Nickel-molybdenum-based self-supporting catalytic material treated by aqueous solution containing oxalic acid / chromium chloride / lithium nitrate and application of nickel-molybdenum-based self-supporting catalytic material in field of electrochemical hydrogen production

Oxalic acid/chromium/lithium-ni-molybdenum-based catalytic material prepared by thermochemical method solves the problems of low performance and short service life caused by adhesives, and achieves efficient and stable OER catalytic performance and long life, which is suitable for industrial applications. .

CN119082769APending Publication Date: 2024-12-06CHENGDU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213726.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing OER catalysts have low performance and short service life due to the use of adhesives, and the high cost and scarcity of precious metal catalysts, which limits their wide application.

Method used

The oxalic acid/chromium chloride/lithium nitrate aqueous solution is treated by industrial compatible thermochemical method to prepare nickel-molybdenum-based self-supporting catalytic materials, avoiding the use of adhesives, and using clean commercial metal foam nickel-molybdenum to form oxalic acid/chromium /Lithium-nickel-molybdenum-based catalytic material.

Benefits of technology

The catalytic material exhibits excellent OER catalytic activity and stability under high current density, significantly reduces the overpotential, and can operate stably for more than 100 hours under industrial conditions, extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020909330000031
    Figure BDA0005020909330000031
  • Figure BDA0005020909330000041
    Figure BDA0005020909330000041
  • Figure HDA0005020909340000011
    Figure HDA0005020909340000011
Patent Text Reader

Abstract

The invention relates to the field of electrochemical hydrogen production, which is characterized in that an aqueous solution containing oxalic acid, chromium chloride and lithium nitrate is placed in a drying oven to be heated by utilizing an industrial compatible thermochemical method, and after the temperature is constant, clean commercial metal foam nickel molybdenum stands in the solution to react to obtain a self-supporting catalytic material, and the surface of the catalyst is covered by square particles. And a plurality of gaps exist among the square particles. The structure effectively increases the surface area of the catalytic material, so that more active sites are exposed, and the catalytic material has excellent OER catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical hydrogen production, and in particular to a nickel-molybdenum-based self-supporting catalytic material treated with an aqueous solution containing oxalic acid / chromium chloride / lithium nitrate, and application thereof in the field of electrochemical hydrogen production. Background Art

[0002] The excessive use of fossil fuels inevitably leads to energy shortages and environmental pollution. Therefore, it is urgent to develop and produce efficient, renewable and environmentally friendly energy. Hydrogen energy is considered to be the ultimate energy source due to its high calorific value and carbon-free nature. In recent years, hydrogen production by electrochemical water splitting has been proven to be the most promising method. However, the hydrogen evolution reaction (HER) in the cathode reaction and the oxygen evolution reaction (OER) in the anode reaction, including water splitting, are limited by sluggish kinetics and high overpotentials. Designing efficient and stable electrocatalysts is necessary to overcome these obstacles.

[0003] Noble metal (Ru, Ir) materials remain highly efficient catalysts for OER, but their high cost and scarcity limit their wide application. Therefore, developing a high-performance and long-life catalyst with non-noble metals still faces many challenges.

[0004] In addition, many OER catalytic materials are in powder form, which inevitably requires the use of adhesives to bond the active substances to the relay surface. However, this adhesive will block most of the active sites, resulting in poor performance. In addition, due to the aging of the adhesive, the active components will fall off, resulting in a decrease in catalytic activity.

[0005] In summary, in order to avoid the above two shortcomings and to achieve a balance between economy and catalytic performance, the present invention utilizes an industrially compatible thermochemical method to prepare a self-supporting catalyst using non-precious metals as materials, and the catalyst has excellent catalytic activity and a long service life, and is suitable for large-scale industrial preparation and application. Summary of the invention

[0006] Technical problems solved by the present invention:

[0007] The self-supporting catalytic material avoids the use of adhesives and solves the problems of low catalyst performance and short service life in the past. Summary of the invention:

[0009] The present invention relates to a nickel-molybdenum-based self-supporting catalytic material treated with an aqueous solution containing oxalic acid / chromium chloride / lithium nitrate, wherein the catalytic material is obtained by placing clean commercial metal foam nickel-molybdenum in an oxalic acid / chromium chloride / lithium nitrate aqueous solution at elevated temperature. The final product is labeled as oxalic acid / chromium / lithium-nickel-molybdenum-based.

[0010] The benefits of the present invention are:

[0011] The self-supporting catalytic material obtained by the present invention has excellent OER catalytic activity at 10 mA cm -2 , 50mAcm -2 , 100mAcm -2 The overpotentials at different current densities are 232.81mV, 258.90mV and 275.72mV respectively. It can run stably for more than 100 hours at industrial current density (over 1A). BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is the LSV curve diagram of each catalytic material.

[0013] Figure 2 Overpotential diagram of each catalytic material.

[0014] Figure 3 This is a stability test chart for oxalic acid / chromium / lithium-nickel-molybdenum based.

[0015] Figure 4 This is the SEM image of oxalic acid / chromium / lithium-nickel molybdenum base. DETAILED DESCRIPTION

[0016] In order to more clearly explain the purpose, technical scheme and advantages of the embodiments of the present invention, the technical scheme in the embodiments will be described in detail below. If specific conditions are not particularly specified, the operation will be carried out according to the usual conditions or the recommendations of the manufacturer. When the manufacturer of the reagent or instrument is not particularly specified, it refers to the conventional products that can be purchased on the market.

[0017] Example

[0018] Oxalic acid / chromium / lithium-nickel-molybdenum-based self-supporting catalytic material, and its preparation method, characterized by: placing an aqueous solution containing oxalic acid, chromium chloride, and lithium nitrate in an oven, setting the ambient temperature to 120°C, and after the solution temperature stabilizes, placing clean commercial metal foam nickel-molybdenum in the above solution for reaction for 90 minutes. Take out the material, rinse the surface residual substances with deionized water, wipe the surface moisture with filter paper, and air-dry at room temperature to obtain the final sample.

[0019] The specific parameters for the preparation of each catalyst in the examples are shown in Table 1-2.

[0020] Table 1 Reagent dosage, reaction temperature and treatment time

[0021]

[0022]

[0023] Test example

[0024] 1.LSV, EIS and IT testing

[0025] The self-supporting catalytic material in the embodiment was tested for OER activity. The conditions for LSV and EIS testing were: using a Coster electrochemical workstation, with the self-supporting material as the anode, mercury / mercuric oxide as the reference electrode, a platinum sheet as the counter electrode, and a 1M KOH solution as the electrolyte.

[0026] Figure 1 The LSV curves of each catalyst can be seen from the figure that the OER performance of the catalytic material after heat treatment is significantly higher than that of commercial metal foam nickel molybdenum (nickel-molybdenum based).

[0027] Figure 2 The overpotential diagram of each catalyst at 10 mA cm -2 , 50mAcm -2 and 100mAcm -2 The overpotentials of oxalate / chromium / lithium-nickel-molybdenum-based materials at the current density are 232.81 mV, 258.90 mV, and 275.72 mV (denoted as 232.81 mV@10 mA cm -2 , 258.90mV@50mAcm -2 , 258.90mV@100mAcm -2 ) is significantly lower than that of NiMo-based (342.25mV@10mA cm -2 , 405.75mV@50mAcm -2 , 441.22mV@100mAcm -2 ).

[0028] Figure 3 This is a stability test chart for oxalic acid / chromium / lithium-nickel-molybdenum based catalyst. Using the chronoamperometry method with 1A as the evaluation standard, the catalyst can run stably for at least 100 hours without a significant drop in current.

[0029] 2. Microstructure

[0030] Figure 4 This is the SEM image of oxalic acid / chromium / lithium-nickel molybdenum base. After heat treatment, the square particles are evenly and firmly loaded on the surface of the substrate material. It is this structure that makes the self-supporting material have excellent OER catalytic performance and a long service life.

[0031] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A nickel-molybdenum-based self-supporting catalytic material treated with an aqueous solution containing oxalic acid / chromium chloride / lithium nitrate, characterized in that: The material is covered with square particles.

2. According to claim 1, the aqueous solution containing oxalic acid / chromium chloride / lithium nitrate is configured as follows: the ratio of oxalic acid, chromium chloride, lithium nitrate and water is: 0.5 mol: 0.05 mol: 0.05 mol: 100 mL.

3. According to claim 1, the temperature at which the commercial metal foam nickel-molybdenum substrate is allowed to stand in an aqueous solution containing oxalic acid / chromium chloride / lithium nitrate for reaction is 120°C.

4. According to claim 1, the commercial metal foam nickel-molybdenum substrate is allowed to stand for 90 minutes in the aqueous solution of oxalic acid / chromium chloride / lithium nitrate.

5. Application of the nickel-molybdenum-based self-supporting catalytic material treated with an aqueous solution containing oxalic acid / chromium chloride / lithium nitrate as described in any one of claims 1 to 4 in the field of electrochemical hydrogen production.