Cast aluminum bronze alloy and heat treatment method thereof

Through solid solution treatment and tempering treatment of ZCuAl9Fe4Ni4Mn2 castings, appropriate combination and structural structure are formed, the problem of insufficient mechanical properties of aluminum bronze materials is solved, the tensile strength and hardness are improved, and the high requirements of seawater pump impellers are met. Improves the comprehensive mechanical properties of the product.

CN119082632APending Publication Date: 2024-12-06CHONGQING HONGJIANG MACHINERY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210898.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Conventional cast aluminum bronze materials cannot meet the high requirements of seawater pump impellers in terms of mechanical properties, especially the tensile strength, yield limit and elongation. The elongation after alloy element optimization and heat treatment is low, so it cannot meet seawater corrosion and brittleness. question.

Method used

ZCuAl9Fe4Ni4Mn2 casting blank was used for solid solution treatment and quenching, followed by tempering treatment, and α-Cu phase, K phase and β'(Cu3Al) phase structure was formed through solid solution diffusion and rapid cooling, and then tempered at 450-550°C. , precipitate fine KⅢ phases, eliminate quenching stress, and improve the elongation and mechanical properties of the material.

Benefits of technology

On the basis of ensuring elongation, the tensile strength and hardness of aluminum bronze alloy are significantly improved, which meets the mechanical performance requirements of seawater pump impellers and improves the operating reliability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082632A_ABST
    Figure CN119082632A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal heat treatment, in particular to a cast aluminum bronze alloy and a heat treatment method thereof.The heat treatment method comprises the following steps that firstly, a ZCuAl9Fe4Ni4Mn2 casting blank is provided; secondly, solution treatment is conducted, specifically, the casting blank is subjected to heat preservation for 1.5-3.0 h under the condition that the temperature ranges from 860 DEG C to 950 DEG C, and then quenching is conducted to the room temperature; and thirdly, tempering treatment is conducted, specifically, the quenched casting blank is subjected to heat preservation for 1.5-2.5 h under the condition that the temperature ranges from 450 DEG C to 550 DEG C, cooling is conducted, and the cast aluminum bronze alloy is obtained. On the premise of ensuring the ductility, the yield strength and hardness of the alloy can be improved, so that the alloy has relatively high comprehensive mechanical properties, and the operation reliability of a product is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal heat treatment, and in particular to a cast aluminum bronze alloy and a heat treatment method thereof. Background Art

[0002] Cast aluminum bronze ZCuAl9Fe4Ni4Mn2 is a common cast aluminum bronze material in GB / T1176 "Casting Copper and Copper Alloys" standard. It has high strength and hardness, good wear resistance, corrosion resistance, and high air tightness. It is mainly used to manufacture propellers, water pump impellers, turbines, flanges, pipe fittings, etc. The mechanical properties of this material under conventional casting conditions are: tensile strength Rm = 640 ~ 710MPa, yield limit Rp 0.2 =250~300MPa, elongation A5≥16%, hardness 160~206HB.

[0003] As a key component, the seawater pump impeller has a large operating load and requires the following mechanical properties: tensile strength Rm ≥ 720MPa, yield strength Rp 0.2 ≥400MPa, elongation A5≥8%, hardness≥210HB. The performance of impeller materials produced by conventional methods cannot meet the requirements. If the mechanical properties are insufficient during use, the service life of the entire water pump will be shortened and the expected design requirements will not be met.

[0004] Through the optimization of alloy elements, the mechanical properties of the cast state still cannot meet the requirements. Adding more than 10.5% Al will increase the yield strength of the alloy to more than 400 MPa, but the elongation of the material is low, resulting in increased brittleness and decreased seawater corrosion resistance.

[0005] According to GB / T1176 "Casting Copper and Copper Alloys" standard ZCuAl9Fe4Ni4Mn2 materials are all used in the casting state. Foreign research on improving the mechanical properties of aluminum bronze by heat treatment started early. In recent years, domestic researchers have conducted more research, including the quenching + secondary aging method based on nickel aluminum bronze profiles to improve the strength and hardness of bronze. Shanghai Jiaotong University studied QAl10-4-4 aluminum bronze bars through single-phase solid solution + two-phase regulation + low-temperature aging + medium-temperature tempering heat treatment, which greatly improved the alloy strength and obtained ultra-high strength aluminum bronze material, but its elongation is low and cannot meet the mechanical properties requirements of seawater pump impellers. Summary of the invention

[0006] The purpose of the present invention is to provide a cast aluminum bronze alloy and a heat treatment method thereof, which can improve the yield strength and hardness of the alloy under the premise of ensuring the elongation, so that the alloy has higher comprehensive mechanical properties and improves the operating reliability of the product.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] In a first aspect, the present invention provides a method for heat treatment of a cast aluminum bronze alloy, comprising the following steps:

[0009] Step 1, providing ZCuAl9Fe4Ni4Mn2 casting blank;

[0010] Step 2: solution treatment, keeping the casting blank at a temperature of 860-950°C for 1.5-3.0h, and then quenching to room temperature;

[0011] Step three, tempering treatment, keeping the quenched casting blank at a temperature of 450-550° C. for 1.5-2.5 hours, and cooling to obtain a cast aluminum bronze alloy.

[0012] Furthermore, in terms of weight percentage, the ZCuAl9Fe4Ni4Mn2 casting blank in step one comprises the following components: 9.2-10.5% Al, 4.0-5.0% Fe, 4.0-5.0% Ni, 0.8-2.5% Mn, and the remainder Cu.

[0013] Furthermore, in terms of weight percentage, the ZCuAl9Fe4Ni4Mn2 casting blank in step one comprises the following components: 9.8-10.5% Al, 4.2-4.6% Fe, 4.2-4.7% Ni, 1.0-1.7% Mn, and the remainder Cu.

[0014] Furthermore, the quenching medium in step 2 includes quenching oil or water with a temperature of 60 to 80°C.

[0015] Furthermore, the cooling in step three includes: after the tempering treatment is completed, cooling to 200-300° C. in the furnace, and then air cooling to room temperature after being taken out of the furnace.

[0016] In a second aspect, the present invention provides a cast aluminum bronze alloy, which is obtained by using the above-mentioned heat treatment method for cast aluminum bronze alloy.

[0017] The present invention has the following unexpected beneficial effects: the present invention adopts sufficient solid solution diffusion and then rapid cooling, and the structure is mainly composed of α-Cu phase, K phase and β' (Cu3Al) phase, wherein the K phase is an intermetallic compound composed of Fe, Ni and Al, which can be further divided into K Ⅰ ~K ⅣPhase. The strength and hardness of the material are high but the elongation is insufficient. Finally, the tempering treatment is carried out, that is, the temperature is kept at 450-550℃ for 1.5-2h, so that the unstable phase in the material structure is fully precipitated and the quenching stress is eliminated. During tempering, the structural changes of the alloy mainly occur in the original β phase area, and the small flakes of nickel-rich K Ⅲ phase precipitates from the supersaturated β'(Cu3Al) phase and transforms into (α+K Ⅲ ) eutectoid, K Ⅲ The phases are dispersed, and the material maintains a high strength while the elongation is improved. Through the above heat treatment, the aluminum bronze alloy maintains sufficient elongation, and the tensile strength and hardness of the aluminum bronze alloy are improved, so that the alloy has higher comprehensive mechanical properties, meets the product's requirements for mechanical properties, and improves the product's operating reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A flow chart of a heat treatment method for a cast aluminum bronze alloy provided in an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0019] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0020] In one embodiment, see Figure 1 As shown, a heat treatment method for a cast aluminum bronze alloy is provided, which comprises the following steps:

[0021] Step 1: Provide ZCuAl9Fe4Ni4Mn2 casting blank.

[0022] Step 2: Solution treatment: keep the casting blank at 860-950°C for 1.5-3.0h, and then quench it to room temperature. During solution treatment, alloy elements (such as Fe, Al, etc.) are fully dissolved in the Cu matrix to form a uniform solid solution, which helps to eliminate segregation and defects in the original cast state. It is then rapidly cooled to room temperature by quenching, so that the high-temperature phase (such as β' phase) in the alloy does not have time to transform into a stable phase and is retained in the room temperature structure. This non-equilibrium structure usually has higher hardness and strength, but lower elongation because rapid cooling leads to the formation of internal stress and brittle phases.

[0023] Step three, tempering treatment, keeping the quenched casting blank at a temperature of 450-550° C. for 1.5-2.5 hours, and cooling to obtain a cast aluminum bronze alloy.

[0024] The main purpose of tempering treatment is to decompose the unstable phase (such as supersaturated β' phase) produced after quenching through appropriate temperature and time control, and precipitate fine K Ⅲ phase, while eliminating or reducing quenching stress, thereby improving the plasticity and toughness of the material while maintaining high strength and hardness.

[0025] At the tempering temperature of 450-550℃, the fine K Ⅲ The phase precipitates from the supersaturated β' phase and forms a eutectic with the α phase (α+K Ⅲ This structural transformation not only refines the grains, but also makes the strengthening phase (K Ⅲ Phase) is dispersed in the matrix, effectively hindering dislocation movement and grain boundary sliding, thereby enhancing the strength and hardness of the material. At the same time, due to the release of quenching stress and the softening of the structure caused by phase transformation, the elongation of the material is also improved.

[0026] Through the above heat treatment, the tensile strength and hardness of the cast aluminum-bronze alloy are improved while maintaining sufficient elongation, so that the alloy has higher comprehensive mechanical properties, meets the product's requirements for mechanical properties, and improves the product's operating reliability.

[0027] In a preferred embodiment, the ZCuAl9Fe4Ni4Mn2 casting blank in step one comprises the following components by weight percentage: 9.2-10.5% Al, 4.0-5.0% Fe, 4.0-5.0% Ni, 0.8-2.5% Mn, and the remainder Cu.

[0028] Aluminum (Al) is the main alloying element in the alloy. The addition of aluminum can significantly improve the strength and hardness of the alloy, while reducing electrical conductivity and thermal conductivity. In aluminum bronze alloys, aluminum forms a variety of intermetallic compound phases with copper, such as CuAl2 (θ phase) and Cu3Al (β' phase or β phase variant at high temperature). The presence of these phases has an important influence on the mechanical properties of the alloy.

[0029] Iron (Fe) plays a major role in aluminum bronze alloys in improving wear resistance and corrosion resistance. Iron interacts with aluminum and copper to form some complex intermetallic compounds, such as Fe3Al2 (K phase), which usually have higher hardness and wear resistance.

[0030] The addition of nickel (Ni) can improve the strength and toughness of aluminum bronze alloys, and enhance their fatigue resistance and stress corrosion cracking resistance. Nickel can also promote phase transformation and microstructure refinement of the alloy during heat treatment, thereby further improving the mechanical properties of the alloy.

[0031] Manganese (Mn) is mainly used as a deoxidizer and grain refiner in aluminum bronze. It helps to eliminate oxide inclusions in the alloy, improve the purity and casting properties of the alloy. At the same time, manganese can also promote grain refinement during the solidification process of the alloy, thereby improving the mechanical properties and processing properties of the alloy.

[0032] Copper (Cu) is the basis of alloy strength and toughness. In aluminum bronze alloys, copper interacts with other alloying elements to form various intermetallic compound phases, which together determine the mechanical properties of aluminum bronze alloys.

[0033] Furthermore, the ZCuAl9Fe4Ni4Mn2 casting blank in step one comprises the following components by weight percentage: 9.8-10.5% Al, 4.2-4.6% Fe, 4.2-4.7% Ni, 1.0-1.7% Mn, and the remainder Cu.

[0034] The preferred ZCuAl9Fe4Ni4Mn2 casting blank chemical composition range is more precise, aiming to further optimize the mechanical properties, corrosion resistance, wear resistance and processability of the alloy by strictly controlling the content of each alloy element. In practical applications, it is also necessary to combine specific casting processes and heat treatment processes to further adjust and optimize the performance of the alloy.

[0035] In a preferred embodiment, the quenching medium in step 2 includes quenching oil or water with a temperature of 60-80°C.

[0036] Quenching oil usually has a lower cooling rate than water, which helps reduce the thermal and structural stresses generated during the quenching process, thereby reducing the risk of cracking and deformation of the workpiece. In addition, quenching oil can maintain stable cooling characteristics at high temperatures and is not prone to steam film effect, thus ensuring that the workpiece can be evenly cooled throughout the quenching process. Quenching oil can also handle workpieces with complex shapes and large cross-sections.

[0037] As a natural resource, water is widely available and inexpensive, which greatly reduces the cost of the quenching process. Water is an efficient cooling medium that can quickly remove heat from the surface of the workpiece, thereby shortening the quenching time and improving production efficiency. Water as a quenching medium does not produce harmful substances and is environmentally friendly.

[0038] If the workpiece has a small cross-sectional size and a simple shape, water can be used as the quenching medium. However, if the workpiece has a large cross-sectional size or a complex shape, it is recommended to use quenching oil to reduce the risk of cracking and deformation.

[0039] If water is chosen as the quenching medium, the water temperature should be strictly controlled between 60 and 80 ° C. Water in this temperature range can maintain a certain cooling rate and reduce the influence of the steam film effect.

[0040] Before quenching, the workpiece can be pre-cooled to lower its initial temperature, thereby reducing thermal stress and structural stress during quenching.

[0041] After quenching, the workpiece should be tempered in time to eliminate internal stress and improve toughness. At the same time, it should also be cleaned and rust-proofed to ensure the quality and service life of the workpiece.

[0042] In a preferred embodiment, the cooling in step 3 includes: cooling to 200-300° C. in the furnace after the tempering treatment is completed, and then cooling to room temperature in the air after being taken out of the furnace.

[0043] Furnace cooling can promote the continued decomposition of a small amount of unconverted unstable phases under high temperature, thus improving the mechanical properties of the material. Furnace cooling can further release internal stress and prevent cracks in the workpiece due to rapid cooling. It should be noted that the speed of furnace cooling should be moderate. Too fast or too slow may affect the final performance of the workpiece. When the furnace temperature drops below 200°C, the phases in the material structure have solidified and will not change with temperature, and then the material is air-cooled after being taken out of the furnace to increase the cooling rate and reduce the processing time.

[0044] In another embodiment, a cast aluminum bronze alloy is provided, wherein the cast aluminum bronze alloy is obtained by processing the heat treatment method for the cast aluminum bronze alloy described in any one of the above-mentioned embodiments.

[0045] The following is an explanation with reference to specific examples.

[0046] Embodiment 1, a heat treatment method for a cast aluminum bronze alloy, comprising the following steps:

[0047] Step 1: Provide ZCuAl9Fe4Ni4Mn2 casting blank.

[0048] The ZCuAl9Fe4Ni4Mn2 casting blank comprises the following components by weight percentage: 10.43% Al, 4.24% Fe, 4.42% Ni, 1.08% Mn, and the balance Cu.

[0049] The raw materials are weighed according to the component proportion of the ZCuAl9Fe4Ni4Mn2 casting blank, and the weighed raw materials are placed in a furnace for heating and melting. After the components are melted, the temperature is raised to 1280±5°C to make the components of the alloy uniform, and after refining and slagging, the alloy is left to stand for 5 to 10 minutes, and then the alloy is taken out of the furnace for casting at a temperature of 1200 to 1250°C to obtain a ZCuAl9Fe4Ni4Mn2 casting blank.

[0050] Step 2: Solution treatment: the casting blank is kept at 860°C for 2.0h, then quenched in water at 80°C, and rapidly cooled to room temperature.

[0051] Step three, tempering treatment, keeping the quenched casting blank at a temperature of 450° C. for 1.5 hours, taking it out of the furnace and air cooling it to obtain a cast aluminum bronze alloy.

[0052] Embodiment 2, a heat treatment method for a cast aluminum bronze alloy, comprising the following steps:

[0053] Step 1: Provide ZCuAl9Fe4Ni4Mn2 casting blank.

[0054] The ZCuAl9Fe4Ni4Mn2 casting blank comprises the following components by weight percentage: 9.85% Al, 4.42% Fe, 4.66% Ni, 1.63% Mn, and the balance Cu.

[0055] The raw materials are weighed according to the component proportion of the ZCuAl9Fe4Ni4Mn2 casting blank, and the weighed raw materials are placed in a furnace for heating and melting. After the components are melted, the temperature is raised to 1280±5°C to make the components of the alloy uniform, and after refining and slagging, the alloy is left to stand for 5 to 10 minutes, and then the alloy is taken out of the furnace for casting at a temperature of 1200 to 1250°C to obtain a ZCuAl9Fe4Ni4Mn2 casting blank.

[0056] Step 2: Solution treatment: the casting is kept at 900°C for 2.0h, then quenched in quenching oil and rapidly cooled to room temperature.

[0057] Step three, tempering treatment, the quenched casting blank is kept at a temperature of 550° C. for 2.0 h, cooled to 300° C. in the furnace, and then air-cooled to obtain a cast aluminum bronze alloy.

[0058] Embodiment 3, a heat treatment method for a cast aluminum bronze alloy, comprising the following steps:

[0059] Step 1: Provide ZCuAl9Fe4Ni4Mn2 casting blank.

[0060] The ZCuAl9Fe4Ni4Mn2 casting blank comprises the following components by weight percentage: 9.21% Al, 4.40% Fe, 4.28% Ni, 1.41% Mn, and the balance Cu.

[0061] The raw materials are weighed according to the component proportion of the ZCuAl9Fe4Ni4Mn2 casting blank, and the weighed raw materials are placed in a furnace for heating and melting. After the components are melted, the temperature is raised to 1280±5°C to make the components of the alloy uniform, and after refining and slagging, the alloy is left to stand for 5 to 10 minutes, and then the alloy is taken out of the furnace for casting at a temperature of 1200 to 1250°C to obtain a ZCuAl9Fe4Ni4Mn2 casting blank.

[0062] Step 2: Solution treatment: the casting blank is kept at 950°C for 2.0h, then quenched in water at 80°C, and rapidly cooled to room temperature.

[0063] Step three, tempering treatment, the quenched casting blank is kept at a temperature of 500° C. for 1.5 hours, cooled to 260° C. in the furnace, and then air-cooled to obtain a cast aluminum bronze alloy.

[0064] Embodiment 4, a heat treatment method for a cast aluminum bronze alloy, comprising the following steps:

[0065] Step 1: Provide ZCuAl9Fe4Ni4Mn2 casting blank.

[0066] The ZCuAl9Fe4Ni4Mn2 casting blank comprises the following components by weight percentage: 9.96% Al, 4.54% Fe, 4.43% Ni, 1.00% Mn, and the balance Cu.

[0067] The raw materials are weighed according to the component proportion of the ZCuAl9Fe4Ni4Mn2 casting blank, and the weighed raw materials are placed in a furnace for heating and melting. After the components are melted, the temperature is raised to 1280±5°C to make the components of the alloy uniform, and after refining and slagging, the alloy is left to stand for 5 to 10 minutes, and then the alloy is taken out of the furnace for casting at a temperature of 1200 to 1250°C to obtain a ZCuAl9Fe4Ni4Mn2 casting blank.

[0068] Step 2: Solution treatment: the casting blank is kept at 880°C for 2.0h, then quenched in water at 80°C, and rapidly cooled to room temperature.

[0069] Step three, tempering treatment, the quenched casting blank is kept at a temperature of 530° C. for 2.5 hours, cooled to 200° C. in the furnace, and then air-cooled to obtain a cast aluminum bronze alloy.

[0070] The mechanical properties of the cast aluminum bronze alloys obtained in Examples 1 to 4 were tested, and the test results are shown in Table 1.

[0071] Table 1 Mechanical properties of cast aluminum bronze alloy

[0072]

[0073] It can be seen from Table 1 that the various mechanical properties of the cast aluminum bronze alloy obtained in Example 1 to Example 4 can meet the mechanical property requirements of the seawater pump impeller. Based on ZCuAl9Fe4Ni4Mn2 of GB / T1176, the present invention slightly increases the weight percentage of aluminum element on the one hand to generate more strengthening phases and improve the tensile strength and yield strength of the alloy material. On the other hand, by reasonably setting the process flow and parameter conditions of the heat treatment method, through sufficient solid solution diffusion and then rapid cooling, the structure is mainly composed of α-Cu phase, K phase and β' (Cu3Al) phase, and the grains are refined at the same time. The strength and hardness of the material are relatively high, but the elongation is insufficient. Finally, tempering treatment is carried out, that is, the temperature is kept at 450-550℃ for 1.5-2h, so that the unstable phase in the material structure is fully precipitated, and the quenching stress is eliminated at the same time. The structural changes of the alloy during tempering mainly occur in the original β phase region, and the fine K Ⅲ phase precipitates from the supersaturated β'(Cu3Al) phase and transforms into (α+K Ⅲ ) eutectoid, the strengthening phase is dispersed, the material maintains a high strength while the elongation is improved. Through the above heat treatment, the aluminum bronze alloy maintains sufficient elongation, and the tensile strength and hardness of the aluminum bronze alloy are improved, so that the alloy has higher comprehensive mechanical properties, meets the product's requirements for mechanical properties, and improves the product's operational reliability.

[0074] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A heat treatment method for a cast aluminum bronze alloy, characterized in that: The steps include: Step 1, providing ZCuAl9Fe4Ni4Mn2 casting blank; Step 2: Solution treatment: keep the casting blank at 860-950°C for 1.5-3.0h, and then quench to room temperature; Step three, tempering treatment, keeping the quenched casting blank at a temperature of 450-550° C. for 1.5-2.5 hours, and cooling to obtain a cast aluminum bronze alloy.

2. The heat treatment method of cast aluminum bronze alloy according to claim 1, characterized in that: In terms of weight percentage, the ZCuAl9Fe4Ni4Mn2 casting blank in the step 1 comprises the following components: 9.2-10.5% Al, 4.0-5.0% Fe, 4.0-5.0% Ni, 0.8-2.5% Mn, and the balance is Cu.

3. The heat treatment method of cast aluminum bronze alloy according to claim 2, characterized in that: In terms of weight percentage, the ZCuAl9Fe4Ni4Mn2 casting blank in the step 1 comprises the following components: 9.8-10.5% Al, 4.2-4.6% Fe, 4.2-4.7% Ni, 1.0-1.7% Mn, and the remainder Cu.

4. The heat treatment method of cast aluminum bronze alloy according to claim 1, characterized in that: The quenching medium in step 2 includes quenching oil or water with a temperature of 60-80°C.

5. The heat treatment method of cast aluminum bronze alloy according to claim 1, characterized in that: The cooling in step 3 includes: after the tempering treatment is completed, cooling to 200-300° C. in the furnace, and then air cooling to room temperature after being taken out of the furnace.

6. A cast aluminum bronze alloy, characterized in that: The cast aluminum bronze alloy is obtained by treating the cast aluminum bronze alloy using the heat treatment method according to any one of claims 1 to 5.