Silica aerogel composite fiber and preparation method thereof

Hydrophobic silica aerogel composite fibers were prepared through an aqueous system, and the cross-linking reaction between sodium alginate and calcium ions was used to solve the problems of low fiber density and pollution in the existing technology, achieving low thermal conductivity, high efficiency heat insulation and environmental protection Preparation of thermal insulation fibers.

CN119082934APending Publication Date: 2024-12-06SUZHOU ZHONGCUI NANO NEW MATERIAL TECH CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411382771.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the prior art, it is difficult to prepare thermal insulation fibers with thermal conductivity below 0.024W/(m·K), and pure silica aerogel has a low density and is easy to float powder, so the preparation process pollutes the environment.

Method used

Hydrophobic silica aerogel composite fibers are prepared using an aqueous system. By mixing hydrophobic silica aerogel powder with sodium alginate and additives, the cross-linking reaction of sodium alginate and calcium ions is used to form a gel to form Low-density and low thermal conductivity composite fibers avoid the use and contamination of organic solvents.

Benefits of technology

It achieves the performance of efficient thermal insulation performance, reduces the density of composite materials, avoids powder loss, and the entire process is green and environmentally friendly, and there is no organic solvent waste liquid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a silicon dioxide aerogel composite fiber and a preparation method thereof, the silicon dioxide aerogel composite fiber is prepared from hydrophobic silicon dioxide aerogel powder and sodium alginate, and the mass ratio of the hydrophobic silicon dioxide aerogel powder to the sodium alginate is (1-4): 1. The hydrophobic silicon dioxide aerogel powder is used as a main component, so that the heat insulation performance of aerogel is exerted to the greatest extent, and meanwhile, the density of the composite material is reduced; meanwhile, water cannot enter the nanopore structure of the hydrophobic aerogel, and the pore structure of the aerogel cannot be damaged in the drying process, so that the aerogel composite fiber has good hydrophobicity. The aerogel powder is wrapped by gel formed through the rapid cross-linking reaction of sodium alginate and calcium ions, and the dried composite fiber does not have the powder falling condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermal insulation materials, and particularly relates to a silica aerogel composite fiber and a preparation method thereof. Background Art

[0002] The demand for thermal insulation fibers in the textile field is growing day by day, and the preparation of high-efficiency thermal insulation fibers is crucial. However, it is difficult to prepare fibers with thermal conductivity lower than 0.024W / (m·K) with existing technologies. Aerogel is a lightweight solid material with a three-dimensional network nanoporous structure. It has many excellent physical and chemical properties, especially its excellent thermal insulation performance. It is an efficient thermal insulation material.

[0003] However, pure silica aerogel has low density and small particles, and is very easy to float into powder during application, which restricts its practicality and makes it difficult to promote and apply.

[0004] There are two solutions. One is to add a binder to the prepared aerogel powder and then perform secondary molding. The other is to add reinforcing fibers during the sol-gel process to enhance the performance of the aerogel block. The latter method can effectively bring out the advantages of aerogel in high-temperature thermal insulation performance and is relatively environmentally friendly.

[0005] CN108569912A discloses a method for preparing a hydrophobic silica aerogel composite fiber felt, and the obtained composite material product has excellent performance. However, this method requires the use of an organic solvent to dissolve the silica sol, and the use of an acidic catalyst and an alkaline catalyst to adjust the acidity and alkalinity of the silica sol. A large amount of waste liquid is generated during the preparation process, which pollutes the environment. Summary of the invention

[0006] In order to overcome the above disadvantages, one of the purposes of the present invention is to provide a silica aerogel composite fiber and a preparation method thereof, the product has excellent performance, the entire preparation process is an aqueous system, and the preparation process is green and pollution-free.

[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is: a silica aerogel composite fiber, the preparation raw materials include hydrophobic silica aerogel powder and sodium alginate, and the mass ratio of hydrophobic silica aerogel powder to sodium alginate is (1-4):1.

[0008] Exemplarily, the mass ratio of the hydrophobic silica aerogel powder to the sodium alginate is 1:1, 2:1, 3:1, 4:1 or a range consisting of any two thereof.

[0009] Furthermore, the hydrophobic silica aerogel powder satisfies at least one of the following conditions: (a) Tap density is 0.02~0.1 g / cm 3 ; (b) average particle size of 1 to 5 microns; (c) a contact angle with water greater than 150°; (d) Thermal conductivity at 25°C is 0.012~0.018 W / (m·K).

[0010] Furthermore, the preparation raw material also includes an auxiliary agent, and the mass ratio of the hydrophobic silica aerogel powder to the auxiliary agent is 1: (0.03-0.08). Exemplarily, the mass ratio of the hydrophobic silica aerogel powder to the auxiliary agent is 1: 0.03, 1: 0.04, 1: 0.05, 1: 0.06, 1: 0.07, 1: 0.08 or a range consisting of any two of them.

[0011] Furthermore, the auxiliary agent is selected from any one or more of anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, and electrically neutral surfactants; Furthermore, the auxiliary agent is selected from any one or more of ammonium salt dispersants, quaternary ammonium salt dispersants, heterocyclic dispersants, carboxylates, and sulfonates.

[0012] Furthermore, the density of the silica aerogel composite fiber is 0.1-0.3 g / cm 3 , contact angle with water>120°, thermal conductivity<0.024W / (m·K), diameter 400~700μm, breaking strength ≥5.5cN / dtex.

[0013] A method for preparing the silica aerogel composite fiber as described above comprises the following steps: S1, preparing an aqueous paste by mixing hydrophobic silica aerogel powder, an additive and water under high-speed stirring; S2, dissolving sodium alginate in water to prepare a sodium alginate solution with a concentration of 5-10%; S3, mixing the aerogel aqueous paste with the sodium alginate solution and spraying the mixture into a calcium chloride aqueous solution to form composite gel fibers, and drying the composite gel fibers to obtain silica aerogel composite fibers.

[0014] Furthermore, in S1, the mass ratio of the silica aerogel powder to the aqueous paste is 15-25%.

[0015] Furthermore, in S1, the speed of high-speed stirring is 1000-3000 rpm, and the time is 10-180 min.

[0016] Exemplarily, the speed of high-speed stirring is 1000 rpm, 1500 rpm, 2000 rpm, 2500 rpm, 3000 rpm or a range consisting of any two thereof, and the time is 10 min, 30 min, 50 min, 80 min, 100 min, 150 min, 180 min or a range consisting of any two thereof.

[0017] Furthermore, in S2, the viscosity of the sodium alginate solution is 10000-20000 mPa·s.

[0018] Furthermore, in S3, the mass ratio of the aerogel aqueous paste to the sodium alginate solution is (0.25-3):1.

[0019] Exemplarily, the mass ratio of the aerogel aqueous paste to the sodium alginate solution is (0.25-3):1, 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1 or a range consisting of any two of them.

[0020] The beneficial effects of the present invention are: 1) The present invention uses hydrophobic silica aerogel powder as the main component, which can maximize the thermal insulation performance of the aerogel and reduce the density of the composite material; at the same time, water cannot enter the nanoporous structure of the hydrophobic aerogel, and the pore structure of the aerogel will not be destroyed during the drying process, so that the aerogel composite fiber has good hydrophobicity.

[0021] 2) The rapid cross-linking reaction of sodium alginate and calcium ions is used to form a gel to wrap the aerogel powder, and the composite fiber will not fall off after drying.

[0022] 3) The entire preparation process is an aqueous system, which does not produce organic solvent waste liquid, and the preparation process is green and pollution-free. DETAILED DESCRIPTION

[0023] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0024] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0025] A method for preparing a silica aerogel composite fiber comprises the following steps: S1, mixing hydrophobic silica aerogel powder, additives and water to prepare an aqueous paste; Hydrophobic silica aerogel powder, additives and water are mixed in a mass ratio of 1:(0.03-0.08):(3-5) under high-speed stirring to prepare a silica aerogel aqueous paste with a content of 15-25%. The aqueous paste is characterized in that the properties of the hydrophobic silica aerogel powder are restored after drying.

[0026] In some embodiments, the tap density of the hydrophobic silica aerogel powder is 0.02-0.1 g / cm 3 The average particle size is 1-5 μm, the contact angle with water is greater than 150°, and the thermal conductivity is 0.012-0.018 W / (m·K) at 25°C. The hydrophobic silica aerogel powder was purchased from Shandong Huacui Energy Saving Technology Co., Ltd., and the product model is AGP-9010.

[0027] In some embodiments, the auxiliary agent is a surfactant, selected from any one or more of anionic, cationic, nonionic, amphoteric, and electrically neutral types.

[0028] In some embodiments, the auxiliary agent is selected from any one or more of ammonium salt dispersants, quaternary ammonium salt dispersants, heterocyclic dispersants, carboxylates, sulfonates, and the like.

[0029] In some embodiments, the rotation speed of high-speed stirring is 1000-3000 rpm, and the stirring time is 10-180 min.

[0030] S2. Dissolve sodium alginate in 90° C. water under vacuum high-speed stirring to prepare a sodium alginate solution with a concentration of 5-10%. The viscosity of the sodium alginate solution is 10000-20000 mPa·s.

[0031] S3. The aerogel aqueous paste and the sodium alginate solution are fully mixed at 90-100°C and then sprayed into a calcium chloride aqueous solution at room temperature to form a composite gel fiber. Specifically, the wet spinning method comprises the following steps: the spinning solution rate from the spinneret is 1-8 m / min, the winding roller rate is 1-7 m / min, the coagulation bath flow rate is 1-3 m / min, and the composite gel fiber is directly dried to obtain a silica aerogel composite fiber. The density of the silica aerogel composite fiber is 0.1-0.3 g / cm 3 , contact angle with water>120°, thermal conductivity<0.024W / (m·K), diameter 400~700μm, breaking strength ≥5.5cN / dtex.

[0032] In some embodiments, the mass ratio of the aerogel aqueous paste to the sodium alginate solution is (0.25-3):1.

[0033] In some embodiments, the mass ratio of hydrophobic silica aerogel powder to sodium alginate is (1-4):1.

[0034] In some embodiments, the concentration of the calcium chloride solution is 1-3 mol / L.

[0035] Example The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0036] Example 1 S1. Mix hydrophobic silica aerogel powder, additives and water at a mass ratio of 1:0.05:4 at a speed of 2000 rpm for 60 minutes to prepare an aqueous paste with a silica aerogel content of 20%. The aqueous paste is characterized in that the properties of the hydrophobic silica aerogel powder are restored after drying.

[0037] The tap density of hydrophobic silica aerogel powder is 0.02g / cm 3 The average particle size is 1 micron, the contact angle with water is 160°, and the thermal conductivity is 0.012W / (m·K) at 25°C.

[0038] The additive is an anionic surfactant, specifically Tego 750W wetting and dispersing agent.

[0039] S2. Dissolve sodium alginate in 90° C. water under vacuum high-speed stirring to prepare a 5% sodium alginate solution, wherein the viscosity of the sodium alginate solution is 10000 mPa·s.

[0040] S3. The aqueous paste prepared in step S1 and the sodium alginate solution prepared in step S2 are fully mixed at a mass ratio of 0.25:1 at 95°C, and then sprayed into a 1 mol / L calcium chloride aqueous solution at room temperature to form a composite gel fiber. Specifically, the wet spinning method comprises the following steps: the spinning solution rate sprayed from the spinneret is 1 m / min, the winding roller rate is 1 m / min, and the coagulation bath flow rate is 1 m / min. The composite gel fiber is directly dried to obtain a low-density hydrophobic, high-efficiency, heat-insulating silica aerogel composite fiber.

[0041] The mass ratio of hydrophobic silica aerogel powder to sodium alginate is (0.25*20%): (1*5%) = 1:1.

[0042] Example 2 S1. Mix hydrophobic silica aerogel powder, additives and water at a mass ratio of 1:0.05:4 at a speed of 2000 rpm for 60 minutes to prepare an aqueous paste with a silica aerogel content of 20%. The aqueous paste is characterized in that the properties of the hydrophobic silica aerogel powder are restored after drying.

[0043] The tap density of hydrophobic silica aerogel powder is 0.05 g / cm 3 The average particle size is 3 microns, the contact angle with water is 162°, and the thermal conductivity is 0.015W / (m·K) at 25°C.

[0044] The additive is an anionic surfactant, specifically Tego 750W wetting and dispersing agent.

[0045] S2. Dissolve sodium alginate in 90° C. water under vacuum and high-speed stirring to prepare a sodium alginate solution with a concentration of 8%. The viscosity of the sodium alginate solution is 15000 mPa·s.

[0046] S3. The aqueous paste prepared in step S1 and the sodium alginate solution prepared in step S2 are fully mixed at a mass ratio of 1:1 at 95°C, and then sprayed into a calcium chloride aqueous solution at room temperature to form a composite gel fiber. Specifically, the wet spinning method comprises the following steps: the spinning solution rate sprayed from the spinneret is 5m / min, the winding roller rate is 4m / min, and the coagulation bath flow rate is 2m / min. The composite gel fiber is directly dried to obtain a low-density hydrophobic, high-efficiency, heat-insulating silica aerogel composite fiber.

[0047] The mass ratio of hydrophobic silica aerogel powder to sodium alginate is (1*20%): (1*8%) = 2.5:1.

[0048] Example 3 S1. Mix hydrophobic silica aerogel powder, additives and water at a mass ratio of 1:0.05:4 at a speed of 2000 rpm for 60 minutes to prepare an aqueous paste with a silica aerogel content of 20%. The aqueous paste is characterized in that the properties of the hydrophobic silica aerogel powder are restored after drying.

[0049] The tap density of hydrophobic silica aerogel powder is 0.1 g / cm 3 The average particle size is 5 microns, the contact angle with water is 165°, and the thermal conductivity is 0.018W / (m·K) at 25°C.

[0050] The additive is an anionic surfactant, specifically Tego 750W wetting and dispersing agent.

[0051] S2. Dissolve sodium alginate in 90° C. water under vacuum and high-speed stirring to prepare a 10% sodium alginate solution. The viscosity of the sodium alginate solution is 20000 mPa·s.

[0052] S3. The aqueous paste prepared in step S1 and the sodium alginate solution prepared in step S2 are fully mixed at a mass ratio of 2:1 at 95°C, and then sprayed into a calcium chloride aqueous solution at room temperature to form a composite gel fiber. Specifically, the wet spinning method comprises the following steps: the spinning solution rate sprayed from the spinneret is 8m / min, the winding roller rate is 7m / min, and the coagulation bath flow rate is 3m / min. The composite gel fiber is directly dried to obtain a low-density, hydrophobic, high-efficiency, heat-insulating silica aerogel composite fiber.

[0053] The mass ratio of hydrophobic silica aerogel powder to sodium alginate is (2*20%): (1*10%) = 4:1.

[0054] Example 4 S1. Mix hydrophobic silica aerogel powder, additives and water at a mass ratio of 1:0.05:4 at a speed of 1000 rpm for 120 minutes to prepare an aqueous paste with a silica aerogel content of 20%. The aqueous paste is characterized in that the properties of the hydrophobic silica aerogel powder are restored after drying.

[0055] The tap density of hydrophobic silica aerogel powder is 0.05 g / cm 3 The average particle size is 3 microns, the contact angle with water is 162°, and the thermal conductivity is 0.015W / (m·K) at 25°C.

[0056] The additive is an anionic surfactant, specifically Tego 750W wetting and dispersing agent.

[0057] S2. Dissolve sodium alginate in 90° C. water under vacuum and high-speed stirring to prepare a sodium alginate solution with a concentration of 8%. The viscosity of the sodium alginate solution is 15000 mPa·s.

[0058] S3. The aqueous paste prepared in step S1 and the sodium alginate solution prepared in step S2 are fully mixed at a mass ratio of 1:1 at 95°C, and then sprayed into a calcium chloride aqueous solution at room temperature to form a composite gel fiber. Specifically, the wet spinning method comprises the following steps: the spinning solution rate sprayed from the spinneret is 5m / min, the winding roller rate is 4m / min, and the coagulation bath flow rate is 2m / min. The composite gel fiber is directly dried to obtain a low-density hydrophobic, high-efficiency, heat-insulating silica aerogel composite fiber.

[0059] The mass ratio of hydrophobic silica aerogel powder to sodium alginate is (1*20%): (1*8%) = 2.5:1.

[0060] Example 5 S1. Mix hydrophobic silica aerogel powder, additives and water at a mass ratio of 1:0.05:4 at a speed of 3000 rpm for 30 minutes to prepare an aqueous paste with a silica aerogel content of 20%. The aqueous paste is characterized in that the properties of the hydrophobic silica aerogel powder are restored after drying.

[0061] The tap density of hydrophobic silica aerogel powder is 0.05 g / cm 3 The average particle size is 3 microns, the contact angle with water is 162°, and the thermal conductivity is 0.015W / (m·K) at 25°C.

[0062] The additive is an anionic surfactant, specifically Tego 750W wetting and dispersing agent.

[0063] S2. Dissolve sodium alginate in 90° C. water under vacuum and high-speed stirring to prepare a sodium alginate solution with a concentration of 8%. The viscosity of the sodium alginate solution is 15000 mPa·s.

[0064] S3. The aqueous paste prepared in step S1 and the sodium alginate solution prepared in step S2 are fully mixed at a mass ratio of 1:1 at 95°C, and then sprayed into a calcium chloride aqueous solution at room temperature to form a composite gel fiber. Specifically, the wet spinning method comprises the following steps: the spinning solution rate sprayed from the spinneret is 5m / min, the winding roller rate is 4m / min, and the coagulation bath flow rate is 2m / min. The composite gel fiber is directly dried to obtain a low-density hydrophobic, high-efficiency, heat-insulating silica aerogel composite fiber.

[0065] The mass ratio of hydrophobic silica aerogel powder to sodium alginate is (1*20%): (1*8%) = 2.5:1.

[0066] Comparative Example 1 The preparation processes of Comparative Example 1 and Example 2 are basically the same, with the main difference being that in step S3, the mass ratio of the aqueous paste to the sodium alginate solution is 0.2:1, and the mass ratio of the hydrophobic silica aerogel powder to the sodium alginate is (0.2*20%):(1*8%)=0.5:1.

[0067] Comparative Example 2 The preparation processes of Comparative Example 2 and Example 2 are basically the same, with the main difference being that in step S3, the mass ratio of the aqueous paste to the sodium alginate solution is 2:1, and the mass ratio of the hydrophobic silica aerogel powder to the sodium alginate is (2*20%):(1*8%)=5:1.

[0068] Comparative Example 3 The preparation processes of Comparative Example 3 and Example 2 are basically the same, with the main difference being that in step S2, the concentration of the prepared sodium alginate solution is 3%, and the mass ratio of the hydrophobic silica aerogel powder to the sodium alginate is (1*20%):(1*3%)=6.6:1.

[0069] Comparative Example 4 The preparation processes of Comparative Example 4 and Example 2 are basically the same, with the main difference being that in step S2, the concentration of the prepared sodium alginate solution is 15%; in step S3, the mass ratio of the aqueous paste to the sodium alginate solution is 0.2:1, and the mass ratio of the hydrophobic silica aerogel powder to the sodium alginate is (0.2*20%):(1*15%)=0.27:1.

[0070] Comparative Example 5 The preparation process of Comparative Example 5 is basically the same as that of Example 2, the main difference being that in step S1, hydrophilic silica aerogel powder is used instead of hydrophobic silica aerogel powder, and other conditions remain unchanged.

[0071] Experimental Examples The performance of the silica aerogel composite fibers prepared in Examples 1-5 and Comparative Examples 1-5 was tested, and the performance parameter comparison table is shown in Table 1.

[0072] Table 1

[0073] It can be seen from the data in Table 1 that one or more of the parameters of the silica aerogel composite fibers provided in Comparative Examples 1 to 5 are not within the scope of the present invention, and the performance of these silica aerogel composite fibers is poor. However, the silica aerogel composite fibers provided in Examples 1 to 5 of the present invention have good hydrophobicity and breaking strength.

[0074] It can be seen from the test data of Examples 1-3 that as the average particle size of the hydrophobic silica aerogel powder gradually increases, the density of the prepared silica aerogel composite fibers gradually increases, and the thermal conductivity and fiber diameter also gradually increase.

[0075] From the test data of Examples 2, 4 and 5, it can be seen that the stirring speed of preparing the aqueous paste has a certain influence on the performance of the silica aerogel composite fiber. When the stirring speed is 1000-3000 rpm, the prepared silica aerogel composite fiber has good performance. In particular, when the rotation speed is 2000 rpm, the prepared silica aerogel composite fiber has the best hydrophobicity, the contact angle reaches 140°, and the breaking strength reaches 7.9 cN / dtex.

[0076] In Comparative Example 1, since too little hydrophobic silica aerogel powder was added, the content of hydrophobic silica aerogel powder in the fiber was too little, and the hydrophobicity of the powder itself could not be exerted, resulting in the fiber still maintaining its own hydrophilicity and high thermal conductivity.

[0077] In Comparative Example 2, since the amount of sodium alginate added is too small, it is impossible to coat all the added silica aerogel, resulting in part of the aerogel sticking to the fiber surface, thus causing powder loss; at the same time, since the aerogel powder is coated on the surface, the fiber diameter is relatively large. From the test results of Examples 1-5 and Comparative Examples 1-2, it can be seen that the silica aerogel composite fiber prepared with a mass ratio of hydrophobic silica aerogel powder to sodium alginate of (1-4):1 has the best performance.

[0078] In Comparative Example 3, the sodium alginate solution has a concentration of less than 5% and a low viscosity. It cannot form gel fibers well when sprayed into a calcium chloride solution, and the strength of the prepared fibers is relatively low.

[0079] In Comparative Example 4, the concentration of the sodium alginate solution is greater than 10%, the viscosity is high, the silicon dioxide is unevenly dispersed, and the gel fiber formed in the calcium chloride aqueous solution is brittle and the fiber is easily broken. Therefore, from Examples 1-5 and Comparative Examples 3-4, it can be seen that the sodium alginate solution concentration is 5% to 10% optimal, and the gel fiber formed in the calcium chloride aqueous solution has high strength and is not easy to break.

[0080] In Comparative Example 5, the hydrophilic silica aerogel absorbs water into the nanoporous structure, and the capillary pressure generated during the drying process causes the aerogel pore structure to collapse, ultimately losing the nanoporous thermal insulation performance.

[0081] Therefore, the present invention uses hydrophobic silica aerogel powder as the main component, maximizes the thermal insulation performance of the aerogel, and reduces the density of the composite material; by limiting the hydrophobicity of the silica aerogel powder, it is ensured that water cannot enter the nanoporous structure of the hydrophobic aerogel, and the pore structure of the aerogel will not be destroyed during the drying process, so that the aerogel composite fiber has good hydrophobicity. The aerogel powder is wrapped by forming a gel through the rapid cross-linking reaction of sodium alginate and calcium ions, and the composite fiber will not fall off after drying.

[0082] The entire preparation process is an aqueous system, and no organic solvent waste is generated. The preparation process is green and pollution-free.

[0083] The present invention illustrates the detailed process equipment and process flow of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed process equipment and process flow, that is, it does not mean that the present invention must rely on the above-mentioned detailed process equipment and process flow to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, change of structural morphology, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0084] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0085] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0086] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

[0087] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A silica aerogel composite fiber, characterized in that: The preparation raw materials include hydrophobic silica aerogel powder and sodium alginate, and the mass ratio of the hydrophobic silica aerogel powder to the sodium alginate is 1-4:

1.

2. The silica aerogel composite fiber according to claim 1, characterized in that: The hydrophobic silica aerogel powder satisfies at least one of the following conditions: (a) Tap density is 0.02~0.1 g / cm 3 ; (b) average particle size of 1 to 5 microns; (c) a contact angle with water greater than 150°; (d) Thermal conductivity at 25°C is 0.012~0.018 W / (m·K).

3. The silica aerogel composite fiber according to claim 1, characterized in that: The preparation raw materials also include auxiliary agents, and the mass ratio of the hydrophobic silica aerogel powder to the auxiliary agent is 1: (0.03-0.08).

4. The silica aerogel composite fiber according to claim 3, characterized in that: The auxiliary agent is selected from any one or more of anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, and electrically neutral surfactants; Preferably, the auxiliary agent is selected from any one or more of ammonium salt dispersants, quaternary ammonium salt dispersants, heterocyclic dispersants, carboxylates, and sulfonates.

5. The silica aerogel composite fiber according to claim 1, characterized in that: The density of the silica aerogel composite fiber is 0.1-0.3 g / cm 3 , contact angle with water>120°, thermal conductivity<0.024W / (m·K), diameter 400~700μm, breaking strength ≥5.5cN / dtex.

6. A method for preparing the silica aerogel composite fiber according to claims 1 to 5, characterized in that: The steps include: S1, preparing an aqueous paste by mixing hydrophobic silica aerogel powder, an additive and water under high-speed stirring; S2, dissolving sodium alginate in water to prepare a sodium alginate solution with a concentration of 5-10%; S3, mixing the aerogel aqueous paste with the sodium alginate solution and spraying the mixture into a calcium chloride aqueous solution to form composite gel fibers, and drying the composite gel fibers to obtain silica aerogel composite fibers.

7. The method for preparing the silica aerogel composite fiber according to claim 6, characterized in that: In S1, the mass ratio of the silica aerogel powder to the aqueous paste is 15-25%.

8. The method for preparing the silica aerogel composite fiber according to claim 6, characterized in that: In S1, the speed of high-speed stirring is 1000-3000 rpm, and the time is 10-180 min.

9. The method for preparing the silica aerogel composite fiber according to claim 6, characterized in that: In S2, the viscosity of the sodium alginate solution is 10000-20000 mPa·s.

10. The method for preparing the silica aerogel composite fiber according to claim 6, characterized in that: In S3, the mass ratio of the aerogel aqueous paste to the sodium alginate solution is 0.25-3:1.

Citation Information

Patent Citations

  • Preparation method of hydrophobic silica aerogel composite fiber felt material

    CN108569912A