Mechanical enhancement method and device for superfine fiber material
By performing submicron-scale directional welding and crosslinking treatment in microfiber materials, a multi-stage bridge structure is formed, which solves the problem of insufficient mechanical properties of fiber materials in the prior art, and significantly improves the mechanical properties and service life of the material. .
Patent Information
- Application Number
- CN202411182137.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The prior art is difficult to prepare damage-free and high-fast microfiber materials, resulting in insufficient mechanical properties and limiting the expansion of their application fields.
By performing submicron-scale directional welding in microfiber materials, a micro/nano-scale bonding point and cross-linking structure are formed, and the bonding and cross-linking between fibers are enhanced by using technical means such as micro-dot hot rolling and ultraviolet irradiation. Form a multi-stage bridge structure.
It significantly improves the mechanical properties of microfiber materials, including tensile strength, compression recovery rate and porosity, avoids large-area adhesions and melt film phenomena, and extends the service life of the material.
Smart Images

Figure CN119083031A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fiber materials, and in particular to a method and device for mechanically reinforcing ultrafine fiber materials. Background Art
[0002] As a new generation of synthetic fibers, ultrafine fibers generally have a diameter of less than 5 μm, so they have the characteristics of large aspect ratio, high specific surface area, and strong structural adjustability. Membranes or flake materials prepared from ultrafine fibers exhibit small pore size, high porosity, and excellent pore connectivity, so they have great application potential in the fields of filtration separation, lightweight warmth preservation, sound absorption and noise reduction, and high-temperature insulation. However, the excessively small diameter of ultrafine fibers and the loosely slipped overlapping structure between fibers cause their products to exhibit poor pore stability, weak shear resistance, and low tensile strength. These problems reduce the service life of the material during service and limit the subsequent expansion of its application areas. For this reason, how to enhance the mechanical properties of ultrafine fiber materials has become a difficult problem that needs to be solved urgently in the field of fiber manufacturing.
[0003] In response to the above problems, researchers have conducted relevant research in this field. In the manufacture of high-strength polymer fiber membrane materials, Patent 202311161572.3 re-immerses the prepared fiber membrane material in a solvent (or fumigates it in a solvent atmosphere) to slightly dissolve the fiber surface to ensure initial adhesion between the fibers, and then hot-rolls the initially bonded fiber membrane so that the fibers form a tighter adhesion structure, avoiding the phenomenon of fiber membrane stratification; however, this method uses solvent to dissolve the fibers, and uses the hot rolling process again to complete the construction of the adhesion structure, which will cause large-area adhesion or even melt film phenomenon in the material, destroying the structural integrity and performance of the fiber membrane. Patent 201910675001.9 soaks the drug sustained-release membrane prepared by electrospinning in a UV crosslinker and crosslinks the fiber membrane under UV light; in this process, the UV crosslinker is applied by immersion. Under the action of surface tension, the crosslinker forms a reagent film between the fibers and forms a closed-cell structure after curing, which destroys the performance of the fiber membrane; in addition, treating the fiber membrane by immersion will cause a large amount of reagent waste. In the manufacture of high-strength fiber flake materials, Patent 202110662354.2 adds skeleton fibers with a low melting point surface to rabbit hair fibers, and prepares three-dimensional thermal insulation flakes by web laying technology; then, it is baked in a large oven and hot-rolled to make the skeleton fibers adhere and weld to the rabbit hair fibers to improve the mechanical properties of the fiber flakes; however, the hot rolling process in this scheme will cause large-area adhesion between the skeleton fibers and the skeleton fibers, and the skeleton fibers and the rabbit hair fibers, thereby reducing the fluffiness and thermal insulation performance of the fiber flakes.
[0004] Therefore, designing a damage-free, high-strength mechanical enhancement method to prepare ultrafine fiber materials with high mechanical properties is the key to the continued development of this field. Summary of the invention
[0005] The purpose of the present invention is to provide a method and device for mechanical enhancement of ultrafine fiber materials in order to overcome the problem that the prior art cannot prepare ultrafine fiber materials that are both damage-free and high-fastness.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] One of the technical solutions of the present invention is to provide a method for mechanically enhancing an ultrafine fiber material, wherein submicron-scale directional welding is performed between ultrafine fibers to obtain an ultrafine fiber material having submicron-scale bonding points, and the interaction between the submicron-scale bonding points is utilized to obtain an ultrafine fiber material having enhanced mechanical properties.
[0008] In some specific embodiments, the ultrafine fiber material includes an ultrafine fiber membrane or an ultrafine fiber flake. When the ultrafine fiber material is an ultrafine fiber membrane, the method for enhancing the mechanical properties of the ultrafine fiber membrane includes the following steps:
[0009] S1-1, subjecting the ultrafine fiber membrane material to micro-point hot rolling reaction to form an ultrafine fiber membrane with micron-level fusion bonding points;
[0010] S1-2, subjecting the ultrafine fiber membrane with micron-scale fusion bonding points obtained in step S1-1 to ultraviolet irradiation, so that nanoscale crosslinks are formed between the fiber intersections, forming a welding structure at a micro / nano-scale, and obtaining an ultrafine fiber membrane with enhanced mechanical properties;
[0011] When the ultrafine fiber material is an ultrafine fiber flake, the method for enhancing the mechanical properties of the ultrafine fiber flake comprises the following steps:
[0012] S2-1, attaching micron-sized sol particles to ultrafine fiber flakes under the traction of negative pressure and electrostatic force, and transferring the micron-sized sol particles to the fiber overlap under capillary action to form ultrafine fiber flakes with sol coating points;
[0013] S2-2, heating the ultrafine fiber flakes with sol-coated points formed at the fiber overlaps obtained in step S2-1 to form a micro-nano scale welding structure, thereby obtaining ultrafine fiber flakes with enhanced mechanical properties.
[0014] In some specific embodiments, in step S1-1, the ultrafine fiber membrane material is an ultrafine organic polymer fiber membrane material, and the ultrafine organic polymer fiber membrane material is selected from polyurethane, polyethylene oxide, polyamide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, aramid 1313, polymethyl methacrylate, polyimide, polystyrene, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polysulfone, polyethyleneimine, polyimide, polytrimethylene terephthalate or polyvinyl butyral fiber, and is composed of any one or more thereof;
[0015] The raw materials used for the ultrafine fiber membrane material include low melting point elastic oligomers, photoreactive reagents and spinning liquid, wherein:
[0016] The low melting point elastic oligomer is selected from any one or more of thermoplastic polyurethane elastomer, polyolefin elastomer, dynamically vulcanized polyolefin elastomer, polystyrene elastomer, polyether ester elastomer or polyamide elastomer, and the final concentration of the low melting point elastic oligomer in the raw material is 0.5-8wt%;
[0017] The photoreactive reagent comprises a photoinitiator and a photocrosslinker, wherein the photoinitiator is selected from any one or more of TPO (diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide), TPO-L (ethyl 2,4,6-trimethylbenzoylphenylphosphonate), 907 initiator, ITX (2-isopropylthioxanthone), 184 initiator, 1173 initiator, BDK (benzoin dimethyl ether), OMBB (methyl o-benzoylbenzoate), BP (benzophenone), CBP (4-chlorobenzophenone), PBZ (biphenylbenzophenone), 369 initiator, 819 initiator, 754 initiator, 127 initiator, 784 initiator or TMO (2,4,6-trimethylbenzoyl-di(p-tolyl)phosphine oxide);
[0018] The photocrosslinking agent is selected from any one or more of 1,4-butanediol dimethacrylate, ethylene glycol dimethacrylate, hexanediol dimethacrylate, trimethylolpropane trimethacrylate, N,N-methylene acrylamide or epichlorohydrin;
[0019] The final concentration of the photoinitiator in the raw material is 0.3-3 wt %, and the final concentration of the photocrosslinker in the raw material is 0.5-5 wt %.
[0020] In some specific embodiments, the spinning solution of the ultrafine organic polymer fiber membrane material is mainly composed of 10-60wt% organic polymer and solvent, wherein the organic polymer is selected from any one or more of polyurethane, polyethylene oxide, polyamide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, aramid 1313, polymethyl methacrylate, polyimide, polystyrene, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polysulfone, polyethyleneimine, polyimide, polytrimethylene terephthalate or polyvinyl butyral. The solvent is selected from any one or more of N,N-dimethylformamide, N,N-dimethylacetamide, ethanol, acetic acid, dimethyl sulfoxide, toluene, acetone, cyclohexane, isobutanol, dichloromethane, butyl acetate, ethyl acetate or chloroform.
[0021] In some specific embodiments, in step S1-1, the method of the micro-point hot rolling reaction is: using a small-sized rigid rolling point with a diameter of 1 to 30 μm, a hot rolling temperature of 100 to 350° C., a loading pressure of 2 to 8 MPa, and a hot pressing time of 2 to 10 s.
[0022] More preferably, the material of the small-sized rigid rolling point is selected from any one of silicon carbide, brown corundum, white corundum and diamond.
[0023] In some specific embodiments, in step S1-2, the ultraviolet wavelength during the ultraviolet irradiation is 365-405 nm, and the irradiation intensity is 500-3000 mW.
[0024] In some specific embodiments, in step S2-1, the ultrafine fiber flake material is an ultrafine organic polymer fiber flake material or an ultrafine inorganic fiber flake material, wherein:
[0025] The ultrafine organic polymer fiber flakes are selected from any one or more of polyurethane, polyethylene oxide, polyamide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, aramid 1313, polymethyl methacrylate, polyimide, polystyrene, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polysulfone, polyethyleneimine, polyimide, polytrimethylene terephthalate or polyvinyl butyral fiber;
[0026] The ultrafine inorganic fiber flakes are selected from ultrafine inorganic fiber flakes composed of any one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and mullite fibers;
[0027] The micron-sized sol particles are selected from any one of styrene, acrylic acid, vinyl acetate-acrylic acid, styrene-vinyl acid, vinyl acetate-versatile carbonic acid-acrylic acid, natural rubber, environmentally friendly resin, silica sol, aluminum sol, zirconium sol, titanium sol, silicon-aluminum sol or silicon-zirconium sol, and have a solid content of 20 to 60 wt %. The diameter of the micron-sized sol particles is 1 to 10 μm.
[0028] In some specific embodiments, the spinning solution of the ultrafine organic polymer fiber flake material is mainly composed of 10-60wt% organic polymer and solvent, wherein the organic polymer is selected from any one or more of polyurethane, polyethylene oxide, polyamide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, aramid 1313, polymethyl methacrylate, polyimide, polystyrene, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polysulfone, polyethyleneimine, polyimide, polytrimethylene terephthalate or polyvinyl butyral. The solvent is selected from any one or more of N,N-dimethylformamide, N,N-dimethylacetamide, ethanol, acetic acid, dimethyl sulfoxide, toluene, acetone, cyclohexane, isobutanol, dichloromethane, butyl acetate, ethyl acetate or chloroform.
[0029] In some specific embodiments, the spinning solution of the ultrafine inorganic fiber flake material is mainly composed of 40-70wt% of inorganic raw materials and solvents, and the inorganic raw materials are selected from any one or more of tetraethyl orthosilicate, tetraethyl orthosilicate, tetra-n-butoxysilane, tetra-n-propoxysilane, trimethylsilyl acetate, vinyltriethoxysilane, titanium tetramethoxide, titanium tetraethoxide, titanium n-propoxide, titanium isopropoxide, titanium n-butoxide, titanium isobutoxide, titanium tert-butoxide, titanium tetrapentanol, titanium isooctoxide, zirconium tetramethoxide, zirconium tetraethoxide, zirconium n-propoxide, zirconium isopropoxide, zirconium n-butoxide, zirconium isobutoxide, zirconium tert-butoxide, zirconium tetrapentanol, trimethoxyaluminum, aluminum triethoxide, tri-n-propoxyaluminum, aluminum isopropoxide, aluminum n-butoxide, aluminum sec-butoxide or aluminum tert-butoxide. The solvent is selected from any one or more of ethanol, n-propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, n-pentanol, ethylene glycol, butanediol, hexanediol, glycerol, acetic acid, and water.
[0030] As a more preferred embodiment, when the ultrafine fiber flakes are ultrafine organic polymer fiber flakes, the sol particles are selected from any one of acrylic acid, styrene, vinyl acetate-acrylic acid, styrene-vinyl acid, vinyl acetate-versatile acid-acrylic acid, natural rubber or environmentally friendly resin, and the solid content thereof is 20 to 50 wt %;
[0031] When the ultrafine fiber flakes are ultrafine inorganic fiber flakes, the sol particles are selected from any one of silica sol, aluminum sol, zirconium sol, titanium sol, silicon-aluminum sol or silicon-zirconium sol, and the solid content thereof is 40-60wt%.
[0032] In some specific embodiments, in step S2-2, the heating method is microwave-assisted heating, the temperature of microwave-assisted heating is 20-800° C., and the frequency is 3000-300000 MHz. Microwave-assisted heating allows microwaves to penetrate deep into the material to quickly heat small molecules and form a submicro-scale welding structure.
[0033] The second technical solution of the present invention is to provide a mechanical reinforcement device for ultrafine fiber materials, which is used to implement the mechanical reinforcement method for ultrafine fiber materials as described in one of the above technical solutions, comprising:
[0034] Spinning system, used for spinning into ultra-fine fiber materials;
[0035] A micro-nano welding system is used to form an ultra-fine fiber material into an ultra-fine fiber material with sub-micron-scale bonding points, and react the sub-micron-scale bonding points to obtain an ultra-fine fiber material with enhanced mechanical properties;
[0036] The winding system is used for rolling and receiving the ultrafine fiber material with enhanced mechanical properties.
[0037] In some specific embodiments, the spinning system uses any one of electrostatic air-jet spinning, solution electrospinning or melt electrospinning.
[0038] In some specific embodiments, the spinning system includes a spinneret for receiving spinning raw materials, a spinning nozzle arranged at the bottom of the spinneret and used for spinning, an auxiliary component arranged at the bottom of the spinning nozzle and used for molding, and a receiving belt for receiving the ultrafine fiber material flowing out through the auxiliary component. The spinning nozzle is also connected to a first high-voltage static power source.
[0039] In some specific embodiments, the ultrafine fiber material includes an ultrafine fiber film or an ultrafine fiber flake.
[0040] When the ultrafine fiber material is an ultrafine fiber membrane, the micro-nano welding system includes a plurality of first transmission belts arranged downstream of the spinning system and used to transmit the ultrafine fiber membrane, a rigid hot rolling roller assembly arranged between two of the first transmission belts and used for micro-spot hot rolling, and an ultraviolet beam assembly arranged downstream of the rigid hot rolling roller assembly and used for ultraviolet irradiation;
[0041] When the ultrafine fiber material is an ultrafine fiber flake, the micro-nano welding system includes a sol coating component disposed downstream of the spinning system and used for releasing sol particles, and a microwave-assisted heating component disposed upstream of the sol coating component and used for heating.
[0042] In some specific embodiments, the rigid hot rolling roller assembly includes an upper rolling roller and a lower rolling roller, the upper rolling roller surface is provided with regularly arranged rigid rolling points, and the lower rolling roller is a rigid roller with a smooth surface.
[0043] The diameter of the rigid rolling point is 1-30 μm, and the material of the rigid rolling point is selected from any one of silicon carbide, brown corundum, white corundum and diamond.
[0044] More preferably, the material of the lower rolling roller is selected from any one of silicon carbide, tungsten carbide, tungsten carbide-titanium carbide-cobalt, and tungsten carbide-titanium carbide-tantalum carbide-cobalt.
[0045] In some specific embodiments, the ultraviolet beam-forming assembly includes an ultraviolet emitter, a concave mirror and a convex mirror sequentially disposed below the ultraviolet emitter.
[0046] In some specific embodiments, the sol coating component includes a second conveyor belt disposed downstream of the spinning system and used to transport the ultrafine fiber flakes, a semi-enclosed shell, a spray component and a dense dot matrix suction component disposed in the semi-enclosed shell and disposed above and below the ultrafine fiber flakes, respectively.
[0047] The spray assembly is used to spray sol to form sol particles, including a spray generator, a second high-voltage static power source, and a plurality of atomizing nozzles connected to the spray generator and the second high-voltage power source.
[0048] The dense dot matrix suction assembly is used to disperse the sol particles inside the fiber flakes, and includes a fractal flow channel plate, suction micropores arranged on the fractal flow channel plate, and a vacuum pump connected to the fractal flow channel plate through an air pipe.
[0049] In some specific embodiments, the microwave-assisted heating assembly includes a third conveyor belt abutting against the second transmission belt, an insulating shell, a microwave generator and a heating roller arranged in the insulating shell and respectively arranged above and below the microfiber flakes, and an air outlet is also provided at the top of the insulating shell.
[0050] The technical principles of the present invention are as follows:
[0051] The present invention achieves submicron-scale bonding points by precisely directional processing of the ultrafine fiber material, and then enhances the mechanical strength of the ultrafine fiber material by reacting the submicron-scale bonding points.
[0052] For the ultrafine fiber membrane material, the present invention pre-embeds low-melting elastic oligomers and photoreactive reagents inside the ultrafine fiber membrane. When the ultrafine fiber membrane passes through a rigid hot roller, the low-melting elastic oligomer melts at high temperature. At this time, it forms extremely small bonding points under the rolling of the ultra-small rigid rolling points, thereby avoiding large-area adhesion of the ultrafine fiber membrane; under the subsequent high-intensity ultraviolet beam radiation, the ultraviolet cross-linking reagent undergoes a photochemical reaction on the surface of the polymer fiber to generate covalent bonds, thereby causing the fiber intersections to undergo cross-linking and curing at a micro / nano graded scale, further enhancing the mechanical properties of the ultrafine fiber membrane material.
[0053] For enhancing the mechanical properties of ultrafine fiber membranes, the present invention mainly performs hot pressing treatment on the fiber membranes through ultra-small rigid rolling points, and the size of the formed physical bonding points is in the submicron scale. This process avoids the large-area melt film phenomenon and ensures the porous structure and flexibility of the fiber membrane. In addition, ultraviolet chemical cross-linking is used to further increase the micro-nano scale welding points between fibers, forming a multi-level bridging structure of physical adhesion-chemical cross-linking, which can disperse the stress at different scales and effectively improve the tensile properties of the fiber membrane material.
[0054] For the ultrafine fiber flake material, the present invention transports the prepared loose ultrafine fiber flakes into a sol-coated component filled with uniformly dispersed micron-sized sol particles, and the sol particles are uniformly diffused into the ultrafine fiber flakes under the traction of negative pressure and electrostatic action, and adhere to the fibers; at this time, the sol particles are gradually directionally stretched to the fiber overlap points under the capillary action formed by the fiber overlap, and form sol-coated points driven by the surface tension of the sol particles; after the ultrafine fiber flakes are transferred to the microwave-assisted heating component, microwaves perform high-frequency heating on the water molecules in the sol-coated points, destroying the stable state inside the sol-coated points, thereby causing the sol-coated points to quickly lose water and solidify, completing the welding of the ultrafine fiber flakes at the micro-nano scale, and greatly improving the mechanical properties of the ultrafine fiber flake material.
[0055] For enhancing the mechanical properties of ultrafine fiber flakes, the present invention mainly forms a mutually bridged structure between fibers by coating sol particles at the fiber overlap points and forming strong micro-nano welding points under high temperature. The tensile force can be efficiently dispersed on each fiber, thereby increasing the tensile properties of the fiber flakes.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] (1) The mechanical properties of the ultrafine fiber materials prepared by the present invention are greatly and effectively improved. Among them, the ultrafine fiber membrane material forms extremely small physical bonding points under the rolling of the ultrafine rigid rolling point, and a large number of chemical crosslinking points occur between the fibers. Through the combined action of physical and chemical crosslinking, the mechanical properties of the ultrafine fiber membrane material are improved to the greatest extent without damaging the fiber membrane material. Compared with the unreinforced fiber membrane, the tensile strength of the ultrafine fiber membrane prepared by the present invention is increased to more than 12MPa.
[0058] The ultrafine fiber flake material is oriented to form stable, high-strength welding points at the fiber overlap points, which maximizes the compression and tensile properties of the material without destroying the porous structure of the fiber flakes; compared with unwelded fiber flakes, its tensile breaking strength is increased to more than 0.3MPa.
[0059] (2) The ultrafine fiber flake material prepared by the present invention also has excellent compression recovery rate and fluffiness. The compression rebound rate of the ultrafine fiber flake material is increased to more than 90%. The ultrafine fiber membrane material prepared also has excellent porosity and elastic recovery rate.
[0060] (3) The present invention also provides a micro-nano welding device for mechanical enhancement of ultrafine fiber materials, which is easy to operate, highly versatile and has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0061] Figure 1 A roadmap for micro-nano welding technology for mechanical enhancement of ultrafine fiber materials.
[0062] Figure 2 Schematic diagram of the spinning system.
[0063] Figure 3 Schematic diagram of the structure of the micro-nano welding system used to prepare ultrafine fiber membrane materials with enhanced mechanical properties.
[0064] Figure 4 for Figure 3 Schematic diagram of the structure of the medium rigidity hot rolling roll assembly.
[0065] Figure 5 for Figure 3 Schematic diagram of the structure of the mid-UV beam-focusing module.
[0066] Figure 6 Schematic diagram of the structure of the micro-nano welding system used to prepare ultrafine fiber flake materials with enhanced mechanical properties.
[0067] Figure 7 for Figure 6 Schematic diagram of the structure of the mesosol-coated component.
[0068] Figure 8 for Figure 7 Schematic diagram of the structure of the middle spray group components.
[0069] Fig. 9 for Figure 7 Schematic diagram of the structure of the medium dense dot matrix suction component.
[0070] Fig.10 for Figure 6 Schematic diagram of the structure of the microwave heating component.
[0071] The following are marked in the figure:
[0072] 11 is a spinneret, 12 is a spinning nozzle, 13 is an auxiliary component, 14 is a first high-voltage static power source, 15 is a receiving belt, and 16 is an ultra-fine fiber material;
[0073] 21 is a rigid hot roller assembly, 211 is an upper roller, 212 is a lower roller, 213 is a rigid nip, 22 is an ultraviolet beam assembly, 221 is an ultraviolet emitter, 222 is a concave mirror, 223 is a convex mirror, 224 is an ultraviolet beam, 23 is a first transmission belt, and 24 is an ultrafine fiber membrane with enhanced mechanical properties;
[0074] 3 is a sol coating component, 31 is a spray component, 311 is a second high-voltage static power source, 312 is a spray generator, 313 is an atomizing nozzle, 314 is a semi-enclosed shell, 32 is a dense dot matrix suction component, 321 is a fractal flow channel plate, 322 is a vacuum pump, 323 is an air pipe, 324 is an air suction micropore, and 33 is a second conveyor belt;
[0075] 4 is a microwave-assisted heating component, 41 is a microwave generator, 42 is a heating roller, 43 is a third conveyor belt, 44 is an air outlet, 45 is a heat-insulating shell, and 46 is a microfiber flake with enhanced mechanical properties. DETAILED DESCRIPTION
[0076] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0077] In the following embodiments, if there is no special description of raw materials or processing technology, it means that they are all conventional commercially available raw materials or conventional processing technologies in the field. If there is no special description of functional components or structures, it means that they are all conventional components or conventional structures used in the field to achieve corresponding functions.
[0078] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0079] In conjunction with the accompanying drawings, some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.
[0080] Embodiment 1:
[0081] like Figure 1 As shown, this embodiment provides a mechanical reinforcement device for ultra-fine fiber materials, comprising:
[0082] Spinning system, used for spinning into ultra-fine fiber materials;
[0083] A micro-nano welding system is used to form an ultra-fine fiber material into an ultra-fine fiber material with sub-micron-scale bonding points, and react the sub-micron-scale bonding points to obtain an ultra-fine fiber material with enhanced mechanical properties;
[0084] The winding system is used for rolling and receiving the ultrafine fiber material with enhanced mechanical properties.
[0085] In this embodiment, the ultrafine fiber material is oriented to obtain submicron-scale bonding points, and the mechanical strength of the ultrafine fiber material is enhanced by these submicron-scale bonding points.
[0086] like Figure 2 As shown, the spinning system can adopt any one of electrostatic air-jet spinning, solution electrostatic spinning or melt electrostatic spinning. Exemplarily, the spinning system can adopt a spinneret 11 for receiving spinning raw materials, a spinning nozzle 12 arranged at the bottom of the spinneret 11 and used for spinning, an auxiliary component 13 such as a heater, an air intake component, etc. arranged at the bottom of the spinning nozzle 12 and used for forming, and a receiving belt 15 for receiving and transmitting the ultrafine fiber material 16 flowing out of the auxiliary component 13, and the spinning nozzle 12 is also connected to a first high-voltage static power source 14. The spinning raw material flows through the spinneret 11, and forms an ultrafine fiber material 16 such as an ultrafine fiber membrane or an ultrafine fiber flake under the action of the electrostatic force or the drawing force of the electrostatic force and the air flow force, and is received on the receiving belt 15. Ultrafine fiber materials of different structures and thicknesses, such as ultrafine fiber membranes or ultrafine fiber flakes, can be obtained by regulating the spinning parameters and combining the auxiliary components 13.
[0087] Embodiment 2:
[0088] Based on the spinning system and winding system provided in Example 1, Figure 3As shown, this embodiment specifically provides a micro-nano welding system for enhancing the mechanical properties of ultrafine fiber membranes, and the micro-nano welding system includes a plurality of first transmission belts 23 that are sequentially connected to the receiving belt 15 and transmit the ultrafine fiber membrane, a rigid hot rolling roller assembly 21 disposed between two of the first transmission belts 23 and used for micro-spot hot rolling, and an ultraviolet beam assembly 22 disposed above the transmission belt 23 and used for ultraviolet irradiation. Directed micro-spot hot rolling physical adhesion occurs through the rigid hot rolling roller assembly 21, combined with ultraviolet chemical cross-linking of the ultraviolet beam assembly 22, while maintaining the original porous structure and flexibility of the fiber membrane, the micro-nano scale welding points are further increased to form a multi-level bridging structure, which can disperse the stress at different scales and effectively improve the mechanical properties of the fiber membrane, such as tensile properties.
[0089] like Figure 4 As shown, in this embodiment, the rigid hot rolling roller assembly 21 includes an upper rolling roller 211 and a lower rolling roller 212. The surface of the upper rolling roller 211 is provided with regularly arranged rigid rolling points 213, and the surface of the lower rolling roller 212 is a rigid roller with a smooth surface. The diameter of the rigid rolling point 213 is 1 to 30 μm, and the material of the rigid rolling point is selected from any one of silicon carbide, brown corundum, white corundum, and diamond. The material of the lower rolling roller 212 is selected from any one of silicon carbide, tungsten carbide, tungsten carbide-titanium carbide-cobalt, and tungsten carbide-titanium carbide-tantalum carbide-cobalt. When the upper rolling roller 211 and the lower rolling roller 212 weld the ultrafine fiber membrane, the rigid rolling point 213 on the upper rolling roller 211 will not have elastic contact with the lower rolling roller 212, which reduces the physical cross-linking points on the surface of the fiber membrane and avoids large-area adhesion.
[0090] like Figure 5 As shown, in this embodiment, the ultraviolet beam assembly 22 includes an ultraviolet emitter 221, a concave mirror 222 and a convex mirror 223 arranged below the ultraviolet emitter 221 in sequence. The ultraviolet light generated by the ultraviolet emitter 221 forms an ultraviolet beam 224 perpendicular to the running direction of the fiber membrane under the beam-gathering effect of the concave mirror 222 and the convex mirror 223, thereby increasing the radiation intensity of the ultraviolet light, greatly improving the efficiency of the cross-linking reaction, and preparing an ultrafine fiber membrane 24 with enhanced mechanical properties. Exemplarily, the light source of the ultraviolet emitter 221 is set as a linear light source, which is highly practical and easy to control.
[0091] Embodiment 3:
[0092] Based on the spinning system and winding system provided in Example 1, Figure 6As shown, this embodiment specifically provides a micro-nano welding system for enhancing the mechanical properties of ultrafine fiber flakes, and the micro-nano welding system includes a second conveyor belt 33 that is sequentially connected to the receiving belt 15 and transmits the ultrafine fiber flakes, a sol coating component 3 for releasing micron-sized sol particles, and a microwave-assisted heating component 4 for heating. Sol coating points are formed at the fiber overlap by the sol coating component 3, and strong micro-nano welding points are formed under the high temperature of the microwave-assisted heating component 4. Since a mutually bridged structure is formed between the fibers, the tensile force can be efficiently dispersed on each fiber, thereby increasing the mechanical properties of the fiber flakes, such as tensile properties.
[0093] like Figure 7-9 As shown, in this embodiment, the sol coating component 3 includes a semi-enclosed shell 314 without a closed inlet and outlet, a spray component 31 and a dense lattice suction component 32 arranged in the semi-enclosed shell 314 and respectively arranged above and below the ultrafine fiber flakes. The spray component 31 is used to spray sol to form micron-sized sol particles, including a spray generator 312, a second high-voltage static power source 311, and a plurality of atomizing nozzles 313 connected to the spray generator 312 and the second high-voltage static power source 311. The exemplary spray generator 312 may be an electrostatic or ultrasonic sprayer. The dense lattice suction component 32 is used to disperse the micron-sized sol particles inside the ultrafine fiber flakes, including a fractal flow channel plate 321, suction micropores 324 arranged on the fractal flow channel plate 321, and a vacuum pump 322 connected to the fractal flow channel plate 321 through an air pipe 323. The voltage of the second high-voltage static power source 311 is set to 1-10 kV, and the operating frequency of the spray generator 312 is set to 10-100 kHZ. Under the dual pulling effect of the electrostatic / ultrasonic sprayer and the high static voltage, the sol forms ultra-fine micron-level sol particles, and the diameter of the sol particles is 1-10 μm. After the vacuum pump 322 of the dense dot matrix suction component 32 is started, the suction speed of the vacuum pump 322 is set to 0.5-2 m / s. 3 / h, the gas evenly enters the fractal flow channel plate 321 from the air suction micropores 324, and the negative pressure formed can evenly disperse the sol particles into the interior of the ultra-fine fiber flakes.
[0094] like Fig.10As shown, in this embodiment, the microwave-assisted heating assembly 4 includes a third conveyor belt 43 abutting against the second conveyor belt 33, a heat-insulating shell 45, a microwave generator 41 and a heating roller 42 disposed in the heat-insulating shell 45 and correspondingly disposed above and below the ultrafine fiber flakes, respectively, and an air outlet 44 is also disposed on the top of the heat-insulating shell 45. The sol-coated points on the ultrafine fiber flakes quickly lose water and become disordered under the action of the electromagnetic waves generated by the microwave generator 41, and quickly form stable and strong welding points under the heat radiation of the heating roller 42, thereby enhancing the mechanical strength of the ultrafine fiber flakes, and preparing an ultrafine fiber flake 46 with enhanced mechanical properties.
[0095] The microwave heating assembly 4 is not limited to curing the sol-coated points on the ultrafine fiber flakes, but can also be used for rapid calcination of ceramic fiber membranes or flake materials. By adjusting the emission frequency of the microwave generator 41, the small molecular chains in the fiber are pre-cracked due to high-frequency vibration, and are quickly removed under the high temperature generated by the heating roller 42, so that a flexible ceramic ultrafine fiber material with small grains and multiple crystal boundaries can be prepared.
[0096] Embodiment 4:
[0097] Using the devices provided in Example 1 and Example 2, this embodiment provides a method for mechanical enhancement of an ultrafine fiber membrane, comprising the following steps:
[0098] (1) A thermoplastic polyurethane elastomer, TOP initiator and ethylene glycol dimethacrylate monomer were added to a polyurethane organic polymer spinning solution (solvent: N,N-dimethylformamide) and uniformly mixed to prepare spinning solutions with elastomer, initiator, reaction monomer and polymer concentrations of 0.5, 0.3, 0.5 and 10 wt %, respectively. A polyurethane ultrafine fiber membrane was prepared by electrostatic air jet spinning.
[0099] (2) The ultrafine fiber membrane obtained by spinning is transported to a rigid hot rolling roller assembly 21 for hot rolling for 2 seconds. The hot rolling temperature is set to 200° C. and the hot rolling pressure is set to 2 MPa to obtain an ultrafine fiber membrane with tiny physical bonding points.
[0100] (3) Subsequently, the ultrafine fiber membrane with tiny physical bonding points is transported to the UV beam assembly 22 for chemical cross-linking. The UV wavelength is set to 365 nm and the irradiation intensity is set to 500 mW, thereby achieving high-strength welding of the ultrafine fiber membrane at the micro-nano scale and obtaining an ultrafine fiber membrane with enhanced mechanical properties.
[0101] The prepared polyurethane ultrafine fiber membrane material has a tensile strength of 20 MPa, a porosity of 89.3%, and an elastic recovery rate of 91.6%.
[0102] Embodiment 5:
[0103] Using the device provided in Example 1, this embodiment provides a method for mechanical enhancement of an ultrafine fiber membrane material, comprising the following steps:
[0104] (1) Polyolefin elastomer, 184 initiator and 1,4-butanediol dimethacrylate monomer were added to polyacrylonitrile organic polymer spinning solution (solvent is N,N-dimethylacetamide) and uniformly mixed to prepare spinning solutions with elastomer, initiator, reaction monomer and polymer concentrations of 4, 1, 5 and 25 wt%, respectively; and polyacrylonitrile ultrafine fiber membranes were prepared by electrostatic air jet spinning.
[0105] (2) The ultrafine fiber membrane obtained by spinning is transported to a rigid hot rolling roller assembly 21 for hot rolling for 10 seconds, and the hot rolling temperature is set to 350° C. and the hot rolling pressure is set to 8 MPa to obtain an ultrafine fiber membrane with tiny physical bonding points.
[0106] (3) Subsequently, the ultrafine fiber membrane with tiny physical bonding points is transported to the UV beam-forming assembly 22 for chemical cross-linking. The UV wavelength is set to 405 nm and the irradiation intensity is set to 3000 mW, thereby achieving high-strength welding of the ultrafine fiber membrane at the micro-nano scale and obtaining an ultrafine fiber membrane with enhanced mechanical properties.
[0107] The prepared polyacrylonitrile ultrafine fiber membrane material has a tensile strength of 15 MPa, a porosity of 85.2%, and an elastic recovery rate of 90%.
[0108] Embodiment 6:
[0109] Using the devices provided in Example 1 and Example 2, this embodiment provides a method for mechanical enhancement of an ultrafine fiber membrane material, comprising the following steps:
[0110] (1) Polyether ester elastomer, TMO initiator and hexanediol dimethacrylate monomer were added to polyvinylidene fluoride organic polymer spinning solution (solvent is N,N-dimethylformamide) and evenly mixed to prepare spinning solutions with elastomer, initiator, reaction monomer and polymer concentrations of 8, 1, 2 and 35 wt%, respectively; and ultrafine fiber membranes were prepared by electrostatic air jet spinning.
[0111] (2) The ultrafine fiber membrane obtained by spinning is transported to a rigid hot rolling roller assembly 21 for hot rolling for 5 seconds. The hot rolling temperature is set to 220° C. and the hot rolling pressure is set to 6 MPa to obtain an ultrafine fiber membrane with tiny physical bonding points.
[0112] (3) Subsequently, the ultrafine fiber membrane with tiny physical bonding points is transported to the UV beam-forming assembly 22 for chemical cross-linking. The UV wavelength is set to 395 nm and the irradiation intensity is set to 1500 mW, thereby achieving high-strength welding of the ultrafine fiber membrane at the micro-nano scale and obtaining an ultrafine fiber membrane with enhanced mechanical properties.
[0113] The prepared polyvinylidene fluoride ultrafine fiber membrane material has a tensile strength of 12 MPa, a porosity of 88.2%, and an elastic recovery rate of 94.3%.
[0114] Embodiment 7:
[0115] Using the device provided in Example 3, this embodiment provides a method for mechanically reinforcing a superfine fiber flake material, and the specific steps are as follows:
[0116] (1) Polystyrene and N,N-dimethylformamide are prepared into a 10 wt% spinning solution, and a polystyrene ultra-fiber flake material is prepared by electrostatic air-spinning, and transported to the sol-coated component 3. At this time, acrylic sol particles with a solid content of 40 wt% and a diameter of 1 μm are uniformly dispersed in the semi-enclosed shell 314; at 0.5 m 3 At a suction rate of 1000 μg / h, the sol particles diffuse evenly into the microfiber flakes and move to the overlapping points to form coating points under the capillary action of the overlapping fibers.
[0117] (2) The fiber flakes are then transferred to a microwave heating assembly 4, and the microwave frequency is set to 3000 MHz and the heating temperature is set to 60°C. The sol-coated points quickly lose water and solidify under the high-frequency vibration of the microwaves, forming stable and strong welding points at the overlap points, thereby obtaining ultrafine fiber flakes with enhanced mechanical properties.
[0118] The thickness of the prepared polystyrene ultrafine fiber flake material is 3 cm, the tensile strength is 0.73 MPa, the compression resilience is 95%, and the volume density is 2.5 mg / cm 3 .
[0119] Embodiment 8:
[0120] Using the device provided in Example 3, this embodiment provides a method for mechanically reinforcing a superfine fiber flake material, and the specific steps are as follows:
[0121] (1) Polyacrylonitrile and dimethyl sulfoxide are prepared into a spinning solution of 12 wt%, and a polyacrylonitrile ultra-fiber flake material is prepared by electrostatic air-jet spinning, and then transported to the sol-coated component 3. At this time, styrene sol particles with a solid content of 25 wt% and a diameter of 7 μm are uniformly dispersed in the semi-enclosed shell 314; at 2 m 3 At a suction rate of 1000 μg / h, the sol particles diffuse evenly into the microfiber flakes and move to the overlapping points to form coating points under the capillary action of the overlapping fibers.
[0122] (2) The fiber flakes are then transferred to a microwave heating assembly 4, and the microwave frequency is set to 200,000 MHz and the heating temperature is set to 80°C. The sol-coated points quickly lose water and solidify under the high-frequency vibration of the microwaves, forming stable and strong welding points at the overlap points, thereby obtaining ultrafine fiber flakes with enhanced mechanical properties.
[0123] The thickness of the prepared polyimide ultrafine fiber flake material is 4 cm, the tensile strength is 0.68 MPa, the compression resilience is 93%, and the volume density is 5 mg / cm 3 .
[0124] Embodiment 9:
[0125] Using the device provided in Example 3, this embodiment provides a method for mechanically reinforcing a superfine fiber flake material, and the specific steps are as follows:
[0126] (1) A 40 wt% spinning solution is prepared by preparing a ethyl orthosilicate and acetic acid solution, and 1 wt% polyvinyl alcohol as an auxiliary raw material is added, and a silica ultrafine fiber flake material is prepared by electrostatic air-jet spinning, and then transported to the sol-coated component 3. At this time, silica sol particles with a solid content of 50 wt% and a diameter of 3 μm are evenly dispersed in the semi-enclosed shell 314. 3 At a suction rate of 1000 μg / h, the sol particles diffuse evenly into the microfiber flakes and move to the overlapping points to form coating points under the capillary action of the overlapping fibers.
[0127] (2) The fiber flakes are then transferred to a microwave heating assembly 4, and the microwave frequency is set to 300,000 MHz and the heating temperature is set to 700° C. The sol-coated points quickly lose water and solidify under the high-frequency vibration of the microwaves, forming stable and strong welding points at the overlap points, thereby obtaining ultrafine fiber flakes with enhanced mechanical properties.
[0128] The thickness of the prepared silica ultrafine fiber flake material is 5 cm, the tensile strength is 0.37 MPa, the compression resilience is 92%, and the volume density is 3.7 mg / cm 3 .
[0129] Embodiment 10:
[0130] Using the device provided in Example 3, this embodiment provides a method for mechanically reinforcing a superfine fiber flake material, and the specific steps are as follows:
[0131] (1) Tetraethyl orthosilicate, aluminum isopropoxide, aluminum nitrate and ethanol are prepared into a 53 wt% spinning solution, and the mullite superfiber flake material prepared by the electrostatic air jet spinning device is transported to the sol coating component 3. At this time, the semi-enclosed shell 314 is evenly dispersed with silica sol particles with a solid content of 60 wt% and a diameter of 2 μm; at 1.5 m 3At a suction rate of 1000 μg / h, the sol particles diffuse evenly into the microfiber flakes and move to the overlapping points to form coating points under the capillary action of the overlapping fibers.
[0132] (2) The fiber flakes are then transferred to a microwave-assisted heating tunnel furnace, and the microwave frequency is set to 300,000 MHz and the heating temperature is set to 800°C. The sol-gel coated points quickly lose water and solidify under the high-frequency vibration of the microwave, forming stable and strong welding points at the overlap points, thereby obtaining ultrafine fiber flakes with enhanced mechanical properties.
[0133] The thickness of the prepared mullite ultrafine fiber flake material is 3 cm, the tensile strength is 0.42 MPa, the compression resilience is 90%, and the volume density is 4.3 mg / cm 3 .
[0134] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for mechanical enhancement of ultrafine fiber materials, characterized in that: Submicron-scale directional welding is performed between ultrafine fibers to obtain an ultrafine fiber material with submicron-scale bonding points, and the interaction of the submicron-scale bonding points is utilized to obtain an ultrafine fiber material with enhanced mechanical properties.
2. The mechanical strengthening method of ultrafine fiber material according to claim 1, characterized in that: The ultrafine fiber material includes an ultrafine fiber membrane or an ultrafine fiber flake. When the ultrafine fiber material is an ultrafine fiber membrane, the mechanical enhancement method of the ultrafine fiber membrane includes the following steps: S1-1, subjecting the ultrafine fiber membrane material to micro-point hot rolling reaction to form an ultrafine fiber membrane with micron-level fusion bonding points; S1-2, subjecting the ultrafine fiber membrane with micron-scale fusion bonding points obtained in step S1-1 to ultraviolet irradiation, so that nanoscale crosslinks are formed between the fiber intersections, forming a welding structure at a micro / nano-scale, and obtaining an ultrafine fiber membrane with enhanced mechanical properties; When the ultrafine fiber material is an ultrafine fiber flake, the mechanical reinforcement method of the ultrafine fiber flake comprises the following steps: S2-1, attaching micron-sized sol particles to the ultrafine fiber material under the traction of negative pressure and electrostatic force, and transferring the micron-sized sol particles to the fiber overlap under the capillary action to form ultrafine fiber flakes at the sol-coated points; S2-2, heating the ultrafine fiber flakes with sol-coated points formed at the fiber overlaps obtained in step S2-1 to form a micro-nano scale welding structure, thereby obtaining ultrafine fiber flakes with enhanced mechanical properties.
3. The mechanical strengthening method of ultrafine fiber material according to claim 2, characterized in that: In step S1-1, the ultrafine fiber membrane material is an ultrafine organic polymer fiber membrane material, and the ultrafine organic polymer fiber membrane material is selected from polyurethane, polyethylene oxide, polyamide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, aramid 1313, polymethyl methacrylate, polyimide, polystyrene, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polysulfone, polyethyleneimine, polyimide, polytrimethylene terephthalate or polyvinyl butyral fiber, and is composed of any one or more thereof; The raw materials used for the ultrafine fiber membrane material include low melting point elastic oligomers, photoreactive reagents and spinning liquid, wherein: The low melting point elastic oligomer is selected from any one or more of thermoplastic polyurethane elastomer, polyolefin elastomer, dynamically vulcanized polyolefin elastomer, polystyrene elastomer, polyether ester elastomer or polyamide elastomer, and the final concentration of the low melting point elastic oligomer in the raw material is 0.5-8wt%; The photoreactive reagent comprises a photoinitiator and a photocrosslinker, wherein the photoinitiator is selected from any one or more of TPO, TPO-L, 907 initiator, ITX, 184 initiator, 1173 initiator, BDK, OMBB, BP, CBP, PBZ, 369 initiator, 819 initiator, 754 initiator, 127 initiator, 784 initiator or TMO; The photocrosslinking agent is selected from any one or more of 1,4-butanediol dimethacrylate, ethylene glycol dimethacrylate, hexanediol dimethacrylate, trimethylolpropane trimethacrylate, N,N-methylene acrylamide or epichlorohydrin; The final concentration of the photoinitiator in the raw material is 0.3-3 wt %, and the final concentration of the photocrosslinker in the raw material is 0.5-5 wt %.
4. The mechanical reinforcement method of ultrafine fiber material according to claim 2, characterized in that: In step S1-1, the micro-spot hot rolling reaction method is: using a small-sized rigid rolling point with a diameter of 1 to 30 μm, a hot rolling temperature of 100 to 350° C., a loading pressure of 2 to 8 MPa, and a hot pressing time of 2 to 10 s; In step S1-2, the ultraviolet wavelength during the ultraviolet irradiation is 365-405 nm, and the irradiation intensity is 500-3000 mW.
5. The mechanical strengthening method of ultrafine fiber material according to claim 2, characterized in that: In step S2-1, the ultrafine fiber flake material is an ultrafine organic polymer fiber flake material or an ultrafine inorganic fiber flake material, wherein: The ultrafine organic polymer fiber flakes are selected from any one or more of polyurethane, polyethylene oxide, polyamide, polyvinyl chloride, polyvinylidene fluoride, polycarbonate, aramid 1313, polymethyl methacrylate, polyimide, polystyrene, polybenzimidazole, polyethylene terephthalate, polycaprolactone, polylactic acid, polyhydroxybutyrate, polyacrylonitrile, polyvinyl alcohol, polyethylene, polysulfone, polyethyleneimine, polyimide, polytrimethylene terephthalate or polyvinyl butyral fiber; The ultrafine inorganic fiber flakes are selected from ultrafine inorganic fiber flakes composed of any one or more of silicon oxide, aluminum oxide, zirconium oxide, titanium oxide, and mullite fibers; The micron-sized sol particles are selected from any one of styrene, acrylic acid, vinyl acetate-acrylic acid, styrene-vinyl acid, vinyl acetate-versatile carbonic acid-acrylic acid, natural rubber, environmentally friendly resin, silica sol, aluminum sol, zirconium sol, titanium sol, silicon-aluminum sol or silicon-zirconium sol, and have a solid content of 20 to 60 wt %. The diameter of the micron-sized sol particles is 1 to 10 μm.
6. The mechanical strengthening method of ultrafine fiber material according to claim 2, characterized in that: In step S2-2, the heating method is microwave-assisted heating, the heating temperature is 20-800°C, and the frequency is 3000-300000 MHz.
7. A mechanical reinforcement device for ultrafine fiber materials, used for implementing the mechanical reinforcement method for ultrafine fiber materials according to any one of claims 1 to 6, comprising: Spinning system, used for spinning into ultra-fine fiber materials; A micro-nano welding system is used to form an ultra-fine fiber material into an ultra-fine fiber material with sub-micron-scale bonding points, and react the sub-micron-scale bonding points to obtain an ultra-fine fiber material with enhanced mechanical properties; The winding system is used for rolling and receiving the ultrafine fiber material with enhanced mechanical properties.
8. The mechanical reinforcement device of ultrafine fiber material according to claim 7, characterized in that: The ultrafine fiber material includes an ultrafine fiber film or an ultrafine fiber flake. When the ultrafine fiber material is an ultrafine fiber membrane, the micro-nano welding system comprises a plurality of first transmission belts (23) arranged downstream of the spinning system and used to transmit the ultrafine fiber membrane, a rigid hot rolling roller assembly (21) used for micro-spot hot rolling, and an ultraviolet beam assembly (22) arranged downstream of the rigid hot rolling roller assembly (21) and used for ultraviolet irradiation; When the ultrafine fiber material is an ultrafine fiber flake, the micro-nano welding system comprises a sol coating component (3) disposed downstream of the spinning system and used for releasing sol particles, and a microwave-assisted heating component (4) disposed downstream of the sol coating component (3) and used for heating.
9. The mechanical reinforcement device of ultrafine fiber material according to claim 8, characterized in that: The rigid hot rolling roller assembly (21) comprises an upper rolling roller (211) and a lower rolling roller (212); the surface of the upper rolling roller (211) is provided with regularly arranged rigid rolling points (213); and the surface of the lower rolling roller (212) is a rigid roller with a smooth surface; The diameter of the rigid rolling point (213) is 1 to 30 μm, and the material of the rigid rolling point is selected from any one of silicon carbide, brown corundum, white corundum and diamond; The ultraviolet beam-focusing component (22) comprises an ultraviolet emitter (221), a concave mirror (222) and a convex mirror (223) which are sequentially arranged below the ultraviolet emitter (221).
10. The mechanical reinforcement device of ultrafine fiber material according to claim 8, characterized in that: The sol coating component (3) comprises a second conveyor belt (33) arranged downstream of the spinning system and used for conveying the ultrafine fiber flakes, a semi-enclosed shell (314), a spray component (31) and a dense dot matrix suction component (32) arranged in the semi-enclosed shell (314) and respectively arranged above and below the ultrafine fiber flakes, The spray assembly (31) is used to spray sol to form micron-sized sol particles, and comprises a spray generator (312), a second high-voltage static power source (311), and a plurality of atomizing nozzles (313) connected to the spray generator (312) and the second high-voltage static power source (311). The dense dot matrix suction component (32) is used to disperse the sol particles inside the fiber flakes, and comprises a fractal flow channel plate (321), suction micropores (324) provided on the fractal flow channel plate (321), and a vacuum pump (322) connected to the fractal flow channel plate (321) via an air pipe (323); The microwave heating assembly (4) comprises a third conveyor belt (43) abutting against the second conveyor belt (33), a heat-insulating outer shell (45), a microwave generator (41) and a heating roller (42) arranged in the heat-insulating outer shell (45) and respectively arranged above and below the microfiber flakes, and an air outlet (44) is also arranged at the top of the heat-insulating outer shell (45).
Citation Information
Patent Citations
Preparation of a sustained-release membrane for poorly soluble drugs
CN110279677B
High-heat-preservation comfortable rabbit wool fiber flocculus material
CN113355805A
Breathable adhesive tape and application thereof
CN117186784A
Shaped article and composite material and method for producing same
CA1197269A
Material such as film, fiber, woven and nonwoven fabric with adsorbancy
CN103648611A