TiN-based thin film for ferroelectric device, ferroelectric structure and preparation method and application of TiN-based thin film
By using plasma enhanced atomic layer deposition technology on the substrate to deposit TiN-based film and perform high-temperature annealing, and then depositing a ferroelectric layer on it, the problems of perovskite ferroelectric film in miniaturization and integration are solved, and the problems of perovskite ferroelectric films are improved. ferroelectricity and device performance.
Patent Information
- Application Number
- CN202411183502.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
AI Technical Summary
The ferroelectricity of traditional perovskite ferroelectric films decreases when their thickness is less than 10nm. The narrow band gap leads to a large leakage current, which is difficult to meet the needs of miniaturization and integration, and the element ratio is difficult to accurately control, affecting the reliability and application of the device.
The TiN-based film is deposited on the substrate by plasma enhanced atomic layer deposition technology (PEALD), and the ferroelectric layer is deposited after high-temperature annealing. The TiN-HfO2-TiN structure is prepared in situ to avoid contamination of interfacial oxygen impurities and enhance iron. Electricity.
The single crystal transformation of TiN-based thin film is realized, the resistivity is reduced, the orthogonal ferroelectricity generation of ferroelectric materials is promoted, and the ferroelectricity of ferroelectric film and the storage capacity and reliability of devices are improved.
Smart Images

Figure CN119082702A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ferroelectric storage, and in particular relates to a TiN-based film for a ferroelectric device, a ferroelectric structure, and a preparation method and application thereof. Background Art
[0002] With the rapid development of my country's electronics industry, traditional perovskite-structured ferroelectric thin film materials (such as lead zirconate titanate (Pb(Zr x Ti 1-x )O3, PZT), strontium bismuth tantalate (SrBi2Ta2O9, SBT), barium titanate (BaTiO3), lead titanate (PbTiO3), etc.) have been extensively studied in semiconductor devices such as low-power non-volatile storage. Among them, PZT materials have been successfully used as ferroelectric memory at the 130nm node. However, the ferroelectricity of perovskite ferroelectric materials will drop sharply or even disappear when the thickness is less than 10nm, and because the band gap of such materials is narrow (Eg ~ 3-4eV), ferroelectric films of nanometer thickness are prone to large leakage currents, which seriously affect the storage capacity and reliability of the device, and thus cannot meet the needs of device miniaturization. Secondly, since Pb and Bi elements are easy to volatilize under high temperature conditions, it is difficult to accurately control the element ratio of multi-component perovskite ferroelectric materials, so it is difficult to meet the current requirements and development direction of large-scale integration of devices, further limiting the application of traditional perovskite ferroelectric films in semiconductor technology.
[0003] Compared with traditional perovskite ferroelectric films, the new hafnium oxide (HfO2)-based ferroelectric film is compatible with complementary metal oxide semiconductor (CMOS) technology, has strong ferroelectricity at a thickness of less than 10nm, and has advantages such as simple element composition and environmental friendliness. It can achieve polarization reversal under a small bias voltage, has low energy consumption, and can to a certain extent solve the problems of miniaturization and integration that are difficult to overcome in traditional perovskite ferroelectric films. In particular, doped HfO2 can obtain multifunctional properties such as dielectric, ferroelectric and antiferroelectric properties through performance regulation, and has a very excellent competitive advantage in ferroelectric film materials within a hundred nanometers.
[0004] At present, the methods for depositing HfO2 are usually pulsed laser deposition (PLD), sol-gel method (Sol-Gel), magnetron sputtering (Sputter) and atomic layer deposition technology (ALD). Different preparation methods and preparation conditions will cause differences in the structure and properties of HfO2 films. In addition, in the preparation process of ferroelectric devices, sputtering technology is usually used to prepare the upper and lower electrodes. For example, in 2011, Germany et al. first used sputtered titanium nitride (TiN) as the upper and lower electrodes and used atomic layer deposition (ALD) technology to prepare a 10nm HfO2 film doped with silicon (Si). The study found that under the clamping of TiN electrodes, the doped HfO2 film showed obvious ferroelectricity after annealing, and the residual polarization intensity (Pr) could reach 10μC·cm -2 . After that, many studies on HfO2 thin films were carried out at home and abroad. At present, sputtering technology is still commonly used to prepare TiN electrodes, and ALD technology is used to prepare HfO2 thin films. These two technologies are combined to prepare TiN-HfO2-TiN structure. However, this non-in-situ preparation of TiN-HfO2-TiN structure is prone to oxygen impurity contamination at the interface, which affects the ferroelectricity of HfO2 thin films to a certain extent. In addition, the TiN prepared by sputtering has poor crystallinity, which is not conducive to the subsequent formation of a ferroelectric layer on TiN. Summary of the invention
[0005] In order to solve all or part of the above technical problems, the present invention provides the following technical solutions:
[0006] One of the purposes of the present invention is to provide a method for preparing a TiN-based thin film for a ferroelectric device, comprising:
[0007] Depositing a TiN-based precursor film on a substrate using plasma enhanced atomic layer deposition technology, wherein the substrate has a hexagonal crystal structure and the material of the TiN-based precursor film includes TiN;
[0008] Under inert atmosphere conditions, the TiN-based precursor film is subjected to a first annealing treatment to obtain a TiN-based film.
[0009] The present invention uses plasma enhanced atomic layer deposition (PEALD) technology to deposit TiN, and performs high temperature annealing after deposition, which can promote the transformation of TiN from polycrystalline to single crystal, and significantly reduce the resistivity; and subsequently depositing a ferroelectric layer on the TiN-based film can promote the generation of orthogonal ferroelectricity of the ferroelectric material. The first annealing treatment is, for example, in-situ annealing performed in a PEALD device.
[0010] In some embodiments, the process conditions for depositing the TiN-based precursor film include: using the Plasma mode in the plasma enhanced atomic layer deposition technology, setting the RF power to 2500W~2800W, the growth temperature to 300℃~400℃, the deposition rate to 0.03nm / cycle~0.038nm / cycle, the pulse time of the titanium source in each cycle to 0.1s~1s, and the pulse time of the nitrogen source to 5s~10s.
[0011] In some embodiments, the titanium source includes TiCl4; the nitrogen source includes NH3 and / or N2.
[0012] In some embodiments, the substrate includes sapphire or Si.
[0013] In some embodiments, the temperature of the first annealing treatment is 900° C. to 1200° C. Annealing within this temperature range can significantly reduce the resistivity of the TiN-based thin film, and in some embodiments, can reduce it to less than 100 μΩ·cm.
[0014] In some embodiments, the first annealing treatment takes 2 minutes to 6 minutes.
[0015] In some embodiments, before depositing the TiN-based precursor film on the substrate, the substrate is further subjected to plasma treatment using N2 and / or NH3. The beneficial effect of pre-plasma treatment using N3 and / or NH3 is that nitrogen plasma treats the surface of the substrate under high temperature and low pressure conditions, thereby reducing C and O impurities in the substrate and the TiN film, increasing surface activity, and increasing the density of the film.
[0016] In some embodiments, the process conditions for plasma treatment of the substrate with N2 and / or NH3 include: setting the RF power to 2500W-2800W, the N2 and / or NH3 pulse time to 30-120s, and the treatment time to 5-10min.
[0017] In some embodiments, before depositing the TiN-based precursor film on the substrate, the method further includes cleaning and / or baking the substrate.
[0018] In some embodiments, the cleaning includes cleaning the substrate with an organic solvent and an inorganic solvent. The organic solvent includes, for example, acetone, isopropanol, etc., but is not limited thereto; in some embodiments, a mixed solvent of an organic solvent and water may also be used. The inorganic solvent includes, for example, sulfuric acid, hydrogen peroxide, an etching solution (BOE) mixed in proportion by an aqueous hydrofluoric acid solution (HF) and an aqueous ammonium fluoride solution (NH4F), etc., but is not limited thereto.
[0019] A second object of the present invention is to provide a TiN-based thin film for ferroelectric devices prepared by the method described in any of the above technical solutions.
[0020] A third object of the present invention is to provide a PEALD in-situ preparation method for a ferroelectric structure, comprising:
[0021] A TiN-based thin film is prepared by the method described in any one of the above technical solutions to form a first electrode;
[0022] In-situ depositing a ferroelectric layer and a second electrode on the first electrode using plasma enhanced atomic layer deposition technology to obtain a precursor structure;
[0023] Under inert atmosphere conditions, the precursor structure is subjected to a second annealing treatment to obtain a ferroelectric structure.
[0024] According to the above, high-temperature annealing of TiN and then depositing the ferroelectric layer can help improve the ferroelectricity of the ferroelectric material. In addition, the methods of preparing TiN and ferroelectric films (such as HZO) in the prior art all adopt non-in-situ growth technology. This non-in-situ growth technology is difficult to avoid the pollution of nitrogen, carbon and oxygen impurities caused by the exposure of different film layers to the air atmosphere during the transfer process, resulting in an increase in the concentration of oxygen impurities at the interface between TiN and the ferroelectric layer, affecting the ferroelectricity of the device; the present invention uses PEALD technology to prepare a sandwich structure of the first electrode-ferroelectric layer-second electrode at one time through in-situ growth, avoiding the interface air pollution problem caused by traditional non-in-situ epitaxy, reducing the oxygen impurity concentration at the interface, and thus further improving the ferroelectricity of the ferroelectric film. The second annealing treatment can be an in-situ annealing performed in a PEALD device.
[0025] In some embodiments, the ferroelectric material contained in the ferroelectric layer includes HZO (hafnium zirconium oxide, Hf x Zr 1-x O2), at least one of HfO2, and ZrO2.
[0026] In some preferred embodiments, the ferroelectric material contained in the ferroelectric layer includes HZO, especially HZO ferroelectric material. HZO is a material with a high dielectric constant, having a variety of crystal orientation structures such as tetragonal phase (t phase), orthorhombic phase (m phase), orthorhombic phase (o phase), etc., and its specific structure depends on the temperature and pressure of the external environment; the o phase has ferroelectricity, and the formation of the o phase is related to the doping of Zr elements and the stress under the clamping of the upper and lower electrodes; the HZO deposited on the TiN crystal structure after high-temperature rapid thermal annealing in the present invention is conducive to the formation of the HZO orthorhombic ferroelectric phase, and the PEALD in-situ growth method can reduce the oxygen impurity concentration at the interface, further improving the ferroelectricity of the HZO film.
[0027] In some embodiments, the thickness of the ferroelectric layer is 6 nm to 10 nm.
[0028] In some embodiments, the process conditions for in-situ deposition of the ferroelectric layer on the first electrode include: using a thermal growth mode of plasma enhanced atomic layer deposition technology, setting the growth temperature to 200°C to 300°C, the pulse time of the ferroelectric material metal source in each cycle to 1.2s to 1.8s, the pulse time of the oxygen source to 0.1s to 0.5s, and the deposition rate to 0.089nm / cycle to 0.11nm / cycle.
[0029] In some embodiments, the material of the second electrode includes TiN.
[0030] In some embodiments, the thickness of the second electrode is 10 nm to 50 nm.
[0031] In some embodiments, the process conditions for depositing the second electrode include: setting the RF power to 2500W~2800W, the growth temperature to 300℃~400℃, the deposition rate to 0.03nm / cycle~0.038nm / cycle, the pulse time of the titanium source in each cycle to 0.1s~1s, and the pulse time of the nitrogen source to 5s~10s.
[0032] In some embodiments, the temperature of the second annealing treatment is 450°C to 600°C.
[0033] In some embodiments, the second annealing treatment lasts for 30s to 60s.
[0034] In some embodiments, the PEALD in-situ preparation method of the ferroelectric structure further includes: setting a dielectric layer between the first electrode or the second electrode and the ferroelectric layer; and / or forming a plurality of the ferroelectric layers on the first electrode and setting a dielectric layer between two of the ferroelectric layers.
[0035] In some preferred embodiments, the method includes: forming a plurality of ferroelectric layers on the first electrode, and arranging a dielectric layer between two of the ferroelectric layers. The device formed by arranging the dielectric layer between the two ferroelectric layers has a smaller leakage current.
[0036] In some embodiments, it specifically includes using plasma enhanced atomic layer deposition technology to in-situ deposit a dielectric layer between two ferroelectric layers or between the first electrode or the second electrode and the ferroelectric layer until the precursor structure is formed, and then performing the second annealing treatment.
[0037] In some embodiments, the material of the dielectric layer includes SiO 2 and / or Al 2 O 3 .
[0038] In some embodiments, the process conditions for depositing the SiO2 dielectric layer include: setting the RF power to 2500w-2800w, the growth temperature to 200℃-300℃, the deposition rate to 0.06nm / cycle~0.09nm / cycle, the pulse time of the silicon source to 0.1s~6s in each cycle, and the pulse time of the oxygen source to 0.1s~0.3s.
[0039] In some embodiments, the process conditions for depositing the Al2O3 dielectric layer include: a growth temperature of 200°C-300°C, a deposition rate of 0.06-0.09nm / cycle, a pulse time of the aluminum source of 0.1s-6s in each cycle, and a pulse time of the oxygen source of 0.1s-0.3s.
[0040] In some embodiments, the dielectric layer has a thickness of 1-2 nm.
[0041] In some typical embodiments, the PEALD in-situ preparation method of the ferroelectric structure comprises the following steps:
[0042] The sapphire or Si substrate is ultrasonically cleaned with acetone, isopropanol and deionized water in sequence to remove organic contamination on the substrate surface; then the substrate is cleaned with H2SO4, H2O2 and BOE solution in sequence to remove the natural oxide layer on the substrate surface;
[0043] The cleaned substrate is introduced into the vacuum chamber of PEALD, where it is first baked in situ and then treated with N2 / NH3-Plasma for 5-10 minutes.
[0044] Performing epitaxy of TiN on the substrate treated as above, and performing an in-situ first annealing treatment on the obtained TiN film;
[0045] Then epitaxy of HZO and top TiN films is performed in sequence to obtain a sandwich structure;
[0046] The obtained sandwich structure is subjected to an in-situ second annealing treatment to obtain a ferroelectric structure.
[0047] A fourth object of the present invention is to provide a ferroelectric structure obtained by the preparation method described in any of the above technical solutions.
[0048] In some typical embodiments, the ferroelectric structure is TiN-HZO-TiN, TiN-HfO2-TiN, TiN-ZrO2-TiN, TiN-HZO-Al2O3-HZO-TiN, TiN-Al2O3-HZO-TiN, TiN-HZO-Al2O3-TiN, TiN-HZO-SiO2-HZO-TiN, TiN-SiO2-HZO-TiN or TiN-HZO-SiO2-TiN.
[0049] A fifth object of the present invention is to provide a ferroelectric device, comprising the TiN-based thin film described in any of the above technical solutions or the ferroelectric structure described.
[0050] In some embodiments, the ferroelectric device includes a ferroelectric capacitor, a ferroelectric memory device, etc.
[0051] Compared with the prior art, the present invention has at least the following beneficial effects:
[0052] (1) The present invention adopts PEALD technology to perform epitaxy of TiN on a substrate and anneal it after the deposition, thereby promoting the transformation of TiN into a hexagonal structure, and the resistivity of TiN after high-temperature annealing is significantly reduced. The ferroelectric layer is further deposited on the TiN, which is conducive to the generation of orthogonal ferroelectricity of the ferroelectric material, and solves the problem that the TiN prepared by the existing sputtering method has poor crystallinity and is not conducive to the subsequent growth of the ferroelectric layer;
[0053] (2) The present invention adopts PEALD technology to in-situ prepare the ferroelectric structure of the present invention. The deposition of different film structures is carried out in a PEALD device without the need for transfer operations, thereby reducing the oxygen impurity concentration at the film interface and further improving the ferroelectricity.
[0054] (3) Furthermore, the present invention has found that the leakage current of the device obtained by providing a dielectric layer in the ferroelectric structure, especially providing a dielectric layer between two ferroelectric layers, is small. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0056] Figure 1a is the XRD diagram of TiN deposited on the sapphire substrate after annealing in Examples 1 to 5 of the present invention;
[0057] Figure 1b The XRD patterns of TiN without annealing (W / O annealing) and after annealing at 450°C, 550°C, 650°C, 750°C, 850°C, 950°C, and 1050°C for 30s in Comparative Example 1 of the present invention;
[0058] Figure 1c is an AFM image of TiN after annealing in Example 5 of the present invention;
[0059] Figure 1d is a graph showing the relationship between the resistivity and annealing temperature of TiN after annealing in Examples 1 to 5 of the present invention;
[0060] Figure 2 is a schematic diagram of a process for preparing a ferroelectric structure in one embodiment of the present invention;
[0061] Figure 3ais the XRD spectrum of the TiN-HZO-TiN structure prepared in Examples 8 to 10 of the present invention before and after annealing;
[0062] Figure 3b is an AFM image of the first TiN in Example 8 of the present invention;
[0063] Figure 3c is a SEM image of a cross section of the TiN-HZO-TiN structure prepared in Example 8 of the present invention;
[0064] Figure 4 It is a schematic diagram of detecting the TiN-HZO-TiN sandwich structure in Example 8 of the present invention. DETAILED DESCRIPTION
[0065] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention. The specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0066] Unless otherwise specified, the raw materials and reagents used in the present invention are all commercially available.
[0067] Example 1
[0068] This embodiment provides a TiN film and a method for preparing the TiN film by plasma enhanced atomic layer deposition, which is as follows:
[0069] First, the sapphire substrate was cleaned organically and inorganically. The sapphire was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 (volume ratio) for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 (volume ratio) for 3 minutes, and then blown dry with a nitrogen gun;
[0070] The treated sapphire substrate was transferred to the vacuum chamber of a plasma enhanced atomic layer deposition device (PEALD), and the growth parameters were set as follows: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to clear the remaining chlorine in the chamber; the RF power was 2600W, the growth temperature was 400℃, and the deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle to obtain a TiN precursor film;
[0071] After the cycle is completed, the prepared TiN precursor film is subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 950°C for 2 minutes to obtain a TiN film.
[0072] Embodiments 2 to 5
[0073] The difference between Examples 2 to 5 and Example 1 is that the annealing temperatures for the rapid thermal annealing of the TiN precursor film are different, namely 1000° C., 1050° C., 1100° C., and 1150° C., respectively, and the annealing time is 2 minutes. The rest is the same as Example 1.
[0074] Figure 1a 1 is the XRD diagram of TiN on sapphire after the recession in Examples 1 to 5. Figure 1c This is an AFM image of TiN in Example 5 after annealing. Figure 1d 3 is a graph showing the relationship between the resistivity of TiN and the annealing temperature in Examples 1 to 5.
[0075] Example 6
[0076] The only difference between Example 6 and Example 1 is that before growing TiN on the sapphire substrate, the cleaned sapphire substrate is first subjected to in-situ plasma treatment with N2. The specific process parameters of the in-situ plasma treatment are: RF power 2500W, N2 pulse time 120s, and treatment time 5min.
[0077] Example 7
[0078] The only difference between Example 7 and Example 1 is that before growing TiN on the sapphire substrate, the cleaned sapphire substrate is first subjected to in-situ plasma treatment with NH3. The specific process parameters of the in-situ plasma treatment are: RF power 2800W, NH3 pulse time 120s, and treatment time 10min.
[0079] Compared with Example 1, Examples 6 and 7 first use NH3 / N2 to perform in-situ plasma treatment on the cleaned sapphire substrate, and then grow TiN, which can clean the substrate and reduce C and O impurities in the substrate, increase surface activity, and further increase the density of the film.
[0080] Example 8
[0081] This embodiment provides a TiN-HZO-TiN structure and a method for in-situ preparing the structure using PEALD. Figure 2 It is a schematic flow diagram of the preparation process of this embodiment, which is as follows:
[0082] First, the Si substrate was cleaned organically and inorganically. The Si substrate was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 for 3 minutes, and then dried with a nitrogen gun;
[0083] The treated Si wafer was transferred to the vacuum chamber of PEALD, and the first TiN layer was grown. The growth parameters were set as follows: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to purge the remaining chlorine in the chamber; RF power was 2500W, growth temperature was 300℃, and deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached to obtain the first TiN precursor film;
[0084] After the cycle is completed, the first TiN precursor film is subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 950° C. for 2 min to obtain a first TiN layer.
[0085] Then, a HZO layer is grown in situ on the first TiN layer, using TMAHf as the hafnium source and H2O as the oxygen source. The pulse time of TMAHf is 1.6s, the pulse time of H2O is 0.1s, and 50% Zr element is doped. The growth temperature is 200°C and the deposition rate is about 0.1nm / cycle to obtain the HZO layer.
[0086] Then, a second TiN layer was grown in situ on the HZO layer, and the growth parameters were set: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to purge the remaining chlorine in the chamber; the RF power was 2500W, the growth temperature was 300°C, and the deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached to obtain the second TiN layer;
[0087] The prepared TiN-HZO-TiN precursor structure was subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 450°C for 30 seconds to obtain a TiN-HZO-TiN ferroelectric structure in which the thickness of TiN was 50 nm and the thickness of HZO was 10 nm.
[0088] The prepared TiN-HZO-TiN sandwich structure was subjected to photolithography and etching. The first and second TiN layers of the device were pierced using a ferroelectric analyzer and a high-voltage and high-current probe station. The 2Pr of the device could reach 40μC / cm 2 , Ec is about 1.5MV / cm, and the leakage current is 10 -6A. The testing process is as follows Figure 4 shown.
[0089] Embodiments 9-10
[0090] The only difference between Examples 9 and 10 and Example 8 is that the annealing temperatures for the rapid thermal annealing treatment of the prepared TiN-HZO-TiN precursor structure are 500° C. and 550° C. respectively, and the rest is implemented in the same way as Example 8, and the obtained effects are equivalent to those of Example 8.
[0091] Figure 3a It is the XRD spectrum of the TiN-HZO-TiN structure prepared in Examples 8 to 10 before and after annealing. Figure 3b This is an AFM image of the first TiN in Example 8. Figure 3c This is a SEM image of the cross section of the TiN-HZO-TiN structure prepared in Example 8.
[0092] Embodiment 11
[0093] This embodiment provides a TiN-HfO2-TiN structure and a method for in-situ preparing the structure using PEALD, which is as follows:
[0094] First, the Si substrate was cleaned organically and inorganically. The Si substrate was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 for 3 minutes, and then dried with a nitrogen gun;
[0095] The treated Si wafer was transferred to the vacuum chamber of PEALD, and the first TiN layer was grown. The growth parameters were set as follows: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to clear the remaining chlorine in the chamber; the RF power was 2800W, the growth temperature was 400℃, and the deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached, thus obtaining the first TiN precursor film;
[0096] After the cycle is completed, the first TiN precursor film is subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 900°C for 6 minutes to obtain a first TiN layer;
[0097] Then, a HfO2 layer was in-situ grown on the first TiN layer, using TMAHf as the hafnium source and H2O as the oxygen source, with a pulse time of TMAHf of 1.6 s, a pulse time of H2O of 0.1 s, a growth temperature of 300°C, and a deposition rate of 0.1 nm / cycle to obtain the HfO2 layer;
[0098] Then, a second TiN layer was grown in situ on the HfO2 layer, and the growth parameters were set: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to purge the remaining chlorine in the chamber; the RF power was 2800W, the growth temperature was 400°C, and the deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached to obtain the second TiN layer;
[0099] The prepared TiN-HfO2-TiN precursor structure was subjected to a rapid thermal annealing treatment in a N2 atmosphere at a temperature of 600°C for 30 seconds to obtain a TiN-HfO2-TiN ferroelectric structure in which TiN was 50 nm and HfO2 was 10 nm.
[0100] XRD, AFM and SEM tests were performed on it, and the results were equivalent to those of Examples 8 to 10.
[0101] Example 12
[0102] This embodiment provides a TiN-ZrO2-TiN structure and a method for in-situ preparing the structure using PEALD, which is as follows:
[0103] First, the Si substrate was cleaned organically and inorganically. The Si substrate was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 for 3 minutes, and then blown dry with a nitrogen gun;
[0104] The treated Si wafer was transferred to the vacuum chamber of PEALD, and the first TiN layer was grown first. The growth parameters were set: TICl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to clear the remaining chlorine in the chamber; the RF power was 2500W, the growth temperature was 300℃, and the deposition rate was about 0.038nm / cycle; in each cycle, the pulse time of TICl4 was 0.1s, the pulse time of NH3 was 5s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached, thus obtaining the first TiN precursor film;
[0105] After the cycle is completed, the first TiN precursor film is subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 950° C. for 2 min to obtain a first TiN layer.
[0106] Then, a ZrO2 layer was in-situ grown on the first TiN layer, using TMAZr as the zirconium source and H2O as the oxygen source. The pulse time of TMAZr was 1.4 s, the pulse time of H2O was 0.3 s, the growth temperature was 250°C, and the deposition rate was 0.1 nm / cycle, resulting in a ZrO2 layer with a thickness of 10 nm.
[0107] Then, a second TiN layer was grown in situ on the ZrO2 layer, and the growth parameters were set: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to purge the remaining chlorine in the chamber; the RF power was 2500W, the growth temperature was 300°C, and the deposition rate was about 0.038nm / cycle; in each cycle, the pulse time of TiCl4 was 0.1s, the pulse time of NH3 was 5s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached to obtain the second TiN layer;
[0108] The prepared TiN-ZrO2-TiN precursor structure was subjected to a rapid thermal annealing treatment in a N2 atmosphere at a temperature of 500°C for 30 seconds to obtain a TiN-ZrO2-TiN ferroelectric structure in which TiN was 50 nm and ZrO2 was 10 nm.
[0109] XRD, AFM and SEM tests were performed on it, and the results were equivalent to those of Examples 8 to 10.
[0110] Example 13
[0111] This embodiment provides a TiN-HZO-Al2O3-HZO-TiN structure, which uses a PEALD in-situ method to prepare the structure, as follows:
[0112] First, the Si substrate was cleaned organically and inorganically. The Si substrate was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 for 3 minutes, and then blown dry with a nitrogen gun;
[0113] The treated Si wafer was transferred to the vacuum chamber of PEALD, and the first TiN layer was grown. The growth parameters were set as follows: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to purge the remaining chlorine in the chamber; RF power was 2600W, growth temperature was 350℃, and deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached, thus obtaining the first TiN precursor film;
[0114] After the cycle is completed, the first TiN precursor film is subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 1100° C. for 4 min to obtain a first TiN layer.
[0115] Then, the first HZO layer is in-situ grown on the first TiN layer, using TMAHf as the hafnium source and H2O as the oxygen source, with a pulse time of 1.6 s for TMAHf and a pulse time of 0.1 s for H2O, and 50% of Zr element is doped, the growth temperature is 300°C, and the deposition rate is about 0.1 nm / cycle, to obtain the first HZO layer;
[0116] Then, an Al2O3 dielectric layer is in-situ grown on the first HZO layer, with TMAl as the Al source and H2O as the oxygen source. The pulse time of TMAl is 0.1s, the pulse time of H2O is 0.1s, the growth temperature is 300°C, and the deposition rate is about 0.089nm / cycle, to obtain an Al2O3 dielectric layer.
[0117] Then, a second HZO layer is in-situ grown on the Al2O3 dielectric layer according to the same process parameters as the first HZO layer; and a second TiN layer is in-situ grown on the second HZO layer according to the same process parameters as the first TiN layer, to obtain a TiN-HZO-Al2O3-HZO-TiN precursor structure;
[0118] In a N2 atmosphere, the TiN-HZO-Al2O3-HZO-TiN precursor structure prepared above was subjected to rapid thermal annealing treatment at an annealing temperature of 550°C and an annealing time of 30s to obtain a TiN (50nm) -HZO (5nm) -Al2O3 (2nm) -HZO (5nm) -TiN (50nm) ferroelectric structure.
[0119] Embodiment 14
[0120] This embodiment provides a ferroelectric structure of TiN (50nm) -Al2O3 (2nm) -HZO (10nm) -TiN (50nm), and the process parameters for depositing TiN, Al2O3, and HZO are the same as those in Example 13, with the only difference being that the first TiN, Al2O3 dielectric layer, HZO layer, and second TiN layer are deposited in sequence according to the ferroelectric structure of this embodiment.
[0121] Embodiment 15
[0122] This embodiment provides a ferroelectric structure of TiN (50nm) -HZO (10nm) -Al2O3 (2nm) -TiN (50nm), and the process parameters for depositing TiN, Al2O3, and HZO are the same as those in Example 13, with the only difference being that the first TiN layer, the HZO layer, the Al2O3 dielectric layer, and the second TiN layer are deposited in sequence according to the ferroelectric structure of this embodiment.
[0123] Compared with the ferroelectric structure without an Al2O3 dielectric layer, the devices obtained in Examples 13, 14, and 15 have smaller overall leakage and better performance; and, by comparing Examples 13 to 15, it is found that the leakage of the device obtained in Example 13 in which the Al2O3 dielectric layer is set between two ferroelectric layers is at the nA level, and the breakdown voltage is 8V.
[0124] Example 16
[0125] This embodiment provides a TiN-HZO-SiO2-HZO-TiN structure and a method for in-situ preparing the structure using PEALD, which is as follows:
[0126] First, the Si substrate was cleaned organically and inorganically. The Si substrate was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 for 3 minutes, and then blown dry with a nitrogen gun;
[0127] The treated Si wafer was transferred to the vacuum chamber of PEALD, and the first TiN layer was grown. The growth parameters were set as follows: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to clear the remaining chlorine in the chamber; RF power was 2600W, growth temperature was 350℃, and deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached, thus obtaining the first TiN precursor film;
[0128] After the cycle is completed, the first TiN precursor film is subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 950° C. for 2 min to obtain a first TiN layer.
[0129] Then, the first HZO layer is in-situ grown on the first TiN layer, using TMAHf as the hafnium source, H2O as the oxygen source, the pulse time of TMAHf is 1.6s, the pulse time of H2O is 0.1s, and 50% of Zr element is doped, the growth temperature is 300°C, and the deposition rate is about 0.1nm / cycle, to obtain the first HZO layer;
[0130] Then, a SiO2 dielectric layer was in-situ grown on the first HZO layer, using 3DMAS as a Si source and O2 as an oxygen source. The pulse time of 3DMAS was 6 s, the pulse time of O2 was 0.3 s, the growth temperature was 300°C, and the deposition rate was about 0.06 nm / cycle, to obtain a SiO2 dielectric layer.
[0131] Then, a second HZO layer is in-situ grown on the SiO2 dielectric layer according to the same process parameters as the first HZO layer; and a second TiN layer is in-situ grown on the second HZO layer according to the same process parameters as the first TiN layer, to obtain a TiN-HZO-SiO2-HZO-TiN precursor structure;
[0132] In a N2 atmosphere, the TiN-HZO-SiO2-HZO-TiN precursor structure prepared above was subjected to rapid thermal annealing at an annealing temperature of 450°C-600°C and an annealing time of 30s to obtain a TiN (50nm) -HZO (5nm) -SiO2 (2nm) -HZO (5nm) -TiN (50nm) ferroelectric structure.
[0133] XRD, AFM and SEM tests were performed on it, and the results were equivalent to those of Examples 8 to 10.
[0134] Embodiment 17
[0135] This embodiment provides a ferroelectric structure of TiN (50nm) -SiO2 (2nm) -HZO (10nm) -TiN (50nm), and the process parameters for depositing TiN, SiO2, and HZO are the same as those in Example 16, with the only difference being that the first TiN layer, SiO2 dielectric layer, HZO layer, and second TiN layer are deposited in sequence according to the ferroelectric structure of this embodiment.
[0136] Embodiment 18
[0137] This embodiment provides a ferroelectric structure of TiN (50nm) -HZO (10nm) -SiO2 (2nm) -TiN (50nm), and the process parameters for depositing TiN, SiO2, and HZO are the same as those in Example 16, with the only difference being that the first TiN layer, the HZO layer, the SiO2 dielectric layer, and the second TiN layer are deposited in sequence according to the ferroelectric structure of this embodiment.
[0138] Compared with the ferroelectric structure without the Al2O3 dielectric layer, the devices obtained in Examples 16, 17, and 18 have smaller overall leakage and better performance; and, by comparing Examples 16 to 18, it is found that the device obtained in Example 16 in which the SiO2 dielectric layer is set between the two ferroelectric layers has even smaller leakage.
[0139] Comparative Example 1
[0140] The only difference between Comparative Example 1 and Example 8 is that the first TiN precursor film deposited on the Si substrate is not subjected to thermal annealing. The specific preparation process is as follows:
[0141] First, the Si substrate was cleaned organically and inorganically. The Si substrate was ultrasonically cleaned with acetone, isopropanol and deionized water for 10 minutes respectively, then immersed in a solution of concentrated H2SO4:H2O2=7:3 for 10 minutes, immersed in a mixed solution of NH4F:HF=20:1 for 3 minutes, and then dried with a nitrogen gun;
[0142] The processed Si wafer was transferred to the vacuum chamber of PEALD, and the first TiN layer was grown first. The growth parameters were set: TICl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to clear the remaining chlorine in the chamber; RF power was 2500W, growth temperature was 300℃, and deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TICl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached to obtain the first TiN layer;
[0143] Then, a HZO layer is grown in situ on the first TiN layer, using TMAHf as the hafnium source and H2O as the oxygen source. The pulse time of TMAHf is 1.6s, the pulse time of H2O is 0.1s, and 50% Zr element is doped. The growth temperature is 200°C and the deposition rate is about 0.1nm / cycle to obtain the HZO layer.
[0144] Then, a second TiN layer was grown in situ on the HZO layer, and the growth parameters were set: TiCl4 was used as the Ti source, NH3 was used as the nitrogen source, and H2 was used to purge the remaining chlorine in the chamber; the RF power was 2500W, the growth temperature was 300°C, and the deposition rate was about 0.033nm / cycle; in each cycle, the pulse time of TiCl4 was 0.5s, the pulse time of NH3 was 7s, and H2 was purged for 2s before entering the next cycle until the set thickness was reached to obtain the second TiN layer;
[0145] The prepared TiN-HZO-TiN precursor structure was subjected to rapid thermal annealing in a N2 atmosphere at a temperature of 450°C for 30 seconds to obtain a TiN-HZO-TiN ferroelectric structure in which the thickness of TiN was 50 nm and the thickness of HZO was 10 nm.
[0146] Comparing Example 8 with Comparative Example 1, the annealed TiN is closer to crystalline TiN, has a lower resistivity, and the HZO grown thereon has better quality.
[0147] In addition, the present invention also tests the effects of TiN film annealing treatment conditions of 450°C-30s, 550°C-30s, 650°C-30s, 750°C-30s, 850°C-30s, 950°C-30s, and 1050°C-30s. Figure 1bThe XRD pattern of TiN annealed under these conditions is shown, and it is found that the effect of TiN transforming into single crystal under these annealing conditions is not good, and the effect of reducing resistivity is not significant. It can be seen that the effect is better when the annealing temperature is 1050°C and the annealing time is more than 2 minutes.
[0148] Comparative Example 2
[0149] Comparative Example 2 uses the sputtering method in the prior art to form a first TiN layer on a Si substrate, and then deposits a HZO layer and a second TiN layer on the first TiN layer in sequence according to the PEALD technology of the present invention. Due to the pollution of nitrogen, carbon and oxygen impurities caused by exposure to air atmosphere during the transfer process, the oxygen impurity concentration at the interface between TiN and the ferroelectric layer increases, and the leakage current of the device increases.
[0150] The present invention also performs performance testing on the obtained ferroelectric device, and the testing structure is shown in Table 1.
[0151] Table 1 Partial device performance of ferroelectric structures of relevant embodiments and comparative examples
[0152]
[0153]
[0154] In summary, the present invention prepares TiN in PEALD, performs high-temperature annealing after TiN deposition to promote the transformation of TiN crystal orientation to hexagonal, and then performs epitaxy of hexagonal HZO. This preparation method greatly promotes the generation of HZO orthogonal ferroelectricity; and the present invention proposes a growth method of in-situ preparation of ferroelectric structure using PEALD technology, avoiding the pollution of nitrogen, carbon and oxygen impurities in the air caused by different epitaxial methods, playing a role in reducing the concentration of oxygen impurities at the interface, and further improving ferroelectricity.
[0155] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0156] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0157] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made without departing from the spirit and scope of the present invention and that the elements of the embodiments may be replaced by substantial equivalents. In addition, many modifications may be made without departing from the scope of the present invention to adapt specific circumstances or materials to the teachings of the present invention. Therefore, it is not intended herein to limit the present invention to the disclosed specific embodiments for performing the present invention, but it is intended that the present invention will include all embodiments within the scope of the appended claims. In addition, unless specifically stated, any use of the terms first, second, etc. does not indicate any order or importance, but rather uses the terms first, second, etc. to distinguish one element from another.
Claims
1. A method for preparing a TiN-based thin film for a ferroelectric device, characterized in that: include: Depositing a TiN-based precursor film on a substrate using plasma enhanced atomic layer deposition technology, wherein the substrate has a hexagonal crystal structure and the material of the TiN-based precursor film includes TiN; Under inert atmosphere conditions, the TiN-based precursor film is subjected to a first annealing treatment to obtain a TiN-based film.
2. The method for preparing a TiN-based thin film for a ferroelectric device according to claim 1, characterized in that: The process conditions for depositing the TiN-based precursor film include: using the Plasma mode in the plasma enhanced atomic layer deposition technology, setting the RF power to 2500W to 2800W, the growth temperature to 300°C to 400°C, the deposition rate to 0.03 to 0.038nm / cycle, the pulse time of the titanium source to 0.1s to 1s in each cycle, and the pulse time of the nitrogen source to 5s to 10s.
3. The method for preparing a TiN-based thin film for a ferroelectric device according to claim 2, wherein: The titanium source includes TiCl4; the nitrogen source includes NH3 and / or N2.
4. The method for preparing a TiN-based thin film for a ferroelectric device according to claim 1, wherein: The substrate comprises sapphire or Si; And / or, the temperature of the first annealing treatment is 900° C. to 1200° C., and / or, the time of the first annealing treatment is 2 min to 6 min.
5. The method for preparing a TiN-based thin film for a ferroelectric device according to claim 1, wherein: Before depositing the TiN-based precursor film on the substrate, the method further comprises subjecting the substrate to plasma treatment using N2 and / or NH3; And / or, before depositing the TiN-based precursor film on the substrate, the method further includes cleaning and / or baking the substrate.
6. A TiN-based thin film for ferroelectric devices prepared by the method according to any one of claims 1 to 5.
7. A PEALD in-situ preparation method for a ferroelectric structure, characterized in that: include: A TiN-based thin film is prepared by the method described in any one of claims 1 to 5 to form a first electrode; In-situ depositing a ferroelectric layer and a second electrode on the first electrode using plasma enhanced atomic layer deposition technology to obtain a precursor structure; Under inert atmosphere conditions, the precursor structure is subjected to a second annealing treatment to obtain a ferroelectric structure.
8. The PEALD in-situ preparation method of a ferroelectric structure according to claim 7, characterized in that: The ferroelectric material contained in the ferroelectric layer includes at least one of HZO, HfO2, and ZrO2; And / or, the thickness of the ferroelectric layer is 6 to 10 nm; And / or, the process conditions for in-situ deposition of the ferroelectric layer on the first electrode include: using a thermal growth mode of plasma enhanced atomic layer deposition technology, setting the growth temperature to 200°C to 300°C, the pulse time of the ferroelectric material metal source in each cycle to 1.2s to 1.8s, the pulse time of the oxygen source to 0.1s to 0.5s, and the deposition rate to 0.089nm / cycle to 0.11nm / cycle.
9. The PEALD in-situ preparation method of a ferroelectric structure according to claim 7, characterized in that: The material of the second electrode includes TiN; And / or, the thickness of the second electrode is 10nm to 50nm; And / or, the process conditions for depositing the second electrode include: setting the RF power to 2500W~2800W, the growth temperature to 300℃~400℃, the deposition rate to 0.03nm / cycle~0.038nm / cycle, the pulse time of the titanium source to 0.1s~1s in each cycle, and the pulse time of the nitrogen source to 5s~10s.
10. The PEALD in-situ preparation method of a ferroelectric structure according to claim 7, characterized in that: The temperature of the second annealing treatment is 450° C. to 600° C., and / or the time of the second annealing treatment is 30 s to 60 s.
11. The PEALD in-situ preparation method of a ferroelectric structure according to claim 7, characterized in that: Also includes: Disposing a dielectric layer between the first electrode or the second electrode and the ferroelectric layer; And / or, a plurality of the ferroelectric layers are formed on the first electrode, and a dielectric layer is disposed between two of the ferroelectric layers.
12. The PEALD in-situ preparation method of a ferroelectric structure according to claim 11, characterized in that: Specifically include: A dielectric layer is in-situ deposited between two ferroelectric layers, or between the first electrode or the second electrode and the ferroelectric layer, using plasma enhanced atomic layer deposition technology until the precursor structure is formed, and then the second annealing treatment is performed.
13. The PEALD in-situ preparation method of a ferroelectric structure according to claim 11, characterized in that: The material of the dielectric layer includes SiO2 and / or Al2O3; And / or, the thickness of the dielectric layer is 1-2 nm.
14. The PEALD in-situ preparation method of a ferroelectric structure according to claim 13, characterized in that: The process conditions for depositing the SiO2 dielectric layer include: setting the RF power to 2500w-2800w, the growth temperature to 200℃-300℃, the deposition rate to 0.06nm / cycle-0.09nm / cycle, the pulse time of the silicon source to 0.1s-6s in each cycle, and the pulse time of the oxygen source to 0.1s-0.3s; The process conditions for depositing the Al2O3 dielectric layer include: a growth temperature of 200°C-300°C, a deposition rate of 0.06nm / cycle-0.09nm / cycle, a pulse time of the aluminum source of 0.1s-6s in each cycle, and a pulse time of the oxygen source of 0.1s-0.3s.
15. A ferroelectric structure obtained by the PEALD in-situ preparation method according to any one of claims 7 to 14.
16. A ferroelectric device, characterized in that: Includes the TiN-based thin film as claimed in claim 6 or includes the ferroelectric structure as claimed in claim 15.