Crawler steel capable of reducing corner cracks and production process and quality inspection equipment thereof
Through the combination of nano Si3N4 ceramic powder and precise quality inspection equipment, the problem of measuring tooth height and inclination angle of the track steel is solved, ensuring the anti-slip performance and safety of the track steel, and avoiding the problem of brittle casting.
Patent Information
- Application Number
- CN202411186766.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art cannot accurately measure the tooth height and inclination angle of tracked steel, resulting in the inability to detect whether the teeth meet the standards, affecting the anti-slip effect.
A track steel including nano Si3N4 ceramic powder is designed, and its production process and quality inspection equipment. The moving components and detection components realize accurate measurement of the tooth height and inclination angle of the track steel, and the combined nano Si3N4 ceramic powder is suppressed during the smelting process. Concentrate stress to avoid brittleness of the casting blank.
Accurate judgment of the standards for the tooth part of the track is achieved, anti-slip performance and safety is ensured, potential risks caused by the failure of the tooth part standard, and the occurrence of cracks in the casting billet is avoided.
Smart Images

Figure CN119082618A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of crawler steel, and in particular to crawler steel capable of reducing corner cracks, a production process thereof, and quality inspection equipment thereof. Background Art
[0002] Track steel is mainly used to make track chains of track-type excavators, and is often used to make track chains of large excavators. It is used in mining of stone, coal, metal ores, etc. The construction conditions are harsh, and the strength, wear resistance and toughness requirements are high, and the size requirements are strict. Therefore, the size of the track steel needs to be tested by a detection device before leaving the factory.
[0003] For example, Chinese patent CN220818815U discloses a hot-rolled track steel measuring device, including a ruler and a slidable reading sliding block, one end of the ruler is provided with a fixed claw perpendicular to the ruler, the sliding block is provided with a movable claw perpendicular to the ruler, and two or more positioning claws with the same height and perpendicular to the ruler are provided on the ruler between the fixed claw and the movable claw. When used for measuring the width of the track steel, the bottom surface of the web of the track steel is overlapped with the end surface of the positioning claw, so that the web and the ruler are guaranteed to be parallel, so that the inner end surfaces of the fixed claw and the movable claw are perpendicular and tightly attached to the outer ends of the long teeth and short teeth of the track steel, and the reading is read through the vernier scale and the main scale after the reading sliding block is fixed, so that the width of the double-tooth track steel can be conveniently and quickly measured.
[0004] Although the above patent can quickly measure the width of the track steel, it cannot accurately measure the height of the track steel teeth, nor can it measure the inclination angle of the teeth. Therefore, it is impossible to detect whether the track steel teeth meet the standards through the above patent. Therefore, the anti-skid effect of the track steel may be affected due to the teeth not meeting the standards.
[0005] Based on this, the present invention designs a track steel with reduced corner cracking, a production process and a quality inspection equipment thereof to solve the above problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a track steel capable of reducing corner cracks, a production process thereof, and a quality inspection device thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A track steel for reducing corner cracking, the track steel comprising the following components in weight percentage: C: 0.17-0.19%, Mn: 0.80-1.40%, Mo: 0.13-0.22%, Zn: 0.08-0.16%, Cr: 0.15-0.27%, V: 0.07-0.12%, nano-Si 3 N 4Ceramic powder: 0.004-0.008%, the balance is Fe and unavoidable impurities;
[0009] Furthermore, the nano-Si 3 N 4 The particle size of ceramic powder is 20-50nm.
[0010] A production process of track steel with reduced corner cracking includes the following steps: smelting, adding nano-Si into the LF furnace 3 N 4 Ceramic powder refining, continuous casting, billet heating, controlled rolling, cooling, and quality inspection by quality inspection equipment.
[0011] A quality inspection device for the production process of the track steel with reduced corner cracking, comprising a frame;
[0012] The upper end of the frame is connected with a moving assembly for moving left and right to facilitate the detection of crawler steel placed at different positions;
[0013] The front end of the moving assembly is connected to a plurality of first detection assemblies for accurately measuring the height of the teeth of the track steel;
[0014] The upper end of the frame is connected to a plurality of second detection components for measuring the inclination angle of the teeth of the crawler steel;
[0015] The first detection assembly includes a third guide rail, a second electric slider, a first connection block, a resistance block and a connecting rod, the front end of the moving assembly is connected to the third guide rail, the second electric slider is limitedly slidably connected to the third guide rail, the front end of the second electric slider is fixedly connected to the first connection block, the lower end of the first connection block is fixedly connected to the connecting rod, and the lower end of the connecting rod is fixedly connected to the resistance block;
[0016] The upper end of the first connecting block is fixedly connected to a cross bar, and the front end of the moving assembly is connected to a limiting rod for cooperating with the limiting cross bar;
[0017] The second detection component includes a fixed plate, a fourth guide rail, a second connecting block, a third connecting block and a trapezoidal interference block. The front end of the movable component is connected to the fixed plate, the front end of the fixed plate is fixedly connected to the fourth guide rail which is symmetrical on both sides, the fourth guide rails are all inclined, the second connecting blocks are all limitedly slidably connected to the fourth guide rails, the front ends of the second connecting blocks are fixedly connected to the third connecting blocks, and the ends of the third connecting blocks close to each other are fixedly connected to the trapezoidal interference blocks.
[0018] Furthermore, a testing platform is fixedly connected to the upper end of the frame, and the track steel is placed on the testing platform.
[0019] Furthermore, the moving assembly includes a first guide rail, a threaded rod, a motor, a slider, a second guide rail, a first electric slider and a connecting plate. The upper end of the frame is fixedly connected to the first guide rail, the middle part of the first guide rail is rotatably connected to the threaded rod, the right side of the first guide rail is fixedly connected to the motor, the output end of the motor is fixedly connected to the threaded rod, the upper limit sliding connection of the first guide rail is a slider, the slider is threadedly connected to the threaded rod, the front end of the slider is fixedly connected to the left and right symmetrical second guide rail, the first electric sliders are all limitedly slidably connected to the second guide rail, and the front end of the first electric slider is fixedly connected to the connecting plate.
[0020] Furthermore, the connecting plate is fixedly connected to the third guide rail; the connecting plate is fixedly connected to the fixing plate; and the connecting plate is fixedly connected to the limiting rod.
[0021] Furthermore, displacement sensors are installed on the first electric slider, the second electric slider and the second connecting block.
[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. The track steel is placed on the inspection table, and after the third guide rail and the fixed plate are moved to a suitable position by the moving assembly, the second electric slider moves downward under the limiting guiding action of the third guide rail, and the second electric slider drives the resistance block to move downward through the first connecting block and the connecting rod. When the resistance block contacts the teeth of the track steel, the second electric slider stops moving. At this time, the displacement sensor can calculate the height of the teeth of the track steel according to the distance moved by the second electric slider; when the upper end of the teeth of the track steel is resisted by the resistance block, the second connecting block moves downward under the limiting guiding action of the fourth guide rail. The second connection block moves obliquely downward, and the trapezoidal resistance block drives the third connection block to move obliquely downward. When the trapezoidal resistance block contacts the inclined surface of the track steel tooth, the second connection block stops moving. At this time, the displacement sensor can measure the inclination angle of the track steel tooth according to the distance moved by the second connection block. With the help of the above detection method, the standard of the track steel tooth can be accurately determined to ensure that the tooth details meet the established specifications. This measure fundamentally prevents the problem of anti-skid performance impairment caused by non-compliance with the tooth standard, thereby ensuring the stable performance and safety of the track steel in actual application and avoiding potential risks of use.
[0023] 2. After the track steel is placed on the inspection table, the motor is started, and the output end of the motor drives the threaded rod to rotate, and the threaded rod drives the slider to move left and right. When the resistance block is just above the teeth of the track steel, the motor stops running, so that the resistance block and the trapezoidal resistance block can detect the height and inclination angle of the teeth of the track steel; when the inspection table needs to be cleaned or repaired, the first electric slider moves upward under the limiting guide of the second guide rail, and the first electric slider drives the third guide rail, the resistance block, the fixed plate, and the trapezoidal resistance block to move upward through the connecting plate, so as to increase the distance between the inspection table and the resistance block and the trapezoidal resistance block, so as to facilitate the cleaning or repair of the operating table;
[0024] 3. The present invention adds nano-Si 3 N 4 Ceramic powder refining inhibits the formation of fine second phases such as Al(C,N) by elements such as Al and carbon or nitrogen in steel at high temperatures, which precipitate at austenite grain boundaries, thereby causing stress concentration and leading to embrittlement of the ingot. This fundamentally avoids the ingot defects caused by various stresses during the continuous casting process, especially the appearance of ingot cracks. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 A three-dimensional diagram of a quality inspection device for track steel that reduces corner cracks according to the present invention;
[0027] Figure 2 It is a front view of a quality inspection device for track steel for reducing corner cracks according to the present invention;
[0028] Figure 3 A partial structural diagram of a track steel quality inspection device for reducing corner cracks according to the present invention Figure 1 ;
[0029] Figure 4 A partial structural diagram of a track steel quality inspection device for reducing corner cracks according to the present invention Figure 2 ;
[0030] Figure 5 for Figure 1 The enlarged view of point A in the middle;
[0031] Figure 6 for Figure 3 The enlarged view of point B in the middle;
[0032] Figure 7 for Figure 4 Enlarged view of point C in the middle;
[0033] Figure 8 for Figure 4 The enlarged view of point D in the middle;
[0034] Fig. 9 for Figure 4 Enlarged view of point E in the middle.
[0035] The numbers in the figure represent:
[0036] 1. Frame; 2. Moving assembly; 21. First guide rail; 22. Threaded rod; 23. Motor; 24. Slider; 25. Second guide rail; 26. First electric slider; 27. Connecting plate; 3. First detection assembly; 31. Third guide rail; 32. Second electric slider; 33. First connecting block; 34. Resistance block; 35. Limiting rod; 36. Connecting rod; 4. Second detection assembly; 41. Fixed plate; 42. Fourth guide rail; 43. Second connecting block; 44. Third connecting block; 45. Trapezoidal resistance block. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The terms “left”, “right”, “front”, “back”, “up” and “down” mentioned in the following description are oriented in the viewing direction of the front view.
[0039] Embodiment 1: In some embodiments, please refer to the drawings of the specification Figure 1-Figure 9 , a quality inspection device for track steel with reduced corner cracks, comprising a frame 1;
[0040] The upper end of the frame 1 is connected with a moving assembly 2 for moving left and right to facilitate the detection of crawler steel placed at different positions;
[0041] The front end of the moving assembly 2 is connected to a plurality of first detection assemblies 3 for accurately measuring the height of the teeth of the track steel;
[0042] The upper end of the frame 1 is connected to a plurality of second detection components 4 for measuring the inclination angle of the teeth of the crawler steel;
[0043] The upper end of the frame 1 is fixedly connected to a testing platform, and the track steel is placed on the testing platform;
[0044] The first detection component 3 includes a third guide rail 31, a second electric slider 32, a first connecting block 33, a resisting block 34 and a connecting rod 36. The front end of the moving component 2 is connected to the third guide rail 31, the second electric slider 32 is limitedly slidably connected to the third guide rail 31, the front end of the second electric slider 32 is fixedly connected to the first connecting block 33, the lower end of the first connecting block 33 is fixedly connected to the connecting rod 36, and the lower end of the connecting rod 36 is fixedly connected to the resisting block 34;
[0045] The upper end of the first connecting block 33 is fixedly connected to a cross bar, and the front end of the moving assembly 2 is connected to a limiting rod 35 for cooperating with the limiting cross bar;
[0046] The second detection assembly 4 includes a fixed plate 41, a fourth guide rail 42, a second connection block 43, a third connection block 44 and a trapezoidal abutment block 45. The front end of the moving assembly 2 is connected to the fixed plate 41, the front end of the fixed plate 41 is fixedly connected to the left-right symmetrical fourth guide rail 42, the fourth guide rails 42 are all inclined, the second connection blocks 43 are all limitedly slidably connected to the fourth guide rails 42, the front ends of the second connection blocks 43 are all fixedly connected to the third connection blocks 44, and the ends of the third connection blocks 44 close to each other are fixedly connected to the trapezoidal abutment block 45;
[0047] The track steel is placed on the inspection table, and after the third guide rail 31 and the fixing plate 41 are moved to a suitable position by the moving assembly 2, the second electric slider 32 moves downward under the limiting guiding action of the third guide rail 31, and the second electric slider 32 drives the abutment block 34 to move downward through the first connecting block 33 and the connecting rod 36. When the abutment block 34 abuts against the teeth of the track steel, the second electric slider 32 stops moving. At this time, the displacement sensor can measure the height of the teeth of the track steel according to the distance moved by the second electric slider 32; when the upper end of the teeth of the track steel is abutted by the abutment block 34, , the second connection block 43 moves obliquely downward under the limiting guiding action of the fourth guide rail 42, and the second connection block 43 drives the trapezoidal contact block 45 to move obliquely downward through the third connection block 44. When the trapezoidal contact block 45 contacts the inclined surface of the teeth of the track steel, the second connection block 43 stops moving. At this time, the displacement sensor can measure the inclination angle of the teeth of the track steel according to the moving distance of the second connection block 43; the above detection method can accurately detect whether the teeth of the track steel meet the standards, thereby preventing the anti-skid effect of the track steel from being affected when it is used due to the teeth not meeting the standards;
[0048] The moving assembly 2 includes a first guide rail 21, a threaded rod 22, a motor 23, a slider 24, a second guide rail 25, a first electric slider 26 and a connecting plate 27. The upper end of the frame 1 is fixedly connected to the first guide rail 21, the middle part of the first guide rail 21 is rotatably connected to the threaded rod 22, the right side of the first guide rail 21 is fixedly connected to the motor 23, the output end of the motor 23 is fixedly connected to the threaded rod 22, the first guide rail 21 is slidingly connected to the slider 24 in an upper limit position, the slider 24 is threadedly connected to the threaded rod 22, the front end of the slider 24 is fixedly connected to the left-right symmetrical second guide rail 25, the first electric slider 26 is slidingly connected to the second guide rail 25 in a limited position, and the front end of the first electric slider 26 is fixedly connected to the connecting plate 27;
[0049] The connecting plate 27 is fixedly connected to the third guide rail 31; the connecting plate 27 is fixedly connected to the fixing plate 41; the connecting plate 27 is fixedly connected to the limiting rod 35;
[0050] The first electric slider 26, the second electric slider 32, and the second connecting block 43 are all equipped with displacement sensors;
[0051] When the track steel is placed on the testing platform, the motor 23 is started, and the output end of the motor 23 drives the threaded rod 22 to rotate, and the threaded rod 22 drives the slider 24 to move left and right. When the resistance block 34 is just above the teeth of the track steel, the motor 23 stops running, so that the resistance block 34 and the trapezoidal resistance block 45 can detect the height and inclination angle of the teeth of the track steel; when the testing platform needs to be cleaned or repaired, the first electric slider 26 moves upward under the limiting and guiding action of the second guide rail 25, and the first electric slider 26 drives the third guide rail 31, the resistance block 34, the fixed plate 41, and the trapezoidal resistance block 45 to move upward through the connecting plate 27, thereby increasing the distance between the testing platform and the resistance block 34 and the trapezoidal resistance block 45, so as to facilitate the cleaning or repair of the operating table.
[0052] Embodiment 2: This embodiment provides a production process for track steel with reduced corner cracking, comprising the following steps:
[0053] (1) Putting C powder, Mn powder, Mo powder, Zn powder, Cr powder, V powder and Fe powder into a smelting furnace for smelting;
[0054] (2) Transfer to LF furnace and add nano-Si with a particle size of 50 nm 3 N 4 Ceramic powder refining;
[0055] (3) Continuous casting;
[0056] (4) Heating the ingot: heating the ingot to 1150°C at a rate of 5°C / min;
[0057] (5) Controlled rolling; high-pressure water dephosphorization, water pressure 20Mpa; rolling temperature controlled at 1250℃;
[0058] (6) Cooling: reducing the temperature to below 650°C;
[0059] (7) Through quality inspection by the quality inspection equipment described in Example 1, qualified track steel with reduced corner cracks is obtained.
[0060] The track steel contains 0.17-0.19% C, 0.80-1.40% Mn, 0.13-0.22% Mo, 0.08-0.16% Zn, 0.15-0.27% Cr, 0.07-0.12% V, and nano-Si 3 N 4 Ceramic powder: 0.004-0.008%, the balance being Fe and unavoidable impurities.
[0061] Embodiment 3: This embodiment provides a production process for track steel with reduced corner cracking, comprising the following steps:
[0062] (1) Putting C powder, Mn powder, Mo powder, Zn powder, Cr powder, V powder and Fe powder into a smelting furnace for smelting;
[0063] (2) Transfer to the LF furnace and add nano-Si with a particle size of 20 nm 3 N 4 Ceramic powder refining;
[0064] (3) Continuous casting;
[0065] (4) Heating the ingot: heating the ingot to 1150°C at a rate of 5°C / min;
[0066] (5) Controlled rolling; high-pressure water dephosphorization, water pressure 20Mpa; rolling temperature controlled at 1250℃;
[0067] (6) Cooling: reducing the temperature to below 650°C;
[0068] (7) Through quality inspection by the quality inspection equipment described in Example 1, qualified track steel with reduced corner cracks is obtained.
[0069] Embodiment 4: This embodiment provides a production process for track steel with reduced corner cracking, comprising the following steps:
[0070] (1) Putting C powder, Mn powder, Mo powder, Zn powder, Cr powder, V powder and Fe powder into a smelting furnace for smelting;
[0071] (2) Transfer to LF furnace and add nano-Si with a particle size of 30 nm 3 N 4 Ceramic powder refining;
[0072] (3) Continuous casting;
[0073] (4) Heating the ingot: heating the ingot to 1150°C at a rate of 5°C / min;
[0074] (5) Controlled rolling; high-pressure water dephosphorization, water pressure 20Mpa; rolling temperature controlled at 1250℃;
[0075] (6) Cooling: reducing the temperature to below 650°C;
[0076] (7) Through quality inspection by the quality inspection equipment described in Example 1, qualified track steel with reduced corner cracks is obtained.
[0077] Comparative Example 1: The difference from Example 4 is that no nano-Si is added in this comparative example. 3 N 4 Ceramic powder;
[0078] This embodiment provides a production process for track steel with reduced corner cracking, comprising the following steps:
[0079] (1) Putting C powder, Mn powder, Mo powder, Zn powder, Cr powder, V powder and Fe powder into a smelting furnace for smelting;
[0080] (2) Transfer to LF furnace for refining;
[0081] (3) Continuous casting;
[0082] (4) Heating the ingot: heating the ingot to 1150°C at a rate of 5°C / min;
[0083] (5) Controlled rolling; high-pressure water dephosphorization, water pressure 20Mpa; rolling temperature controlled at 1250℃;
[0084] (6) Cooling: reducing the temperature to below 650°C;
[0085] (7) Through quality inspection by the quality inspection equipment described in Example 1, qualified track steel with reduced corner cracks is obtained.
[0086] Comparative Example 2: The difference from Example 4 is that the nano-Si 3 N 4 The particle size of ceramic powder is 80nm;
[0087] This embodiment provides a production process for track steel with reduced corner cracking, comprising the following steps:
[0088] (1) Putting C powder, Mn powder, Mo powder, Zn powder, Cr powder, V powder and Fe powder into a smelting furnace for smelting;
[0089] (2) Transfer to LF furnace and add nano-Si with particle size of 20-50nm 3 N 4 Ceramic powder refining;
[0090] (3) Continuous casting;
[0091] (4) Heating the ingot: heating the ingot to 1150°C at a rate of 5°C / min;
[0092] (5) Controlled rolling; high-pressure water dephosphorization, water pressure 20Mpa; rolling temperature controlled at 1250℃;
[0093] (6) Cooling: reducing the temperature to below 650°C;
[0094] (7) Through quality inspection by the quality inspection equipment described in Example 1, qualified track steel with reduced corner cracks is obtained.
[0095] Experimental Example: The tensile strength of the track steels obtained in Example 2, Example 3, Example 4, Comparative Example 1 and Comparative Example 2 was tested according to GB / T 10423-2002 standard, and the results are as follows:
[0096] Detect the cross-sectional shrinkage rate. The cross-sectional shrinkage rate is the ratio of the cross-sectional area reduction to the original area when the material breaks under tension.
[0097] Sectional reduction rate = (S0-S1) / S0×100%, where S0 represents the original cross-sectional area and S1 represents the cross-sectional area after fracture;
[0098] project Embodiment 2 Embodiment 3 Embodiment 4 Comparative Example 1 Comparative Example 2 Tensile strength (MPa 695 674 691 689 678 Sectional shrinkage (% 74.32 68.49 71.86 47.54 59.87
[0099] When the cross-sectional shrinkage exceeds 60%, the continuous casting billet has sufficient plasticity at this temperature and will not produce cracks;
[0100] The present invention adds nano-Si with a particle size of 20-50nm 3 N 4 Ceramic powder refining inhibits the formation of fine second phases such as Al(C,N) by elements such as Al and carbon or nitrogen in steel at high temperatures, which precipitate at austenite grain boundaries, thereby causing stress concentration and leading to embrittlement of the ingot. This fundamentally avoids the ingot defects caused by various stresses during the continuous casting process, especially the appearance of ingot cracks.
[0101] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A track steel for reducing corner cracks, characterized in that: The track steel includes the following components in weight percentage: C: 0.17-0.19%, Mn: 0.80-1.40%, Mo: 0.13-0.22%, Zn: 0.08-0.16%, Cr: 0.15-0.27%, V: 0.07-0.12%, nano Si3N4 ceramic powder: 0.004-0.008%, and the balance is Fe and inevitable impurities.
2. The crawler steel with reduced corner cracking according to claim 1, characterized in that: The nano Si3N4 ceramic powder has a particle size of 20-50 nm.
3. A production process for track steel with reduced corner cracking as claimed in claim 1 or claim 2, characterized in that: The following steps are involved: Smelting, adding nano-Si3N4 ceramic powder into LF furnace for refining, continuous casting, heating of ingot, controlled rolling, cooling, and quality inspection by quality inspection equipment.
4. A quality inspection device for the production process of crawler steel with reduced corner cracking as claimed in claim 3, characterized in that: comprising a frame (1); The upper end of the frame (1) is connected to a moving component (2) for moving left and right to facilitate detection of crawler steel placed at different positions; The front end of the moving component (2) is connected to a plurality of first detection components (3) for accurately measuring the height of the teeth of the crawler steel; The upper end of the frame (1) is connected to a plurality of second detection components (4) for measuring the inclination angle of the teeth of the crawler steel; The first detection component (3) comprises a third guide rail (31), a second electric slider (32), a first connecting block (33), a contact block (34) and a connecting rod (36); the front end of the moving component (2) is connected to the third guide rail (31); the second electric slider (32) is connected to the third guide rail (31) in a limited sliding manner; the front end of the second electric slider (32) is fixedly connected to the first connecting block (33); the lower end of the first connecting block (33) is fixedly connected to the connecting rod (36); and the lower end of the connecting rod (36) is fixedly connected to the contact block (34); The upper end of the first connecting block (33) is fixedly connected to a cross bar, and the front end of the moving assembly (2) is connected to a limiting rod (35) for cooperating with the limiting cross bar; The second detection component (4) comprises a fixed plate (41), a fourth guide rail (42), a second connection block (43), a third connection block (44) and a trapezoidal abutment block (45); the front end of the moving component (2) is connected to the fixed plate (41); the front end of the fixed plate (41) is fixedly connected to a left-right symmetrical fourth guide rail (42); the fourth guide rails (42) are all inclined; the second connection blocks (43) are all limitedly slidably connected to the fourth guide rails (42); the front ends of the second connection blocks (43) are fixedly connected to the third connection blocks (44); and the ends of the third connection blocks (44) that are close to each other are fixedly connected to the trapezoidal abutment block (45).
5. The track steel with reduced corner cracking, its production process and its quality inspection equipment according to claim 4, characterized in that: The upper end of the frame (1) is fixedly connected to a testing platform, and the track steel is placed on the testing platform.
6. The track steel with reduced corner cracking, its production process and its quality inspection equipment according to claim 5, characterized in that: The moving assembly (2) comprises a first guide rail (21), a threaded rod (22), a motor (23), a slider (24), a second guide rail (25), a first electric slider (26) and a connecting plate (27); the upper end of the frame (1) is fixedly connected to the first guide rail (21); the middle of the first guide rail (21) is rotatably connected to the threaded rod (22); the right side of the first guide rail (21) is fixedly connected to the motor (23); the output end of the motor (23) is fixedly connected to the threaded rod (22); the first guide rail (21) is upper limit slidingly connected to the slider (24); the slider (24) is threadedly connected to the threaded rod (22); the front end of the slider (24) is fixedly connected to the second guide rail (25) symmetrically on the left and right; the first electric slider (26) is limitedly slidably connected to the second guide rail (25); and the front end of the first electric slider (26) is fixedly connected to the connecting plate (27).
7. The track steel with reduced corner cracking, its production process and its quality inspection equipment according to claim 6, characterized in that: The connecting plate (27) is fixedly connected to the third guide rail (31); the connecting plate (27) is fixedly connected to the fixing plate (41); and the connecting plate (27) is fixedly connected to the limiting rod (35).