Color-change-resistant antibacterial polyamide fiber and preparation method thereof
Through the combination of functional polyamide and biomass fibers and ion exchange treatment, the problem of insufficient color discoloration and washing resistance of traditional antibacterial nylon fibers is solved, and the antibacterial and color change resistance is improved, which extends the service life and improves the cost-effectiveness. .
Patent Information
- Application Number
- CN202411428203.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional antibacterial nylon fibers are prone to discoloration during processing and use, and their antibacterial properties and water-resistant properties are insufficient, which affects their service life and cost-effectiveness.
Functional polyamide is prepared by polycondensation reaction, combined with biomass fibers and antioxidants, and ion exchange treatment to form color-resistant antibacterial nylon fibers, improving antibacterial and water-washing resistance.
It has achieved the improvement of color change resistance and antibacterial properties, extended service life, and improved the cost-effectiveness of the product, making it suitable for industrial production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical fibers, and in particular to a color-discoloration-resistant and antibacterial nylon fiber and a preparation method thereof. Background Art
[0002] Nylon fiber is one of the earliest synthetic fibers, also known as nylon or nylon. It is widely used in chemical fiber, textile clothing, manufacturing and other fields due to its good mechanical properties, corrosion resistance and good textile processing properties. In recent years, it has occupied the forefront of synthetic fiber production and sales. However, the traditional nylon fiber has poor antibacterial properties. It is under this situation that antibacterial nylon fiber came into being, and its appearance has attracted widespread attention in the industry.
[0003] At present, antibacterial nylon fiber usually achieves its antibacterial function by adding silver ion antibacterial agent. This type of antibacterial nylon fiber has good antibacterial properties. However, it is very easy to discolor during processing and use. When the fiber is left for too long or the acidity and alkalinity of the environment changes, it will produce red, brown and other color changes. The fabric made of this fiber will produce uneven color spots and blocks, which seriously affects the use of antibacterial nylon fiber. The main reason for the discoloration is that the silver ions in the loaded antibacterial agent precipitate too quickly, especially in high temperature and high humidity environments. The precipitated silver ions generate colored compounds, causing the color of the fiber or fabric to change. The discoloration phenomenon is particularly obvious in nylon 6 or nylon 66.
[0004] In order to solve the above problems, antibacterial nylon fibers that resist discoloration have been widely studied in the industry. For example, the Chinese invention patent with the authorization announcement number CN108385203B discloses a method for preparing antibacterial nylon fibers that resist discoloration, comprising the following steps: (1) weighing long-chain nylon, silver-ion-carrying antibacterial agent, dispersant, antioxidant and light stabilizer, melt-blending and extruding, and pelletizing to obtain masterbatch; (2) adding the masterbatch prepared in step (1) together with nylon slices into a spinning machine to spin out anti-discoloration nylon fibers. The antibacterial nylon fibers prepared by the invention hardly change color during processing and use, have excellent anti-discoloration performance, and have stable and long-lasting antibacterial performance. However, the silver-ion-carrying antibacterial agent is still used, which is not only expensive, but also has a need for further improvement in its water washing resistance.
[0005] Therefore, it is necessary to seek a more effective method to prepare a color-resistant and antibacterial nylon fiber with good color-resistant and antibacterial properties, sufficient water-resistant performance, high cost-effectiveness, and long service life. Summary of the invention
[0006] The main purpose of the present invention is to provide a color-discoloration-resistant antibacterial nylon fiber with good color-discoloration resistance and antibacterial performance, sufficient water-washing resistance, high cost performance and long service life, and a preparation method thereof.
[0007] To achieve the above object, the present invention provides a method for preparing color-discoloration-resistant antibacterial nylon fiber, comprising the following steps: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, then the mixture is added to a reaction kettle, the air in the kettle is replaced with an inert gas, and the mixture is reacted at 115-125° C. under normal pressure for 2-4 hours, then the temperature is raised to 230-250° C., and a polycondensation reaction is carried out at 100-400 Pa for 13-18 hours, then the mixture is cooled to room temperature, adjusted to normal pressure, precipitated in water, the crude product is washed with ethanol for 3-6 times, and then placed in a vacuum drying oven at 85-95° C. to dry to constant weight to obtain a functional polyamide; Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a sodium alginate aqueous solution at 50-60° C. for 20-30 hours, take it out and soak it in water for 10-20 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
[0008] Preferably, the molar ratio of 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst and high boiling point solvent in step S1 is 1:1:(0.8-1):(8-15).
[0009] Preferably, the catalyst is at least one of thiophosphonate, phosphorous acid, and thiophosphoramide; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is any one of nitrogen, helium, neon, and argon.
[0010] Preferably, the mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:(3-5):(10-20):(1-2):(1-2).
[0011] Preferably, the biomass fiber is at least one of bamboo pulp fiber and hemp pulp fiber; the average diameter of the biomass fiber is 3-9 μm, and the aspect ratio is (20-30):1.
[0012] Preferably, the coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; the antioxidant is at least one of antioxidant 1010 and antioxidant 168; and the lubricant is at least one of pentaerythritol stearate and ethylene bisstearamide.
[0013] Preferably, the temperature of the melt blending extrusion in step S2 is 255-280° C., and the extrusion pressure is 6-9 MPa.
[0014] Preferably, the mass ratio of the functional masterbatch to the nylon chips in step S3 is 1:(5-10).
[0015] Preferably, the nylon slice is a nylon 6 slice, the number average molecular weight of which is 20,000-30,000 and the relative viscosity is 2.8-3.0.
[0016] Preferably, the spinning process parameters in step S3 are: spinning temperature 260-280° C., winding speed 1000-1500 m / min, and drafting multiple 2-4.
[0017] Preferably, the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 5-10%.
[0018] Another object of the present invention is to provide a color-discoloration-resistant antibacterial nylon fiber made by the above-mentioned preparation method of the color-discoloration-resistant antibacterial nylon fiber.
[0019] Due to the application of the above technical solution, the present invention has the following beneficial effects: (1) The method for preparing the color-discoloration-resistant antibacterial nylon fiber disclosed in the present invention has a short and simple process flow, convenient operation and control, low energy consumption, high preparation efficiency and finished product qualification rate, and is suitable for industrial production.
[0020] (2) The antibacterial nylon fiber with color change resistance disclosed in the present invention has a functional masterbatch made of functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant. The functional polyamide is made of 3,7-diamino-5-phenylphenazine chloride and thiazo[5,4-d]thiazole-2,5-dicarboxylic acid through polycondensation reaction. Amide groups, thiazolyl groups and phenylphenazine cationic groups are simultaneously introduced into the polyamide molecular chain. These structures can effectively improve the antibacterial performance and color change resistance under the multiple effects of electronic effect, steric effect and conjugation effect, so that the product has better water washing resistance and longer service life. The addition of biomass fiber can not only play a reinforcing role, but also further cooperate with other raw materials to improve the antibacterial effect.
[0021] (3) The color change resistant and antibacterial nylon fiber disclosed in the present invention is first made into a functional masterbatch, and then blended with nylon chips and pelletized, and spun, which can effectively improve the dispersion uniformity and compatibility between the raw materials, and thus improve the performance stability; sodium alginate can undergo ion exchange reaction with the phenylphenazine chloride structural unit in the functional polyamide to form ionic crosslinking, which can effectively improve the antibacterial and color change resistance, make the water washing resistance more sufficient, and the service life longer. DETAILED DESCRIPTION
[0022] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations. Example 1
[0023] A method for preparing color-discoloration-resistant antibacterial nylon fiber comprises the following steps: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, and then the mixture is added to a reaction kettle, and the air in the kettle is replaced with an inert gas, and the reaction is carried out at 115° C. for 2 hours under normal pressure, and then the temperature is raised to 230° C., and a polycondensation reaction is carried out at 100 Pa for 13 hours, and then cooled to room temperature, adjusted to normal pressure, precipitated in water, and washed with ethanol. The crude product was dried three times and then placed in a vacuum drying oven at 85°C to constant weight to obtain a functional polyamide; the molar ratio of the 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst, and high boiling point solvent was 1:1:0.8:8; the catalyst was a thiophosphonate; the high boiling point solvent was dimethyl sulfoxide; the inert gas was nitrogen; the functional polyamide was measured by GPC test to have Mn=15523 g / mol, M W / M n =1.352; calculated by elemental analysis and weight change, the molar ratio of the structural units introduced by 3,7-diamino-5-phenylphenazine chloride and thiazo[5,4-d]thiazole-2,5-dicarboxylic acid in the functional polyamide is the same as the theoretical value.
[0024] Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a 50° C. sodium alginate aqueous solution for 20 hours, take it out and soak it in water for 10 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
[0025] The mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:3:10:1:1; the biomass fiber is bamboo pulp fiber; the average diameter of the biomass fiber is 3 μm, and the aspect ratio is 20:1; the coupling agent is silane coupling agent KH550; the antioxidant is antioxidant 1010; and the lubricant is pentaerythritol stearate.
[0026] The temperature of the melt blending extrusion in step S2 is 255° C., and the extrusion pressure is 6 MPa; the mass ratio of the functional masterbatch and the nylon slice in step S3 is 1:10; the nylon slice is a nylon 6 slice, and its number average molecular weight is 20,000 and the relative viscosity is 2.8.
[0027] The spinning process parameters in step S3 are: spinning temperature 260° C., winding speed 1000 m / min, and drafting multiple 2; the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 5%.
[0028] Disclosed is a color-change resistant antibacterial nylon fiber produced by the method for preparing the color-change resistant antibacterial nylon fiber. Example 2
[0029] A method for preparing color-discoloration-resistant antibacterial nylon fiber comprises the following steps: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, then the mixture is added to a reaction kettle, the air in the kettle is replaced with an inert gas, and the mixture is reacted at 118° C. under normal pressure for 2.5 hours, then the temperature is raised to 235° C., and a polycondensation reaction is carried out at 200 Pa for 15 hours, then the mixture is cooled to room temperature, adjusted to normal pressure, precipitated in water, the crude product is washed with ethanol 4 times, and then placed in a vacuum drying oven at 87° C. to dry to constant weight to obtain a functional polyamide; Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a sodium alginate aqueous solution at 53° C. for 23 hours, take it out and soak it in water for 12 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
[0030] In step S1, the molar ratio of 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst and high boiling point solvent is 1:1:0.85:9; the catalyst is phosphorous acid; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is helium.
[0031] The mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:3.5:13:1.2:1.3; the biomass fiber is hemp pulp fiber; the average diameter of the biomass fiber is 5 μm, and the aspect ratio is 23:1; the coupling agent is silane coupling agent KH560; the antioxidant is antioxidant 168; and the lubricant is ethylene bisstearamide.
[0032] The temperature of the melt blending extrusion in step S2 is 265°C, and the extrusion pressure is 7MPa; the mass ratio of the functional masterbatch and the nylon slice in step S3 is 1:8; the nylon slice is a nylon 6 slice, and its number average molecular weight is 23,000 and the relative viscosity is 2.9; the spinning process parameters in step S3 are: spinning temperature 265°C, winding speed 1200m / min, and drafting multiple 2.5; the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 6%.
[0033] Disclosed is a color-change resistant antibacterial nylon fiber produced by the method for preparing the color-change resistant antibacterial nylon fiber. Example 3
[0034] A method for preparing color-discoloration-resistant antibacterial nylon fiber comprises the following steps: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, then the mixture is added to a reaction kettle, the air in the kettle is replaced with an inert gas, and the mixture is reacted at 120° C. for 3 hours at normal pressure, then the temperature is raised to 240° C., and a polycondensation reaction is carried out at 250 Pa for 15 hours, then the mixture is cooled to room temperature, adjusted to normal pressure, precipitated in water, the crude product is washed with ethanol 4 times, and then placed in a vacuum drying oven at 90° C. and dried to constant weight to obtain a functional polyamide; Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a 55° C. sodium alginate aqueous solution for 25 hours, take it out and soak it in water for 15 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
[0035] In step S1, the molar ratio of 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst and high boiling point solvent is 1:1:0.9:12; the catalyst is thiophosphoramide; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is neon.
[0036] The mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:4:15:1.5:1.5; the biomass fiber is bamboo pulp fiber; the average diameter of the biomass fiber is 6 μm, and the aspect ratio is 25:1; the coupling agent is silane coupling agent KH570; the antioxidant is antioxidant 1010; the lubricant is pentaerythritol stearate; the temperature of the melt blending extrusion in step S2 is 270°C, and the extrusion pressure is 7.5 MPa; the mass ratio of the functional masterbatch and nylon slices in step S3 is 1:7; the nylon slices are nylon 6 slices, whose number average molecular weight is 25,000 and the relative viscosity is 2.9; the spinning process parameters in step S3 are: spinning temperature 270°C, winding speed 1300m / min, and drafting multiple 3; the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 8%.
[0037] Disclosed is a color-change resistant antibacterial nylon fiber produced by the method for preparing the color-change resistant antibacterial nylon fiber. Example 4
[0038] A method for preparing color-discoloration-resistant antibacterial nylon fiber comprises the following steps: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, then the mixture is added to a reaction kettle, the air in the kettle is replaced with an inert gas, and the mixture is reacted at 123° C. under normal pressure for 3.5 hours, then the temperature is raised to 245° C., and a polycondensation reaction is carried out at 350 Pa for 17 hours, then the mixture is cooled to room temperature, adjusted to normal pressure, precipitated in water, the crude product is washed with ethanol for 6 times, and then placed in a vacuum drying oven at 93° C. to dry to constant weight to obtain a functional polyamide; Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a sodium alginate aqueous solution at 58° C. for 28 hours, take it out and soak it in water for 18 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
[0039] The molar ratio of 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst and high boiling point solvent in step S1 is 1:1:0.95:14; the catalyst is a mixture of thiophosphonate, phosphorous acid and thiophosphoramide in a mass ratio of 1:2:3; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is argon.
[0040] The mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:4.5:18:1.8:1.8; the biomass fiber is a mixture of bamboo pulp fiber and hemp pulp fiber in a mass ratio of 3:5; the average diameter of the biomass fiber is 8 μm, and the aspect ratio is 28:1; the coupling agent is a mixture of silane coupling agent KH550, silane coupling agent KH560 and silane coupling agent KH570 in a mass ratio of 1:2:3; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 3:5; the lubricant is a mixture of pentaerythritol stearate and ethylene bisstearamide in a mass ratio of 1:3.
[0041] The temperature of the melt blending extrusion in step S2 is 275°C, and the extrusion pressure is 8.5MPa; the mass ratio of the functional masterbatch and the nylon slice in step S3 is 1:6; the nylon slice is a nylon 6 slice, and its number average molecular weight is 28,000 and the relative viscosity is 3.0; the spinning process parameters in step S3 are: spinning temperature 275°C, winding speed 1400m / min, and drafting multiple 3.5; the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 9%.
[0042] Disclosed is a color-change resistant antibacterial nylon fiber produced by the method for preparing the color-change resistant antibacterial nylon fiber. Example 5
[0043] A method for preparing color-discoloration-resistant antibacterial nylon fiber comprises the following steps: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, then the mixture is added to a reaction kettle, the air in the kettle is replaced with an inert gas, and the mixture is reacted at 125° C. under normal pressure for 4 hours, then the temperature is raised to 250° C., and a polycondensation reaction is carried out at 400 Pa for 18 hours, then the mixture is cooled to room temperature, adjusted to normal pressure, precipitated in water, the crude product is washed with ethanol for 6 times, and then placed in a vacuum drying oven at 95° C. to dry to constant weight to obtain a functional polyamide; Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a 60° C. sodium alginate aqueous solution for 30 hours, take it out and soak it in water for 20 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
[0044] In step S1, the molar ratio of 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst and high boiling point solvent is 1:1:1:15; the catalyst is thiophosphonate; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is nitrogen.
[0045] The mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:5:20:2:2; the biomass fiber is bamboo pulp fiber; the average diameter of the biomass fiber is 9 μm, and the aspect ratio is 30:1; the coupling agent is silane coupling agent KH560; the antioxidant is antioxidant 1010; and the lubricant is ethylene bisstearamide.
[0046] The temperature of the melt blending extrusion in step S2 is 280°C, and the extrusion pressure is 9MPa; the mass ratio of the functional masterbatch and the nylon slice in step S3 is 1:5; the nylon slice is a nylon 6 slice, and its number average molecular weight is 30,000 and the relative viscosity is 3.0; the spinning process parameters in step S3 are: spinning temperature 280°C, winding speed 1500m / min, and drafting multiple 4; the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 10%.
[0047] Disclosed is a color-change resistant antibacterial nylon fiber produced by the method for preparing the color-change resistant antibacterial nylon fiber.
[0048] Comparative Example 1 A color change resistant antibacterial nylon fiber and a preparation method thereof, which is similar to Example 1, except that an equal amount of adipic acid is used instead of thiazo[5,4-d]thiazole-2,5-dicarboxylic acid.
[0049] Comparative Example 2 A color change resistant antibacterial nylon fiber and a preparation method thereof, which is similar to Example 1, except that an equal amount of hexamethylenediamine is used instead of 3,7-diamino-5-phenylphenazine chloride.
[0050] In order to further illustrate the beneficial technical effects of the color discoloration resistant antibacterial nylon fibers involved in each embodiment of the present invention, relevant performance tests were carried out on the color discoloration resistant antibacterial nylon fibers involved in Examples 1-5 and Comparative Examples 1-2. The test results are shown in Table 1. The test method is as follows: after the color discoloration resistant antibacterial nylon fibers prepared in each example are woven into socks, the antibacterial rate is tested with reference to GB / T 20944.3-2008, and after washing 30 times, the antibacterial rate is tested again with reference to GB / T 20944.3-2008; after spinning into pre-oriented yarns, the yarns are placed outdoors in the south for 10 days, the outer layer is woven into socks, and the colors before and after the placement are tested with a colorimeter to obtain ΔE.
[0051] It can be seen from Table 1 that the color-discoloration-resistant antibacterial nylon fibers involved in the embodiments of the present invention have more excellent antibacterial properties and water washability, and better color-discoloration resistance. The combined use of thiazolyl[5,4-d]thiazole-2,5-dicarboxylic acid and 3,7-diamino-5-phenylphenazine chloride is beneficial to improving the above properties.
[0052] Table 1
[0053] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing color-discoloration-resistant antibacterial nylon fiber, characterized in that: The steps include: Step S1, preparation of functional polyamide: 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid and a catalyst are added to a high boiling point solvent and mixed evenly to obtain a mixture, then the mixture is added to a reaction kettle, the air in the kettle is replaced with an inert gas, and the mixture is reacted at 115-125° C. under normal pressure for 2-4 hours, then the temperature is raised to 230-250° C., and a polycondensation reaction is carried out at 100-400 Pa for 13-18 hours, then the mixture is cooled to room temperature, adjusted to normal pressure, precipitated in water, the crude product is washed with ethanol for 3-6 times, and then dried in a vacuum drying oven at 85-95° C. to constant weight to obtain a functional polyamide; Step S2, preparation of functional masterbatch: after uniformly mixing the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant prepared in step S1, adding them into a twin-screw extruder for melt blending and extrusion, and pelletizing to obtain functional masterbatch; Step S3, spinning: adding the functional masterbatch prepared in S2 and the nylon slices into a spinning machine, and spinning to obtain nylon fibers; Step S4, ion exchange: soak the nylon fiber prepared in step S3 in a sodium alginate aqueous solution at 50-60° C. for 20-30 hours, take it out and soak it in water for 10-20 hours, and finally dry it to obtain color change resistant antibacterial nylon fiber.
2. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The molar ratio of 3,7-diamino-5-phenylphenazine chloride, thiazo[5,4-d]thiazole-2,5-dicarboxylic acid, catalyst and high boiling point solvent in step S1 is 1:1:(0.8-1):(8-15).
3. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The catalyst is at least one of thiophosphonate, phosphorous acid, and thiophosphoramide; the high boiling point solvent is dimethyl sulfoxide; and the inert gas is any one of nitrogen, helium, neon, and argon.
4. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The mass ratio of the functional polyamide, coupling agent, biomass fiber, antioxidant and lubricant in step S2 is 100:(3-5):(10-20):(1-2):(1-2).
5. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The biomass fiber is at least one of bamboo pulp fiber and hemp pulp fiber; the average diameter of the biomass fiber is 3-9 μm, and the aspect ratio is (20-30):
1.
6. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The coupling agent is at least one of silane coupling agent KH550, silane coupling agent KH560, and silane coupling agent KH570; the antioxidant is at least one of antioxidant 1010 and antioxidant 168; and the lubricant is at least one of pentaerythritol stearate and ethylene bisstearamide.
7. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The temperature of the melt blending extrusion in step S2 is 255-280° C., and the extrusion pressure is 6-9 MPa.
8. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The mass ratio of the functional masterbatch to the nylon slice in step S3 is 1:(5-10); the nylon slice is a nylon 6 slice, the number average molecular weight of which is 20,000-30,000, and the relative viscosity is 2.8-3.
0.
9. The method for preparing the color change resistant antibacterial nylon fiber according to claim 1, characterized in that: The spinning process parameters in step S3 are: spinning temperature 260-280° C., winding speed 1000-1500 m / min, and drafting multiple 2-4; the mass percentage concentration of the sodium alginate aqueous solution in step S4 is 5-10%.
10. A color-discoloration-resistant antibacterial nylon fiber produced by the method for preparing the color-discoloration-resistant antibacterial nylon fiber according to any one of claims 1 to 9.
Citation Information
Patent Citations
A method for preparing colorfast and antibacterial nylon fiber
CN108385203B
Color-change-resistant anti-bacterial polyamide fiber
CN108385202A
Preparation method of color-change-resistant anti-bacterial polyamide fiber
CN108385203A
Anti-infection antibacterial fabric for infants and preparation method thereof
CN111394868A
Color-change-resistant antibacterial polyamide fiber and preparation method thereof
CN116219745A
Cited By
Antistatic biaxially oriented nylon film
CN120310243A
Antibacterial fiber as well as preparation method and fabric thereof
CN121610924A