc. High-entropy alloys are mainly divided into high-entropy alloy blocks, films and coatings. The preparation of high-entropy alloy blocks mainly adopts vacuum melting and powder metallurgy methods; the preparation of high-entropy alloy films mainly adopts electrochemical deposition and magnetron sputtering methods; the preparation of high-entropy alloy coatings mainly adopts laser cladding, plasma cladding and plasma spraying methods. Arc melting, magnetron sputtering and other technologies have certain limitations in the preparation of large-size parts, and there are problems of component segregation and coarse grains. The rapid solidification characteristics of laser cladding technology can effectively avoid these problems by preparing size-controllable high-entropy alloy coatings, and the laser cladding process is simpler and cheaper.
[0004] Patent CN 110760843 A discloses a FeNiMoCoCrTi high entropy alloy coating obtained by layer-by-layer melting and covering on the surface of 45 steel by laser cladding method, and the hardness of the coating is about 4 times that of the substrate; Patent CN 112226766A discloses a high temperature wear resistant laser cladding CoCrFeMnNiCx high entropy alloy coating; Patent CN 117385252 A discloses a laser cladding and laser remelting FeCrMnVY high entropy alloy coating resistant to lead and bismuth corrosion; Patent CN 114481121 A discloses a laser cladding method for high entropy alloy for surface repair and strengthening, and a wear-resistant high entropy alloy coating is obtained by heat treating the laser cladding layer to precipitate the strengthening phase. Therefore, modifying the material surface by laser cladding technology is an effective method to improve the material performance.
[0005] However, defects such as pores, cracks and uneven structure are prone to occur in the high entropy alloy coating prepared by laser cladding using the synchronous powder feeding method. Summary of the invention
[0006] Purpose of the invention: The purpose of the present invention is to provide a corrosion-resistant high-entropy alloy coating with uniform structure and no need for subsequent heat treatment to strengthen the alloy properties;
[0007] The second object of the present invention is to provide a method for preparing the above-mentioned corrosion-resistant high-entropy alloy coating.
[0008] Technical solution: The corrosion-resistant high-entropy alloy coating described in the present invention comprises elements of Co, Fe, Mo, Ni, and V; the atomic percentage of Co, Fe, Mo, Ni, and V is 1:1:1:1:1.
[0009] Wherein, the corrosion-resistant high-entropy alloy coating is a single body-centered cubic solid solution structure.
[0010] The method for preparing the above-mentioned corrosion-resistant high-entropy alloy coating comprises the following steps:
[0011] (1) preparing raw materials of cobalt powder, iron powder, molybdenum powder, nickel powder and vanadium powder in equal atomic ratios and mixing them by ball milling;
[0012] (2) adding an ethyl cellulose ethanol solution to the ball-milled metal powder, stirring, coating on the pretreated substrate surface, and vacuum drying to obtain a pre-laid metal powder layer;
[0013] (3) The pre-laid metal powder layer is laser clad to obtain a high entropy alloy coating.
[0014] Among them, in step (3), the process parameters of laser cladding are: laser power is 1000-1300W, scanning speed is 6-7mm / s, and overlap distance is 1.5-1.9mm.
[0015] Wherein, in step (2), the mass ratio of the ethyl cellulose ethanol solution to the metal powder is 1-1.5:2.5.
[0016] Wherein, in step (2), the mass concentration of the ethyl cellulose ethanol solution is 3-8%.
[0017] Wherein, in step (2), the thickness of the pre-laid metal powder layer is 0.4-1.2 mm.
[0018] Wherein, in step (1), the process parameters of ball milling are: ball-to-material ratio is 10-15:1, ball milling time is 5-10h, and rotation speed is 200-450rpm.
[0019] Wherein, in step (1), zirconia ceramic balls are used for ball milling, and the diameter of the zirconia ceramic balls is 2-12 mm.
[0020] Wherein, in step (1), the particle size of the metal powder after ball milling is 5-15 μm.
[0021] Beneficial effects: Compared with the prior art, the present invention achieves the following significant effects: (1) The corrosion-resistant high-entropy alloy coating of the present invention first pre-lays powder on the surface of the substrate, and then performs laser cladding, so as to prepare a single-phase high-entropy alloy coating with uniform structure in one step, without the need for subsequent heat treatment to strengthen the alloy properties. (2) The cladding material used in the present invention is a mixed powder of five metals, which is low in cost compared to high-entropy alloy powder. A high-hardness, high-corrosion-resistant single-phase body-centered cubic NiFeCoMoV high-entropy alloy coating is obtained on the surface of the substrate through laser cladding technology. (3) The cladding layer prepared by the present invention is metallurgically bonded to the substrate, the coating structure is fine and dense, without pores and crack defects, and the Vickers hardness of the cladding layer reaches 340HV 0.05 , which is 1.4 times that of arc-melted high-entropy alloy and 1.6 times that of 45 steel substrate. The corrosion resistance of laser cladding high-entropy alloy coating in different corrosion environments of 0.5MNaCl, H2SO4 and NaOH is better than that of arc-melted high-entropy alloy and 45 steel substrate, showing good corrosion resistance. (4) The present invention is suitable for large-area modification of the workpiece surface, and can also be used for surface repair of failed workpieces to increase the service life of the workpiece. The present invention provides a new idea for the design and preparation of corrosion-resistant high-entropy alloy coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is the XRD spectrum of the ball-milled powder and the laser-clad NiFeCoMoV high-entropy alloy coating of Example 1;
[0023] Figure 2 is the microstructure of the laser cladding coating of Example 1;
[0024] Figure 3 is the cross-sectional gradient hardness of the laser cladding coating of Example 1;
[0025] Figure 4 are polarization curves of the laser cladding coating, arc-melted high entropy alloy and 45 steel substrate in 0.5 M NaOH solution of Example 1;
[0026] Figure 5 This is the surface macroscopic morphology of a single pass of the high entropy alloy coating at different powers in Comparative Example 2;
[0027] Figure 6 This is the cross-sectional macroscopic morphology of a single layer of high entropy alloy coating at different powers in Example 2. DETAILED DESCRIPTION
[0028] The present invention is described in further detail below.
[0029] Example 1
[0030] A corrosion-resistant high-entropy alloy coating, whose constituent elements are NiFeCoMoV in equiatomic ratios; and a preparation method thereof is as follows:
[0031] Step 1: Ball milling
[0032] First, the raw materials of cobalt powder, iron powder, molybdenum powder, nickel powder and vanadium powder are prepared in equal atomic ratios, put into a planetary ball mill, and mechanically mixed under argon protection. The ball-to-material ratio is 15:1, and the mass ratio of zirconia ceramic balls of different diameters is Φ12mm:Φ8mm:Φ4mm:Φ2mm=1:1:1:1. The ball milling time is 10h, and the speed is 450rpm; the particle size of the metal powder after ball milling is 5-15μm.
[0033] Step 2: Pre-lay powder
[0034] 5% mass fraction of ethyl cellulose ethanol solution was added to the ball-milled powder and stirred into a paste, and then evenly coated on the pretreated 45 steel substrate surface, with a pre-coating thickness of 0.4 mm. After standing to dry, it was placed in a vacuum drying oven and dried at 80°C for 3 hours.
[0035] Step 3: Laser Cladding
[0036] IPS-YLS-3000 fiber laser was used for laser cladding. The process parameters were as follows: spot diameter of 4 mm, laser power of 1200 W, scanning speed of 6 mm / s, overlap distance of 1.7 mm, and inert gas Ar or He gas protection was used during cladding.
[0037] The surface of the obtained high entropy alloy coating was ground and polished, and structural characterization and performance testing were carried out.
[0038] Example 2
[0039] A corrosion-resistant high-entropy alloy coating, whose constituent elements are NiFeCoMoV in equiatomic ratios; and a preparation method thereof is as follows:
[0040] Step 1: Ball milling
[0041] First, the raw materials of cobalt powder, iron powder, molybdenum powder, nickel powder and vanadium powder were prepared in equal atomic ratios, put into a planetary ball mill, and mechanically mixed under argon protection. The ball-to-material ratio was 15:1, and the mass ratio of zirconia ceramic balls of different diameters was Φ12mm:Φ8mm:Φ4mm:Φ2mm=1:1:1:1. The ball milling time was 5h and the rotation speed was 200rpm.
[0042] Step 2: Pre-lay powder
[0043] 3% mass fraction of ethyl cellulose ethanol solution was added to the ball-milled powder and stirred into a paste, and then evenly coated on the pre-treated 45 steel substrate surface, with a pre-coating thickness of 0.4 mm. After standing to dry, it was placed in a vacuum drying oven and dried at a temperature of 80°C for 3 hours.
[0044] Step 3: Laser Cladding
[0045] IPS-YLS-3000 fiber laser was used for laser cladding. The process parameters were as follows: spot diameter of 4 mm, laser power of 1100 W, scanning speed of 6 mm / s, overlap distance of 1.5 mm, and inert gas Ar or He gas protection was used during cladding.
[0046] Example 3
[0047] A corrosion-resistant high-entropy alloy coating, whose constituent elements are NiFeCoMoV in equiatomic ratios; and a preparation method thereof is as follows:
[0048] Step 1: Ball milling
[0049] First, the raw materials of cobalt powder, iron powder, molybdenum powder, nickel powder and vanadium powder were prepared in equal atomic ratios, put into a planetary ball mill, and mechanically mixed under argon protection. The ball-to-material ratio was 15:1, and the mass ratio of zirconia ceramic balls of different diameters was Φ12mm:Φ8mm:Φ4mm:Φ2mm=1:1:1:1. The ball milling time was 5h and the rotation speed was 200rpm.
[0050] Step 2: Pre-lay powder
[0051] 8% mass fraction of ethyl cellulose ethanol solution was added to the ball-milled powder and stirred into a paste, and then evenly coated on the pretreated 45 steel substrate surface, with a pre-coating thickness of 0.4 mm. After standing to dry, it was placed in a vacuum drying oven and dried at 80°C for 3 hours.
[0052] Step 3: Laser Cladding
[0053] IPS-YLS-3000 fiber laser was used for laser cladding. The process parameters were as follows: spot diameter of 4 mm, laser power of 1300 W, scanning speed of 7 mm / s, overlap distance of 1.9 mm, and inert gas Ar or He gas protection was used during cladding.
[0054] Comparative Example 1
[0055] NiFeCoMoV high entropy alloys with the same composition were prepared by vacuum melting technology. Their microhardness and corrosion resistance were tested.
[0056] Comparative Example 2
[0057] On the basis of Example 1, different from Example 1, three groups of comparative experiments with different laser powers are set up, and the powers are 1000W, 1100W, 1200W, and 1300W respectively.
[0058] Experimental Example 1 Microstructure Analysis of Laser Cladding NiFeCoMoV High Entropy Alloy Coating
[0059] Phase analysis of the metal powder and laser cladding coating obtained after ball milling of the raw material in Example 1 was performed. The results are as follows: Figure 1 As shown. The study shows that after 10 hours of ball milling, the diffraction peaks of the pure elements corresponding to each principal element still exist clearly, and the alloying degree of the mixed powder is low. The three diffraction peaks of the laser cladding coating correspond to the (110), (200) and (211) crystal planes of the body-centered cubic structure, so the laser cladding NiFeCoMoV high entropy alloy coating is a single-phase body-centered cubic structure. Figure 2 The microstructure of the laser cladding coating shows that the laser cladding NiFeCoMoV high entropy alloy coating has fine and uniform structure and is a dense equiaxed dendrite. The laser cladding layer of Example 1 has no pores or cracks.
[0060] Experimental Example 2: Cross-sectional gradient hardness test of laser cladding NiFeCoMoV high entropy alloy coating
[0061] The cross section of the laser cladding layer of Example 1 was tested for gradient hardness using a microhardness tester (HVS-1000). The results are as follows: Figure 3 The experiment shows that the hardness of the high entropy alloy coating is significantly higher than that of the substrate, and the hardness changes gradually from the surface to the inside. The average microhardness of the high entropy alloy coating is about 340HV. 0.05 , which is 1.65 times that of 45 steel substrate. The coating and substrate are subjected to laser thermal cycle and accompanied by mutual diffusion of coating and substrate elements, forming a heat-affected zone, increasing the depth of the hardened layer, and the depth of the hardened layer reaches about 0.9mm. Compared with the comparative example, the microhardness of the arc-melted high-entropy alloy is about 240HV 0.05 , the hardness of laser cladding high entropy alloy coating is about 1.4 times that of the original one.
[0062] Experimental Example 3 Corrosion Performance Test of Laser Cladding NiFeCoMoV High Entropy Alloy Coating
[0063] Electrochemical tests were performed on the laser cladding high entropy alloy coating of Example 1, the arc-melted high entropy alloy of the comparative example, and the 45 steel substrate in different corrosive solutions of 0.5 M NaCl, H2SO4, and NaOH. The results are shown in Tables 1 and Figure 5 As shown. Studies have shown that laser cladding high entropy alloy coatings exhibit excellent corrosion resistance in three different corrosive media, and their corrosion resistance is better than that of arc-melted high entropy alloys and substrate 45 steel. Figure 4As shown in the figure, in 0.5M NaOH solution, NiFeCoMoV high entropy alloy presents a stable passivation zone at the anode, and the laser cladding high entropy alloy coating has the widest stable passivation zone and the lowest passivation current density, which is one order of magnitude lower than that of arc-melted high entropy alloy and two orders of magnitude lower than that of 45 steel. Therefore, the passivity of the laser cladding high entropy alloy coating is the most stable and more corrosion-resistant.
[0064] Table 1 Corrosion performance results of comparative example 1, substrate and embodiment 1
[0065]
[0066] Figure 5 The surface macroscopic morphology of a single high entropy alloy coating at different powers in Comparative Example 2 is shown in Figure 2, where (a) is 1000W, (b) is 1100W, (c) is 1200W, and (d) is 1300W. After repeated experiments, it was found that when the laser power was less than 1000W, the coating was discontinuous and alloying was not achieved. When the laser power was in the range of 1000W-1300W, the morphology of each single coating showed good continuous spreading, and the corresponding coating cross-sectional morphology ( Figure 6 ) is also relatively flat.
[0067] Figure 6 The cross-sectional macroscopic morphology of a single channel of the high entropy alloy coating at different powers in Comparative Example 2, where (a) 1000W, (b) 1100W, (c) 1200W, and (d) 1300W. It can be seen that the coating is tightly bonded to the substrate and has good metallurgical bonding. The thickness of the coating is between 0.3mm and 0.4mm at different laser powers of 1000W-1300W, and the coating thickness meets expectations and the surface is relatively flat. When the power is 1200W, the coating surface molding quality is the best, and it is continuously flat and smooth without cracks and pores. In summary, the laser cladding method provided by the present invention is an ideal preparation method for obtaining a high-strength, high-corrosion-resistant NiFeCoMoV high-entropy alloy coating. Under appropriate process parameters, the laser cladding coating obtains a single-phase, fine equiaxed crystal, and its microhardness is 1.4 times that of the arc-melted high-entropy alloy and 1.65 times that of the substrate 45 steel, and exhibits good corrosion resistance under different corrosion environments.
Claims
1. A corrosion-resistant high-entropy alloy coating, characterized in that: The constituent elements of the high entropy alloy coating include Co, Fe, Mo, Ni, and V; the atomic percentage of Co, Fe, Mo, Ni, and V is 1:1:1:1:
1.
2. The corrosion-resistant high-entropy alloy coating according to claim 1, characterized in that: The corrosion-resistant high-entropy alloy coating is a single body-centered cubic solid solution structure.
3. A method for preparing the corrosion-resistant high-entropy alloy coating according to claim 1, characterized in that: The following steps are involved: (1) preparing raw materials of cobalt powder, iron powder, molybdenum powder, nickel powder and vanadium powder in equal atomic ratios and mixing them by ball milling; (2) adding an ethyl cellulose ethanol solution to the ball-milled metal powder, stirring, coating on the pretreated substrate surface, and vacuum drying to obtain a pre-laid metal powder layer; (3) The pre-laid metal powder layer is laser clad to obtain a high entropy alloy coating.
4. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (3), the process parameters of laser cladding are: laser power is 1000-1300W, scanning speed is 6-7mm / s, and overlap distance is 1.5-1.9mm.
5. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (2), the mass ratio of the ethyl cellulose ethanol solution to the metal powder is 1-1.5:2.
5.
6. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (2), the mass concentration of the ethyl cellulose ethanol solution is 3-8%.
7. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (2), the thickness of the pre-laid metal powder layer is 0.4-1.2 mm.
8. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (1), the process parameters of ball milling are: ball-to-material ratio is 10-15:1, ball milling time is 5-10h, and rotation speed is 200-450rpm.
9. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (1), zirconia ceramic balls are used for ball milling, and the diameter of the zirconia ceramic balls is 2-12 mm.
10. The method for preparing the corrosion-resistant high-entropy alloy coating according to claim 3, characterized in that: In step (1), the particle size of the metal powder after ball milling is 5-15 μm.