Method for preparing wear-resistant titanium-based composite coating through laser decomposition
The titanium-based composite coating was prepared through laser decomposition technology, and the nonstability of the MAX phase was used to form the TiC/Ti2AlC core-shell structure, which solved the wear resistance and corrosion resistance of the titanium alloy surface coating under high temperature conditions, and realized the coating The high strength and self-lubricating properties avoid powder splashing and pore problems in traditional synthesis reactions.
Patent Information
- Application Number
- CN202411200188.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing titanium alloy surface coatings are difficult to meet the composite coupling requirements of wear resistance, oxidation and corrosion under high temperature and complex operating conditions, and there are problems of powder splashing and internal pores of the coating in traditional synthesis reactions.
The titanium-based composite coating was prepared by laser decomposition technology, and the Ti2AlC and TC4 powder were mixed, and the high-energy beam scanning cladding was carried out using the unstability of the MAX phase to form a TiC/Ti2AlC core-shell structure to reduce the generation of intermediate products and pores in the synthesis reaction. Defects, enhance the metallurgical bonding and wear resistance of the coating.
The mechanical properties of TC4 surface are significantly improved, and a wear-resistant titanium-based composite coating with uniform and dense structure is prepared, with good metallurgical bonding and self-lubricating properties, which improves the wear and corrosion resistance of the coating.
Smart Images

Figure CN119082725A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of metal ceramic coatings, and in particular to a method for preparing a wear-resistant titanium-based composite coating by utilizing laser decomposition. Background technology:
[0002] Titanium alloys are widely used in high-precision devices such as aerospace equipment, marine equipment, and weapon systems due to their many characteristics, such as stability at high temperatures, corrosion resistance in marine environments, and fatigue resistance under continuous loads. However, the harsh service environment of titanium alloys further exposes the defects of the mechanical properties of the titanium alloy surface, exacerbating the failure of components. Surface modification technology can most directly and effectively improve the surface properties of titanium alloys to meet the service requirements under complex working conditions.
[0003] At present, the component composition systems of titanium alloy surface coatings, such as pure ceramic and pure metal coatings, mostly focus on improving fracture toughness, corrosion and oxidation, but have poor surface strengthening effects on the substrate. Therefore, it is difficult to meet the service requirements when facing the complex coupling of wear, oxidation and corrosion under actual working conditions. In comparison, the ternary layered metal ceramic M developed in recent years n+1 AX n Phase, due to its special layered structure and bonding method, has the dual characteristics of metal and ceramic. The existence of weak van der Waals force between its MA sheets can form graphite-like self-lubricating properties and has excellent corrosion resistance. MAX phase has become a surface modification material that has attracted much attention. Summary of the invention:
[0004] The present invention solves the problems of powder splashing and many pores in the coating caused by violent heat release in traditional synthesis reactions in the prior art, and provides a method for preparing a wear-resistant titanium-based composite coating by laser decomposition. The method proposed in the present invention effectively reduces the generation of intermediate products in the synthesis process, significantly improves the surface mechanical properties of TC4, and prepares a wear-resistant titanium-based composite coating with uniform and dense structure and good metallurgical bonding.
[0005] The object of the present invention is to provide a method for preparing a wear-resistant titanium-based composite coating by laser decomposition, comprising the following steps:
[0006] S1. Preparation of coating original powder: Ti2AlC and TC4 powder are mixed evenly to obtain coating original powder, wherein the volume fraction of Ti2AlC in the coating original powder is 5%-30%;
[0007] S2. Spread the original powder of the coating onto the pretreated substrate with a thickness of 0.8-1.0 mm. After laser high-energy beam scanning and cladding, a titanium-based composite coating is obtained. The cladding process parameters are as follows: spot diameter 4-5 mm, cladding power 2100-2400 W, scanning rate 6-7 mm / s, and argon flow rate 8-12 L / min.
[0008] Based on the advantages of high energy and high efficiency, good metallurgical bonding, etc. of laser cladding, the composite coating is prepared by utilizing the escape behavior of A atoms in the new ternary layered metal ceramic MAX phase, which can effectively reduce defects such as powder splashing and many pores inside the coating during the synthesis reaction. At the same time, based on the advantages of good toughness, high strength, and wear resistance of TC4 titanium alloy, TiC and MAX phases are introduced by in-situ decomposition to further strengthen the titanium base, and it can avoid the single element or double element powder from producing too many intermediate products during the synthesis preparation process, thereby affecting the final service performance of the coating. The binary MX phase formed by in-situ decomposition has good performance and excellent wettability with the substrate phase, which can achieve high-strength bonding, and in this process, the continuous diffusion of the A element promotes the formation of a core-shell structure. The synergistic strengthening effect of this special structure can effectively improve the coating performance. The present invention utilizes the characteristics of MAX being easily decomposed by heat, and develops a titanium-based composite coating with wear-resistant and self-lubricating properties through laser cladding technology.
[0009] Preferably, the volume fraction of Ti2AlC in the original powder of the coating in step S1 is 15%-20%.
[0010] Preferably, the coating original powder described in step S1 is prepared by the following steps: in an argon protection environment, Ti2AlC and TC4 powders are uniformly mixed using a planetary ball mill, and then placed in a vacuum drying oven and dried at 100° C. for 4 hours for use.
[0011] Further preferably, the ball milling parameters of the planetary ball mill are as follows: ball milling speed 200r / min, ball milling time 160min, ball-to-material ratio 5:1.
[0012] Preferably, the base material described in step S2 is TC4 titanium alloy.
[0013] Preferably, the pretreatment steps of the substrate in step S2 are as follows: the substrate is cut into rectangular blocks as needed, its surface oxide layer is polished, and then placed in an anhydrous ethanol solution to clean surface stains, and finally dried in a vacuum drying oven for use.
[0014] Preferably, the powder spreading thickness in step S2 is 1 mm.
[0015] Preferably, the cladding process parameters described in step S2 are as follows: spot diameter 5 mm, cladding power 2100 W, scanning rate 7 mm / s, argon gas flow rate 10 L / min.
[0016] The present invention also protects the wear-resistant titanium-based composite coating obtained by the method of preparing the wear-resistant titanium-based composite coating by laser decomposition, wherein the wear rate of the wear-resistant titanium-based composite coating is 8.19×10 -5 -1.60×10 -4 mm 3 ·N -1 ·m -1 . The present invention induces the decomposition of Ti2AlC MAX phase through laser cladding technology to form a metal ceramic composite coating with a TiC / Ti2AlC core-shell structure. The method can realize the decomposition and resynthesis process of the MAX phase, and the TiC / Ti2AlC core-shell structure effectively plays a role in buffering the load, and the grains of the formed reinforcement phase organization are refined. The coating has significantly high microhardness, excellent wear resistance, and the interface presents good metallurgical bonding characteristics.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] 1. The method proposed in the present invention for preparing a composite coating by decomposing the non-stable phase characteristics of the MAX phase through laser cladding technology can effectively avoid problems such as powder splashing and many pores inside the coating caused by the violent heat release in the synthesis reaction. The titanium-based composite coating is based on the basket structure formed by a large amount of TC4 in the original powder after the non-equilibrium martensitic phase transformation, which gives the composite coating good toughness and wear resistance. The decomposition and introduction of TiC and a small amount of MAX phase further enhances the strength and self-lubricating effect to strengthen the titanium base. In addition, the MAX phase depends on the TiC nucleation to produce a special core-shell structure. Its soft and hard alternating characteristics can play a significant buffering effect in the process of bearing loads, improve the wear resistance of the coating, and finally obtain a wear-resistant titanium-based composite coating with few defects, good metallurgical bonding, and uniform and dense structure.
[0019] 2. The present invention uses the laser cladding technology with high efficiency and short process integration as a preparation method to deposit a coating with good metallurgical bonding, and develops a titanium-based composite coating with wear-resistant and self-lubricating properties, providing a strong technical guarantee for the large-scale industrial application of titanium-based composite coatings. Description of the drawings:
[0020] Figure 1 is the XRD phase analysis of the composite coatings with different Ti2AlC reinforcement phase contents in Examples 1-4;
[0021] Figure 2 is the hardness analysis of the composite coatings with different Ti2AlC reinforcement phase contents in Examples 1-4;
[0022] Figure 3 This is the SEM morphology of the middle part and the bonding area of the coating in Example 1;
[0023] Figure 4 This is the SEM morphology of the middle part and the bonding area of the coating in Example 2;
[0024] Figure 5 This is the SEM morphology of the middle part and the bonding area of the coating of Example 3;
[0025] Figure 6 This is the SEM morphology of the middle part and the bonding area of the coating of Example 4;
[0026] Figure 7 This is the cross-sectional morphology of the coating of Example 5;
[0027] Figure 8 This is the SEM morphology of the middle part and the bonding area of the coating of Example 6;
[0028] Fig. 9 is the wear scar cross section of TC4, Example 1, Example 2, Example 3, and Example 4;
[0029] Fig.10 is the wear rate of the wear scar surface of TC4, Example 1, Example 2, Example 3, and Example 4;
[0030] Fig.11 Schematic diagram of the structure of the composite coating obtained in Examples 1-4 and a scanning electron microscope diagram of the core-shell structure. Specific implementation method:
[0031] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0032] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.
[0033] The method for preparing wear-resistant titanium-based composite coating by laser decomposition proposed by the present invention mainly comprises the following steps: selection and preparation of matrix material, proportioning and preparation of original powder, and preparation of composite coating.
[0034] The detailed steps are as follows:
[0035] S1. Selection of base material: The present invention uses TC4 titanium alloy as the base material, cuts it into rectangular blocks as needed, grinds its surface oxide layer with a grinder, then puts it into an anhydrous ethanol solution to ultrasonically clean its surface stains, and finally dries it in a vacuum drying oven for use. The preferred rectangular block size of the following embodiment is 40mm×15mm×10mm.
[0036] S2. Original powder ratio and preparation: The original powder of the cladding coating is Ti2AlC (purity 99%, <72μm) and TC4 (purity 99%, <48μm). Ti2AlC is mixed with TC4 powder at a volume fraction of 5%-20%, and the sum of the two raw materials is 100%. The powder is mixed by a planetary ball mill and placed in a vacuum drying oven at 100°C for 4 hours for use. The experimental environment is an argon atmosphere. The specific ball milling parameters are as follows: ball milling speed 200r / min, ball milling time 160min, ball to material ratio 5:1.
[0037] S3, preparation of composite coating: using the pre-set powder method, the original powder obtained in step S2 is spread on the TC4 substrate pretreated in step S1, and the powder thickness is 0.8-1.0mm. The laser cladding process is carried out on a laser system with a self-provided argon protection chamber. The cladding process parameters are as follows: spot diameter is 4-5mm, cladding power is 2100-2400W, scanning rate is 6-7mm / s, argon flow rate is 8-10L / min, and titanium-based composite coating is obtained by laser high-energy beam scanning cladding.
[0038] Example 1
[0039] A method for preparing a wear-resistant titanium-based composite coating by laser decomposition comprises the following steps:
[0040] S1. Selection of base material: TC4 titanium alloy is used as the base material. It is cut into rectangular blocks with specifications of 40mm×15mm×10mm according to needs, and its surface oxide layer is polished with a grinder. Then, it is placed in anhydrous ethanol solution for ultrasonic cleaning of surface stains, and finally dried in a vacuum drying oven for use.
[0041] S2. Preparation of original coating powder: Ti2AlC and TC4 powder are mixed evenly to obtain original coating powder, in which the volume fraction of Ti2AlC is 5%. Specifically, the powder is mixed by a planetary ball mill and placed in a vacuum drying oven for drying at 100°C for 4 hours for use, wherein the experimental environment is an argon atmosphere, and the ball milling parameters are as follows: ball milling speed 200r / min, ball milling time 160min, ball-to-material ratio 5:1.
[0042] S3. Spread the original powder of the coating onto the pretreated substrate with a powder thickness of 1 mm, and obtain a titanium-based composite coating by laser high-energy beam scanning cladding. The cladding process parameters are as follows: spot diameter 5 mm, cladding power 2100 W, scanning rate 7 mm / s, and argon flow rate 10 L / min.
[0043] Example 2
[0044] The same as Example 1, except that: the volume fraction of Ti2AlC in the original powder of the coating in step S2 is 10%.
[0045] Example 3
[0046] The same as Example 1, except that the volume fraction of Ti2AlC in the original powder of the coating in step S2 is 15%.
[0047] Example 4
[0048] The same as Example 1, except that: the volume fraction of Ti2AlC in the original powder of the coating in step S2 is 20%.
[0049] Example 5
[0050] The same as Example 1, except that: the volume fraction of Ti2AlC in the original powder of the coating in step S2 is 30%.
[0051] Example 6
[0052] The same as Example 4, except that the powder thickness is 0.8 mm. The laser cladding process is carried out on a laser system with a self-provided argon protection chamber, and the cladding process parameters are as follows: spot diameter 4 mm, cladding power 2400 W, scanning rate 6 mm / s, argon flow rate 8 L / min.
[0053] The composite coatings prepared in Examples 1-6 were cut into rectangular blocks of 8 mm × 15 mm × 10 mm, and phase sample preparation, coating interface metallographic preparation, and chemical etching were performed to obtain the phase and microstructure results as shown in the following figure: Figure 1 , Figure 3-8 shown.
[0054] The phase composition of the titanium-based composite coating prepared in Examples 1-4 is mainly α-Ti, β-Ti, Ti2AlC, TiC and a small amount of TiAl. The peak intensity of TiC and Ti2AlC MAX phases in Example 4 is the largest among all the examples. The composite coating has a good metallurgical bond with the substrate, and the structure is uniform and dense without obvious holes and cracks.
[0055] Figure 7 This is the cross-sectional morphology of the coating prepared in Example 5. When the volume fraction of Ti2AlC increases to 30%, large-area agglomeration occurs in the coating structure, resulting in a decrease in the density of the structure, which seriously affects the service effect of the coating.
[0056] Figure 8 This is the cross-sectional microstructure of the coating prepared in Example 6. Under high power, the TiC is broken into flakes due to heat, which greatly weakens the strengthening effect of the reinforced coating.
[0057] Fig.11 Schematic diagram of the TiC / Ti2AlC core-shell structure composite coating prepared in Example 1. The core-shell structure is a reinforcement phase particle formed by Ti2AlCMAX phase coating TiC phase.
[0058] The composite coatings obtained in Examples 1-4 were subjected to the following performance tests:
[0059] Coating hardness test: Use a microhardness tester to test the hardness performance of the cladding coating cross section. During the test, the load is 1 kg, the load time is 10 seconds, and the test is performed every 0.15 mm between the surface and the substrate. The hardness distribution of five points at the same level is tested to obtain the average hardness value to ensure the accuracy of the experimental results. The results are as follows Figure 2 As shown, the microhardness of TC4 titanium alloy is 360HV 1.0 The average microhardness of the surface layer of Example 1, Example 2, Example 3, and Example 4 is 463.2 HV 1.0 、466.7HV 1.0 、479.3HV 1.0 、501.3HV 1.0 The microhardness of the four groups of examples is higher than that of the TC4 matrix, and Example 4 has the highest microhardness of 501.3HV 1.0 , which is 1.39 times that of TC4 matrix.
[0060] Test of coating wear performance: Cut the four groups of clad specimens into 8mm×15mm×10mm blocks, use sandpaper (maximum grinding and polishing mesh is 2000 mesh) to grind the coating surface and TC4 substrate until smooth, and then use the friction and wear test system to test the wear performance of the specimen surface. During the experiment, the grinding pair material is Si3N4 ball with a diameter of 6mm. The specific experimental parameters are: experimental load 10N, experimental time is 20min, test reciprocating distance is 5mm, frequency is 1Hz. The experimental environment is atmospheric atmosphere, and the temperature is controlled at 20±5℃. The results are as follows Fig.10 As shown, the wear rate of TC4 titanium alloy is 1.74×10 -4 mm 3 ·N -1 ·m -1 The wear rates of Example 1, Example 2, Example 3, and Example 4 are 1.60×10 -4 mm 3 ·N -1 ·m -1 , 1.42×10 -4 mm 3 ·N -1 ·m -1 ,9.62×10 -5 mm 3 ·N-1 ·m -1 ,8.19×10 -5 mm 3 ·N -1 ·m -1 .
[0061] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a wear-resistant titanium-based composite coating by laser decomposition, characterized in that: The steps include: S1. Preparation of coating original powder: Ti2AlC and TC4 powder are mixed evenly to obtain coating original powder, wherein the volume fraction of Ti2AlC in the coating original powder is 5%-30%; S2. Spread the original powder of the coating onto the pretreated substrate with a powder thickness of 0.8-1.0 mm. After laser high-energy beam scanning and cladding, a titanium-based composite coating is obtained. The cladding process parameters are as follows: spot diameter 4-5 mm, cladding power 2100-2400 W, scanning rate 6-7 mm / s, and argon flow rate 8-10 L / min.
2. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1, characterized in that: The volume fraction of Ti2AlC in the original coating powder in step S1 is 15%-20%.
3. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1, characterized in that: The coating original powder described in step S1 is prepared by the following steps: in an argon protection environment, Ti2AlC and TC4 powders are mixed evenly by a planetary ball mill, and then placed in a vacuum drying oven and dried at 100° C. for 4 hours for use.
4. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 3, characterized in that: The milling parameters of the planetary ball mill are as follows: milling speed 200 r / min, milling time 160 min, ball-to-material ratio 5:
1.
5. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1, characterized in that: The base material described in step S2 is TC4 titanium alloy.
6. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1 or 5, characterized in that: The pretreatment steps of the substrate described in step S2 are as follows: the substrate is cut into rectangular blocks as needed, its surface oxide layer is polished, and then placed in anhydrous ethanol solution to clean the surface stains, and finally dried in a vacuum drying oven for use.
7. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1, characterized in that: The powder spreading thickness described in step S2 is 1 mm.
8. The method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1, characterized in that: The cladding process parameters described in step S2 are as follows: spot diameter 5 mm, cladding power 2100 W, scanning rate 7 mm / s, argon gas flow rate 10 L / min.
9. The wear-resistant titanium-based composite coating obtained by the method for preparing a wear-resistant titanium-based composite coating by laser decomposition according to claim 1, characterized in that: The wear rate of the wear-resistant titanium-based composite coating is 8.19×10 -5 -1.60×10 -4 mm 3 ·N -1 ·m -1 .