Steel belt special for mortise and tenon joint structure

By optimizing the chemical composition and process of steel strips, the problem of the difficulty of both tensile strength and elongation after break in the existing steel materials in the mortise and tenon structure is solved, and high-performance steel strip materials are realized, which are suitable for construction projects.

CN119082609APending Publication Date: 2024-12-06ZHEJIANG TOPSUN LOGISTIC CONTROL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411239806.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

It is difficult for existing steel materials to have high tensile strength and elongation after break in mortise and tenon structures. The chemical composition of conventional steel strips is not suitable, resulting in increased brittleness and decreased plasticity.

Method used

By optimizing the chemical composition of the steel strip, the content of elements such as C, Si, Mn, P, S, Cr, Ni, Cu is controlled, and C is ensured that C≤0.2%, Si≤0.60%, Mn≤2.0%, and P≤0.025%. S≤0.015%, Cr 0.30%-1.25%, Ni 0.12%-0.65%, Cu 0.16%-0.55%, to improve tensile strength and elongation after break, and ensure through precise process processing such as converter oxygen smelting, etc. Ingredients synergistically.

Benefits of technology

The high tensile strength (≥550MPa) and high elongation (≥20%) of the steel belt are achieved, and weldability and weather resistance are improved, which is suitable for steel structures in construction projects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005028892890000121
    Figure BDA0005028892890000121
Patent Text Reader

Abstract

The invention relates to a special steel belt for a mortise and tenon joint structure, and belongs to the technical field of alloy steel materials. In order to solve the problem that the mechanical strength of an existing steel belt cannot be achieved at the same time, the steel belt special for the mortise and tenon joint structure is provided and is prepared from, by mass, smaller than or equal to 0.2% of C; si: less than or equal to 0.60%; mn: < = 2.0%; p: less than or equal to 0.025%; less than or equal to 0.015% of S; 0.30% to 1.25% of Cr; 0.12% to 0.65% of Ni; 0.16%-0.55% of Cu and the balance Fe. The steel strip has the performance of high tensile strength and elongation after fracture, the tensile strength reaches 650 MPa or above, the lower yield strength reaches 550 MPa or above, and the elongation after fracture reaches 20% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a special steel belt for mortise and tenon structures, belonging to the technical field of alloy steel materials. Background Art

[0002] The mortise and tenon structure (steel structure) is a structure composed of steel materials. The main frame of the mortise and tenon structure is composed of multiple beams, columns, trusses and other components made of steel materials such as steel strips and steel sections. This mortise and tenon structure is widely used in buildings, bridges, shelves, venues and other fields due to its convenient construction and high strength, especially in construction projects. It plays an increasingly important role. However, the application of steel materials in these mortise and tenon structures also needs to consider the demand for mechanical strength of the steel structure and the connection nodes of the mortise and tenon structure. The existing ordinary steel structure materials are not strong enough in mechanical strength and are prone to deformation and movement. Therefore, higher requirements are placed on the mechanical strength performance of the steel materials used in the mortise and tenon structure, especially on the control of indicators such as tensile strength and elongation of steel materials. This is mainly because general steel materials have opposite performance in tensile strength and elongation. This requires considering how to achieve both performances, which is also the key technical performance requirements for the application of steel materials used in mortise and tenon structures. Conventional steel materials are difficult to achieve the performance index requirements of both. For example, the steel strip disclosed in the existing literature has the following chemical composition weight percentage content: C: ≤0.5%; Si: ≤0.5%; Mn: 0.30%~0.5%; P: 0.07%~0.15%; S: ≤0.035%; Cr: 0.30%~1.2%; Ni: 0.10~0.5%; Cu: 0.25%~0.40%, and the balance is Fe. For the steel strips of the above type, the P and S contents are relatively high. The presence of excessive S content easily leads to the formation of MnS and other inclusions in the alloy, resulting in the enrichment of MnS in local areas of the organization, breaking the continuity of the matrix, causing the steel material to become more brittle and its plasticity to decrease; similarly, excessive P content will also cause non-metallic compounds to be included in the alloy, resulting in increased brittleness of the steel strip, thereby reducing its plasticity and thus reducing the elongation performance after fracture, and it is not easy to operate and process. Summary of the invention

[0003] In view of the defects existing in the above prior art, the present invention provides a special steel belt for mortise and tenon structure, and solves the problem of how to achieve the performance of the steel belt with both high tensile strength and elongation after fracture.

[0004] The object of the present invention is achieved through the following technical solution: a special steel strip for mortise and tenon structure, the steel strip is made of the following components in mass percentage:

[0005] C: ≤0.2%; Si: ≤0.60%; Mn: ≤2.0%; P: ≤0.025%; S: ≤0.015%; Cr: 0.30%~1.25%; Ni: 0.12%~0.65%; Cu: 0.16%~0.55%, the balance is Fe.

[0006] The C element in the composition of the special steel strip mainly plays the role of strengthening and refining the grains, which helps to increase the strength performance of the steel strip. However, the amount of C element not only affects the strength performance of the steel material, but more importantly, it also affects the plasticity and toughness of the steel strip. If the added content is too high, the plasticity and toughness of the steel will be reduced, which will eventually affect the elongation after fracture of the material, and it is impossible to ensure that the elongation after fracture of the steel reaches the required index requirements. Therefore, by controlling the amount of C within 0.2%, the performance of strengthening and elongation after fracture can be achieved at the same time; the Si element is for the purpose of deoxidation, which is beneficial to avoid the formation of impurities such as non-metallic oxides due to the oxygen content process in the steel material, which affects the final elongation after fracture of the steel strip; the Mn element is an important element for enhancing toughness and has the performance of solid solution, which is beneficial to improve the strength and toughness of the steel strip. Compared with the general steel strip, the present invention improves the addition of the Mn element, and by controlling the amount of Mn within the upper limit of 2.0%, it controls it at a relatively high content, so that the steel can have both high strength and high toughness. At the same time, it is also to avoid the hardenability caused by the high dosage, which affects the weldability of the steel strip. However, when the strength performance is improved by increasing the dosage of the Mn element, the brittleness of the corresponding steel strip becomes higher and the toughness is affected, resulting in a decrease in the elongation after fracture. The present invention has found in the process of research that after increasing the upper limit content of the Mn element, by controlling the Si element and the S and P elements in the steel strip and controlling them within a lower range, the residual amount in the raw material of the steel material, here by accurately controlling its addition amount, can effectively ensure that the steel strip has a high tensile strength and lower yield strength while having the effect of high elongation after fracture. In addition, by the synergistic effect between the various components in the steel strip, the solid solution strengthening effect and the toughness enhancement function of elements such as C and Mn can be maximized, and Mn can more effectively weaken or eliminate the hot brittleness caused by a small amount of S, improve the processing performance, and at the same time cooperate with the control of elements such as S and P to play a synergistic role, so that the effect of both high tensile strength and elongation after fracture is effectively achieved, and the weldability is good, and the weathering effect of the weather-resistant steel strip itself against atmospheric corrosion can be guaranteed. The special steel strip for the mortise and tenon structure of the present invention can be used as special steel for the mortise and tenon structure of steel structures in the field of construction engineering (for beams, columns, etc.), and the steel strip can also be further made into specific products such as steel plates and steel pipes according to the application requirements of the steel materials of the mortise and tenon structure.

[0007] Furthermore, in order to solve the problem of brittle material after the strength (tensile strength and yield strength) of the steel strip is improved, so as to better ensure that the elongation of the steel strip is above 20%, the present invention adopts a system with low P content and low S content through more precise and strict control, which can promote the anisotropy of the steel strip, avoid the inclusion of sulfides (such as MnS) or non-metallic oxides in the system and affect the toughness, effectively achieve the index requirement of elongation after fracture of more than 20%, and effectively improve the mechanical properties, the tensile strength performance reaches ≥550MPa, and the lower yield strength reaches 450MPa. At the same time, a small amount of P and S elements in the system is beneficial to ensure weather resistance, and the added Cr, Cu elements and Ni work together to ensure the weather resistance of the steel, and adjust the content of Cu-Cr-Ni among the three, which can also effectively ensure the corrosion resistance of the steel strip. Specifically, by adding Cr elements to the composition of the steel strip and controlling the content within the above-mentioned range, the strength performance and toughness can be guaranteed, and the weather resistance of the steel strip can be effectively guaranteed. The added Ni and Cu elements play a role of solid solution and precipitation strengthening, and can also effectively avoid factors that may affect the weather resistance of the steel strip when the upper limit of the Mn content is high; in addition, the presence of Cu and P elements can make the steel strip have better weather resistance, thereby ensuring the performance of improving the toughness of the steel strip while having weather resistance, so as to achieve the effect of high elongation after fracture.

[0008] In the above-mentioned special steel strip for the mortise and tenon structure, as a preference, the steel strip is made of the following components in mass percentage:

[0009] C: 0.13% ~ 0.15%; Si: 0.45% ~ 0.56%; Mn: 1.55% ~ 1.85%; P: ≤ 0.015%; S: ≤ 0.015%; Cr: 0.30% ~ 1.25%; Ni: 0.12% ~ 0.65%; Cu: 0.16% ~ 0.55%, the balance is iron. By controlling the Mn element in a relatively high content range and the Si element in a range of 0.45% to 0.56%, it can effectively deoxidize, better reduce the oxygen content in the steel material, and avoid the high silicon content affecting the toughness of the material. By synchronously adjusting the content of Mn, Si, S and P, it can more effectively avoid the formation of sulfide impurities and non-metallic oxides, thereby ensuring the continuity of the organization in the steel strip, avoiding the delamination and fracture of the steel strip organization caused by the influence of sulfide inclusions or non-metallic oxides, and better ensuring the mechanical strength of the steel strip, so that the tensile strength is increased to more than 650MPa, and the lower yield strength reaches more than 550MPa. In addition, by making the addition amount of Si relatively high so that it can play a deoxidation effect, it can better avoid the generation of other non-metallic impurities, so that it can more effectively have the performance of high toughness and achieve the performance of high elongation after fracture, and generally make the elongation after fracture reach more than 22%. As a further preferred embodiment, the mass percentage of Mn is 1.62% to 1.80%.

[0010] In the special steel strip for the mortise and tenon structure, as a preferred embodiment, the mass ratio of (C+Mn+Si): (Si+P+S) is 2.48:0.562-0.564, which is equivalent to 1:0.226-0.228. By strictly controlling the dosage of the above components, the components of the system can achieve a better synergistic effect, effectively ensuring that the steel strip has both strength performance and elongation after fracture. Both have obvious performance guarantees, with a tensile strength of more than 700MPa, a lower yield strength of more than 640MPa, and an elongation after fracture of more than 28%.

[0011] In the above-mentioned special steel strip for mortise and tenon structure, as a preference, the composition of the steel strip also includes the following components in mass percentage:

[0012] B: 0.08% to 0.12%; In: 0.04% to 0.06%; Bi: 0.01% to 0.02%; Ta: 0.01% to 0.02%. By adding the above B (boron), In (indium), Bi (bismuth) and Ta (tantalum) elements, the toughness of the steel strip can be better improved, especially the addition of In and Ta can make the steel strip have excellent toughness, can make the elongation after fracture have better performance, and can also make the steel strip have excellent performance in tensile strength and yield strength. Further preferably, the mass ratio of (Mn+Cu): (In+Ta) is 1.72 to 1.78: 0.06. By more accurately controlling the proportional relationship between the above elements in the system, better synergy can be achieved, so that the steel strip has more excellent toughness performance, achieves a high elongation after fracture, and can ensure high tensile strength and yield strength performance, with the elongation after fracture reaching more than 30%, the tensile strength reaching more than 700MPa, and the lower yield strength reaching more than 620MPa.

[0013] In the special steel strip for the mortise and tenon structure, as a preferred embodiment, the composition of the steel strip also includes Nb, V and Ti, and the sum of the mass percentages of (Nb+V+Ti) is ≤0.22%. The strength and toughness are improved, so that the steel strip has both tensile strength and high mechanical strength properties after elongation. Specifically, the addition of Nb elements can promote the grain refinement of the steel strip organization, improve strength and enhance toughness, but too much Nb element will promote the evolution of ferrite δ phase or other brittleness, which will reduce the toughness of the matrix of the steel strip. Therefore, it is best to control the Nb content to 0.012% to 0.015%. The addition of Ti can inhibit the growth of austenite grains during rolling and refine the grains, but when too much is added, large particles are easily formed, which is easy to lose the function of refining grains, so it is best to control the Ti content to 0.03% to 0.04%. The addition of V elements can also improve the overall ductility of the steel strip and increase toughness.

[0014] In summary, compared with the prior art, the present invention has the following advantages:

[0015] 1. By controlling the amount of Mn within the upper limit of 2.0%, the manganese content is relatively increased, which can make the steel have both high strength and high toughness properties; at the same time, by controlling the S and P elements in the steel strip and keeping them in a lower range, it can effectively ensure that the steel strip has a high tensile strength and lower yield strength while also having a high elongation after fracture.

[0016] 2. The steel strip of the present invention has the properties of high tensile strength and elongation after fracture, with the tensile strength reaching above 650 MPa, the lower yield strength reaching above 550 MPa, and the elongation after fracture reaching above 20%.

[0017] 3. The mass ratio of (C+Mn+Si):(Si+P+S) in the steel strip composition can be 2.55:0.562-0.564. It can effectively ensure that the steel strip has both strength performance and elongation after fracture, with the tensile strength reaching more than 700MPa, the lower yield strength reaching more than 630MPa, and the elongation after fracture reaching more than 28%. DETAILED DESCRIPTION

[0018] The technical solution of the present invention is further specifically described below through specific embodiments, but the present invention is not limited to these embodiments.

[0019] Example 1

[0020] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0021] C: 0.11%; Si: 0.56%; Mn: 1.85%; P: ≤0.015%; S: ≤0.015%;

[0022] Cr: 0.81%; Ni: 0.15%; Cu: 0.25%, and the balance is iron.

[0023] The following processes can be used to process the special steel strip for the mortise and tenon structure, but the process is not limited thereto. The main innovation of the present invention is the design of the composition of the steel strip and the control of the content. It is best to use conventional converter oxygen smelting for processing. Specifically, it includes the processes of primary refining, preliminary refining, vacuum refining, continuous casting and rolling. In other words, the processing process of the weathering steel strip is as follows:

[0024] Primary refining: according to the content ratio of each component in the steel strip, raw materials are added as needed, and then slag-making agent is added for primary refining to obtain primary molten steel; the primary refining temperature is preferably controlled at 1530℃~1680℃, and the time is controlled at 10min~18min;

[0025] Preliminary refining: the above-mentioned molten steel is transferred to a refining furnace and alloyed with raw materials such as ferrochrome, ferrosilicon, carbon ferromanganese, etc. to obtain molten steel after preliminary refining; preferably, the preliminary refining temperature is 1560℃~1690℃ and the time is controlled within 45min~50min;

[0026] Vacuum refining: Put the molten steel after preliminary refining into a vacuum refining furnace and perform vacuum refining under the condition of blowing argon gas; then perform continuous casting process and rolling to obtain the required steel strip. Of course, it is best to control the temperature of vacuum refining at 1510℃~1670℃, the vacuum degree at 100Pa~300Pa, and the time at 10min~18min to obtain refined molten steel. It is best to control the thickness of the steel strip within 16mm, and the preferred thickness specification range is 3.0~16.0mm, and the width specification range is 1000~1600mm. In this embodiment, the specification adopts a thickness of 3.0mm~6.0mm.

[0027] Example 2

[0028] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0029] C: 0.15%; Si: 0.55%; Mn: 1.68%; P: ≤0.015%; S: ≤0.015%;

[0030] Cr: 1.25%; Ni: 0.12%; Cu: 0.16%, and the balance is iron.

[0031] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0032] Example 3

[0033] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0034] C: 0.13%; Si: 0.45%; Mn: 1.55%; P: ≤0.015%; S: ≤0.015%;

[0035] Cr: 0.30%; Ni: 0.65%; Cu: 0.55%, and the balance is iron.

[0036] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0037] Example 4

[0038] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0039] C: 0.12%; Si: 0.52%; Mn: 1.60%; P: ≤0.013%; S: ≤0.011%;

[0040] Cr: 1.12%; Ni: 0.23%; Cu: 0.28%, and the balance is iron.

[0041] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0042] Example 5

[0043] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0044] C: 0.14%; Si: 0.49%; Mn: 1.58%; P: ≤0.012%; S: ≤0.012%;

[0045] Cr: 0.36%; Ni: 0.12%; Cu: 0.16%; Nb: 0.012%; Ti: 0.03%, V: 0.12%, and the balance is iron.

[0046] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0047] Example 6

[0048] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0049] C: 0.14%; Si: 0.47%; Mn: 1.74%; P: ≤0.012%; S: ≤0.012%;

[0050] Cr: 1.12%; Ni: 0.12%; Cu: 0.16%~0.55%, Nb: 0.015%; Ti: 0.04%, V: 0.11%, and the balance is iron.

[0051] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0052] Example 7

[0053] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0054] C: 0.14%; Si: 0.54%; Mn: 1.80%; P: 0.013%; S: 0.011%; Cr: 1.12%; Ni: 0.23%; Cu: 0.28%, and the balance is iron.

[0055] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0056] Example 8

[0057] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0058] C: 0.15%; Si: 0.55%; Mn: 1.78%; P: 0.006%; S: 0.006%; Cr: 1.12%; Ni: 0.23%; Cu: 0.28%, and the balance is iron.

[0059] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0060] Example 9

[0061] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0062] C: 0.15%; Si: 0.55%; Mn: 1.78%; P: 0.006%; S: 0.006%; Cr: 1.12%; Ni: 0.23%; Cu: 0.28%, Nb: 0.015%; Ti: 0.04%, V: 0.11%, and the balance is iron.

[0063] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0064] Example 10

[0065] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0066] C: 0.15%; Si: 0.55%; Mn: 1.78%; P: 0.006%; S: 0.006%; Cr: 1.12%; Ni: 0.23%; Cu: 0.28%, Nb: 0.015%; Ti: 0.04%, V: 0.11%, B: 0.12%; In: 0.05%; Bi: 0.01%; Ta: 0.01%, the balance is iron.

[0067] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0068] Embodiment 11

[0069] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0070] C: 0.15%, Si: 0.55%, Mn: 1.78%, P: 0.006%, S: 0.006%, Cr: 1.12%, Ni: 0.23%, Cu: 0.20%, Nb: 0.015%, Ti: 0.04%, V: 0.11%, B: 0.12%, In: 0.05%, Bi: 0.01%, Ta: 0.01%, and the balance is iron.

[0071] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0072] Example 12

[0073] The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in percentage by mass:

[0074] C: 0.13%; Si: 0.52%; Mn: 1.65%; P: 0.012%; S: 0.012%; Cr: 0.68%; Ni: 0.16%; Cu: 0.3%, Nb: 0.012%; Ti: 0.03%, V: 0.12%, B: 0.10%; In: 0.05%; Bi: 0.02%; Ta: 0.02%, the balance is iron.

[0075] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0076] Comparative Example 1

[0077] In order to better illustrate the influence of the synergistic effect between the components of the present invention on the tensile strength performance and the elongation after break.

[0078] In order to illustrate the effect of the amount of Si, Mn, P and S on the elongation after fracture, this comparative example increases the content of P and S through artificial control. The content of each component in the special steel strip for the mortise and tenon structure of this example specifically includes the following mass percentages:

[0079] C: 0.11%; Si: 0.56%; Mn: 1.85%; P: 0.07%; S: 0.035%; Cr: 0.81%; Ni: 0.15%; Cu: 0.25%, and the balance is iron.

[0080] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0081] Comparative Example 2

[0082] In order to better illustrate the synergistic effect between the components of the present invention on the tensile strength performance and elongation after fracture, this comparative example is used to illustrate the effect of the dead amount of Si and Mn elements on the elongation after fracture;

[0083] The content of Si element is relatively low for comparison. The content of each component in the special steel strip for mortise and tenon structure of this example specifically includes the following components in mass percentage:

[0084] C: 0.15%; Si: 0.55%; Mn: 1.68%; P: 0.06%; S: ≤0.025%;

[0085] Cr: 1.25%; Ni: 0.12%; Cu: 0.16%, and the balance is iron.

[0086] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0087] Comparative Example 3

[0088] In order to illustrate the effect of the content control of Si and Mn on the elongation after fracture of the present invention, this comparative example adjusts these two components so that the corresponding addition is controlled within a low content range;

[0089] At the same time, the contents of P and S are controlled within the range required by the present invention for comparison. The contents of the various components in the special steel strip for the mortise and tenon structure of this example specifically include the following components in mass percentage:

[0090] C: 0.12%; Si: 0.41%; Mn: 0.85%; P: ≤0.02%; S: ≤0.011%;

[0091] Cr: 1.12%; Ni: 0.23%; Cu: 0.28%, and the balance is iron.

[0092] The following process can be used to process the special steel strip for the mortise and tenon structure, but it is not limited thereto. That is, it is best to use converter oxygen blowing smelting for processing. The specific processing technology refers to Example 1 and will not be repeated here.

[0093] The steel strips obtained in the above embodiments were randomly selected for mechanical strength performance tests. The sampling was carried out according to GB / T 2975 and the test method was GB / T 228.1. The corrosion rate was tested by simulating atmospheric corrosion test. The specific test results are shown below:

[0094] Table 1:

[0095]

[0096] At the same time, the steel strips obtained in the above-mentioned Examples 1-12 of the present invention were sampled and tested, and the sampling and testing methods were based on GB / T 10561. The results showed that the coarse non-metallic inclusions in the steel strips were not greater than 2.0, and the fine non-metallic inclusions were not greater than 2.5, while the corresponding indicators in Comparative Examples 1 and 2 did not meet the requirements. The overall weldability of the steel strip was good.

[0097] The specific embodiments described in the present invention are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the attached claims.

[0098] Although the present invention has been described in detail and some specific embodiments have been cited, it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.

Claims

1. A special steel strip for mortise and tenon structure, characterized in that: The steel strip is made of the following composition in mass percentage: C: ≤0.2%; Si: ≤0.60%; Mn: ≤2.0%; P: ≤0.025%; S: ≤0.015%; Cr: 0.30%~1.25%; Ni: 0.12%~0.65%; Cu: 0.16%~0.55%, the balance is Fe.

2. The special steel strip for the mortise and tenon structure according to claim 1 is characterized in that: The steel strip is made of the following components in mass percentage: C: 0.13%~0.15%; Si: 0.45%~0.56%; Mn: 1.55%~1.85%; P: ≤0.015%; S: ≤0.015%; Cr: 0.30%~1.25%; Ni: 0.12%~0.65%; Cu: 0.16%~0.55%, the balance is iron.

3. The special steel strip for the mortise and tenon structure according to claim 2 is characterized in that: The mass percentage of Mn is 1.62% to 1.80%.

4. The special steel strip for the mortise and tenon structure according to claim 1, 2 or 3, characterized in that: The mass ratio of (C+Mn+Si):(Si+P+S) is 2.48:0.562-0.

564.

5. The special steel strip for the mortise and tenon structure according to claim 1, 2 or 3, characterized in that: The composition of the steel strip also includes the following components in mass percentage: B:0.08%~0.12%; In: 0.04%~0.06%; Bi: 0.01%~0.02%; Ta: 0.01%~0.02%.

6. The special steel strip for the mortise and tenon structure according to claim 5, characterized in that: The mass ratio of (Mn+Cu):(In+Ta) is 1.85-2.0:0.

06.

7. The special steel strip for the mortise and tenon structure according to claim 1, 2 or 3, characterized in that: The steel strip also includes Nb, V and Ti in its composition, and the sum of the mass percentages of (Nb+V+Ti) is ≤0.22%.

8. The special steel strip for the mortise and tenon structure according to claim 7, characterized in that: The sum of the mass percentages of (Nb+V+Ti) is ≤0.13%, the mass percentage of Nb is 0.012% to 0.015%, and the mass percentage of Ti is 0.03% to 0.04%.