Composite fabric with function of blocking and decomposing PAHs (polycyclic aromatic hydrocarbons) smoke as well as preparation method and application of composite fabric

By using a double-layer fabric with high temperature-resistant modified TiO2-CN catalyst and zirconium hydroxide particles in protective clothing, the problem of PAHs flue gas barrier and decomposition at the fire site was solved, and efficient removal and cleaning of toxic substances was achieved, improving the The safety and ease of cleaning of protective clothing.

CN119083155APending Publication Date: 2024-12-06TIANJIN FIRE SCI & TECH RES INST OF MEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411232338.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing protective clothing cannot effectively block and decompose polycyclic aromatic hydrocarbons (PAHs) flue gas at fire rescue sites, resulting in the accumulation of carcinogens in clothing and affecting personnel's health and safety.

Method used

Using high-temperature-resistant modified TiO2-CN catalyst and zirconium hydroxide particles, the assembly and ultrasonic dispersion of polydimethylsiloxane (PDMS) is used to form a double-layer fabric, enhancing the catalytic activity and adsorption capacity under high temperature environments, and realizing PAHs Blocking and decomposition of smoke.

Benefits of technology

It improves the barrier and decomposition efficiency of PAHs flue gas, reduces the migration and accumulation of pollutants, simplifies the cleaning process, and enhances the safety and cleanability of protective clothing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083155A_ABST
    Figure CN119083155A_ABST
Patent Text Reader

Abstract

The invention provides a composite fabric with a function of blocking and decomposing PAHs smoke as well as a preparation method and application of the composite fabric, the composite fabric is a double-layer fabric compounded with functional particles, and the functional particles comprise a high-temperature-resistant modified TiO2-CN catalyst and high-temperature-resistant modified zirconium hydroxide. Firstly, the migration capability of PAHs in the multi-layer structure of the protective clothing can be reduced, so that toxic pollution is blocked on the outer layer surface of the protective clothing; secondly, the decomposition level of PAHs is improved, so that the fabric has poison digestion capability; and finally, by improving the surface characteristics of the protective clothing, the clothing is easier to clean, and toxic substances are easier to strip from a fabric matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of personal protective equipment, and in particular relates to a composite fabric with the function of blocking and decomposing PAHs smoke, and a preparation method and application thereof. Background Art

[0002] Polycyclic aromatic hydrocarbons (PAHs) in fire smoke can easily induce colon cancer, lung cancer, prostate cancer and skin cancer. Personal protective equipment is the first barrier to protect life safety during the rescue process, but a large number of PAHs carcinogens were found in human skin and urine after the rescue. It can be seen that PAHs pollutants can migrate through clothing and pose a threat to human percutaneous absorption. In the real fire environment, 70-90% of fire smoke particles are distributed in 0.01-0.11μm, and PAHs exist in the gas phase or attach to solid smoke particles. During the process of smoke pollution of protective clothing, the PAHs content in the middle layer is the highest, indicating that PAHs smoke is adsorbed and accelerated to penetrate the pore structure of the outer fabric under the action of high temperature. Domestic and foreign studies have shown that the PAHs content in the middle layer of fire-fighting protective clothing after smoke pollution is 2-4 times that of the outer layer; the water washing process can achieve a maximum PAHs removal rate of 85% of the outer fabric of the protective clothing, while the cleaning efficiency of the middle layer is less than 50%. Even if the outer structure of the protective clothing contains a waterproof coating (fluorocarbon finishing agent), it can neither enhance the ability to block the migration of PAHs smoke nor improve the cleaning effect of PAHs smoke pollution, resulting in the accumulation of carcinogenic PAHs remaining in the fabric structure over time, which seriously threatens the safety and health of personnel. However, the application of conventional catalysts is mostly limited to room temperature environments. As the temperature rises, the catalytic activity decreases, and the application effect in high-temperature fields is limited. Therefore, it is necessary to develop a multifunctional fabric that can block and decompose PAHs and is easy to clean in the high-temperature service environment at the fire rescue site. Summary of the invention

[0003] In view of this, the present invention aims to overcome the defects in the prior art and proposes a composite fabric with the function of blocking and decomposing PAHs smoke and a preparation method and application thereof.

[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0005] In a first aspect, the present invention provides a composite fabric having the function of blocking and decomposing PAHs smoke, wherein the composite fabric is a double-layer fabric composited with functional particles, wherein the functional particles include a high temperature resistant modified TiO2-CN catalyst and a high temperature resistant modified zirconium hydroxide;

[0006] The preparation method of the high temperature resistant modified TiO2-CN catalyst is:

[0007] TiO2-CN is added to ZrO2 sol and stirred to obtain a first mixed solution, and the particles are dispersed by ultrasonic wave, and the powder after the particles are dried is transferred into a muffle furnace and sintered at 350-650° C. for 1-3 hours to obtain a high temperature resistant modified TiO2-CN catalyst;

[0008] The preparation method of the high temperature resistant modified zirconium hydroxide is:

[0009] Zirconium hydroxide is added to the ZrO2 sol and stirred evenly to obtain a second mixed solution, and then the solution is dispersed by ultrasonic wave and dried. The dried powder is transferred into a muffle furnace and sintered at 350-650° C. for 1-3 hours to obtain high temperature resistant modified zirconium hydroxide.

[0010] The present invention performs high temperature resistant surface modification and finishing on CN-doped TiO2 and zirconium hydroxide so that ZrO2 is attached to their surfaces, with the purpose of protecting the surface structure of the active material, reducing surface defects, and lowering the recombination probability of photogenerated electrons and holes in a high temperature environment, while utilizing metal oxides to enhance catalytic activity.

[0011] The present invention assembles mesoporous TiO2 and CN compounds through polydimethylsiloxane (PDMS), and introduces zirconium hydroxide particles on this basis, in order to synergistically achieve efficient decomposition of PAHs flue gas pollutants.

[0012] Preferably, the mass percentage of TiO2-CN particles in the first mixed solution is 5-20wt%.

[0013] Preferably, the mass percentage of zirconium hydroxide particles in the second mixed solution is 5-20wt%.

[0014] Preferably, the preparation method of the TiO2-CN is: dispersing TiO2 and CN compounds in a polydimethylsiloxane solvent at a mass ratio of 1:1, and then physically assembling them through mechanical stirring and ultrasound to obtain TiO2-CN liquid, and drying the TiO2-CN liquid to obtain TiO2-CN.

[0015] Preferably, the preparation method of TiO2 is: dissolving hexadecylamine in anhydrous ethanol, adding potassium chloride solution, placing it on a magnetic stirring device for stirring, then adding titanium isopropoxide, stirring evenly and placing it at room temperature for 12-24 hours, then repeatedly washing with anhydrous ethanol for 3-5 times, centrifugally drying, and calcining in a muffle furnace at 400-650°C for 1.5-3 hours. After grinding, spherical anatase phase TiO2 can be obtained.

[0016] Preferably, the preparation method of the CN compound is: placing melamine in a crucible, placing the crucible cover in a muffle furnace, calcining at 450-650° C. for 1.5-2.5 h, and grinding after cooling to obtain the CN compound.

[0017] Preferably, the preparation method of the ZrO2 sol is: dissolving zirconium chloride in deionized water, slowly adding ammonia water until the solution becomes a white precipitate, filtering out the precipitate and washing it with deionized water for 3-5 times until the pH of the washing solution is close to neutral, re-dispersing the white precipitate in anhydrous ethanol, and ultrasonically stirring to form a uniform ZrO2 sol.

[0018] Mesoporous TiO2 needs to be exposed to ultraviolet light to generate electron-hole pairs, which in turn stimulate redox reactions to generate highly oxidizing hydroxyl radicals (·OH) and superoxide radicals (·O2 - ), these active species can decompose harmful substances in the flue gas, such as formaldehyde, benzene and other organic matter, nitrogen oxides, sulfur oxides, etc., and reduce them into harmless substances.

[0019] CN compounds are introduced on the basis of mesoporous TiO2 to expand its absorption range of visible light, thereby improving its catalytic activity under visible light. Compared with pure TiO2, TiO2-CN has higher catalytic efficiency under visible light and can more effectively decompose pollutants in flue gas. The enhancement effect of TiO2-CN mainly comes from the reduction of band gap energy after carbon and nitrogen doping, which enables it to generate electron-hole pairs more effectively under visible light. In addition, carbon and nitrogen doping can also increase the active sites on the surface of TiO2, thereby improving its adsorption and reaction ability to pollutants.

[0020] The typical photocatalytic reaction mechanism is similar to that of pure TiO2, but due to the reduction of the band gap, the reaction can occur under visible light. Therefore, this solution can ensure the decomposition effect of PAHs while the fire-fighting suit is in the performance of fire-fighting and rescue tasks. It can achieve efficient decomposition of flue gas PAHs pollutants through visible light catalysis while being worn, avoiding the increase in the difficulty of cleaning due to the long-term attachment of harmful substances on the surface of the clothing and deep penetration.

[0021] Preferably, the double-layer fabric includes a surface yarn and an inner yarn, the surface yarn includes aramid 1313, aramid 1414, conductive fiber, and nylon, wherein the mass fraction of aramid 1313 is 50-70 parts, the mass fraction of aramid 1414 is 5-15 parts, the mass fraction of conductive fiber is 1-3 parts, and the mass fraction of nylon is 10-15 parts; the inner yarn includes aramid 1313, flame retardant viscose, and lyocell fiber, wherein the mass fraction of aramid 1313 is 20-40 parts, the mass fraction of flame retardant viscose is 35-45 parts, and the mass fraction of lyocell fiber is 15-25 parts.

[0022] Preferably, the surface yarn is made by mixing aramid 1313, aramid 1414 and conductive fiber evenly, and then core-wrapped with nylon filament 40D, and the yarn count is 40s / 2-45s / 2; the inner yarn is made by mixing aramid 1313, flame-retardant viscose and Lyocell fiber, and the single yarn twist coefficient of the yarn is set to 280, the ply twist coefficient is set to 390, and the yarn count is 45s / 2-60s / 2.

[0023] Furthermore, the double-layer fabric has a mass per unit area of ​​200-280 gsm.

[0024] Furthermore, the surface yarn in the double-layer fabric adopts 2 / 1 variable twill checkered cloth, and the inner yarn adopts plain weave.

[0025] Furthermore, the warp yarn density of the surface yarn and the inner yarn is configured as (2.2-2.5):1, and the weft density is configured as (1.8-2.2):1; wherein the surface warp yarn and the inner warp yarn are arranged at 1.7-2.1, and the surface weft yarn and the inner weft yarn are arranged at 1.7-2.1; when threading the reed, the surface yarn and the inner yarn are cycled every 1.2 cm, and the surface yarn and the inner yarn are arranged between 0.7-1 cm and 3 are inserted, and the remaining reed tooth width is pressed into 1 reed tooth by 2 surface yarns and 3 inner yarns.

[0026] Furthermore, the surface yarn and the inner yarn are connected in the warp and weft directions with additional binding yarns. The binding yarn structure adopts 1 / 2 and 1 / 3, and the binding yarn adopts the surface yarn to avoid the inner yarn being exposed on the surface. The size of the gap between the surface and the inner layer formed by the binding yarn is (0.8cm-1.2cm)×(0.8cm-1.2cm).

[0027] Furthermore, the double-layer fabric is woven using a double-weaving-shaft loom, the upper shaft is the inner yarn, the lower shaft is the surface yarn, and the tension of the surface yarn and the inner yarn is controlled to be 1.5:1.

[0028] Furthermore, the double-layer fabric is subjected to post-finishing and tentering after the woven grey cloth is dried at a high temperature of 175° C.-185° C. for 80-100 seconds and then pre-shrunk to form a finished product.

[0029] In a second aspect, the present invention provides a method for preparing the above-mentioned composite fabric, comprising the following steps:

[0030] Dissolve polydimethylsiloxane (PDMS) and curing agent in n-heptane, stir to fully mix and dissolve, add high temperature resistant modified TiO2 / CN catalyst and high temperature resistant modified zirconium hydroxide respectively, ultrasonically disperse for 5-15 minutes, stir for 0.5-2 hours to obtain an impregnation solution, immerse the double-layer fabric in the impregnation solution to obtain a coated fabric, and then put it in a 60-80°C oven to dry for 3-6 hours to obtain a composite fabric.

[0031] Preferably, the mass ratio of the PDMS, curing agent, high temperature resistant modified TiO2 / CN catalyst and high temperature resistant modified zirconium hydroxide is (1-15): (0.1-1.5): (1-10): (1-4), wherein the amount of n-heptane is 10-50 mL of n-heptane per 1-15 g of PDMS dissolved.

[0032] In a third aspect, the present invention provides another method for preparing the above-mentioned composite fabric, comprising the following steps:

[0033] Add PDMS and curing agent to n-heptane, stir to mix and dissolve them thoroughly, then spray the double-layer fabric with a spray gun pressure of 0.3-0.5 bar and a distance of 10-20 cm from the fabric, then put it in a 60-80°C oven and pre-bake for 20-60 minutes. Disperse the mixture of high-temperature resistant modified TiO2 / CN and high-temperature resistant modified zirconium hydroxide particles in ethanol and ultrasonicate for 5-15 minutes, then spray it onto the double-layer fabric. After spraying, put the double-layer fabric in an 80-100°C oven and dry it for 5-30 minutes to obtain a composite fabric.

[0034] Preferably, the amount of the high temperature resistant modified TiO2 / CN catalyst is 1-5wt%, and the amount of the high temperature resistant modified zirconium hydroxide is 1-2wt%.

[0035] In a fourth aspect, the present invention also provides a use of the above-mentioned composite fabric in preparing outer fabrics of protective clothing.

[0036] The present invention is to compound the TiO2-CN catalyst and zirconium hydroxide modified by the high temperature resistant coating into the coating material, and then immerse / spray it into the mixed fabric with special structure to achieve the effect of 1+1>2, and prepare the multifunctional fabric with PAHs blocking, decomposition and easy cleaning in high temperature environment, which is the innovation point of the present invention as an overall solution. Specifically:

[0037] (1) Barrier: Physical barrier of flue gas pollutants is achieved through the design and preparation of multi-layer structural fabrics, and efficient barrier of chemical toxic substances is achieved through coating / spraying finishing.

[0038] (2) Catalytic decomposition in high temperature environment: CN doped TiO2 can enhance visible light catalysis, and zirconium hydroxide can synergistically catalyze the decomposition of PAHs, achieving efficient decomposition of flue gas PAHs pollutants. CN doped TiO2 and zirconium hydroxide modified with high temperature resistant coating can protect photocatalytic functional materials from high temperature phase change, prevent surface chemical reactions, and maintain the catalytic activity of materials. Through the above treatment, harmful substances can be prevented from adhering to the surface of clothing for a long time.

[0039] (3) Easy to clean: a. Due to the low surface energy of PDMS and the rough microscopic surface constructed by functional particles, smoke pollution is easier to clean; b. The fabric coating exists on the surface of the yarn, which can prevent particles / PAHs from penetrating and migrating into the pores and interior of the yarn, thereby allowing these pollutants to remain on the fiber surface more and reduce the difficulty of cleaning; c. During the process of PAHs penetrating into the fabric, the functional coating decomposes them, which reduces the concentration of PAHs remaining in the fabric and reduces the cleaning cost.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] The present invention can firstly reduce the migration ability of PAHs in the multi-layer structure of protective clothing, so that the toxic pollution is blocked on the outer surface of the protective clothing; secondly, the decomposition level of PAHs is improved, so that the fabric has the ability to detoxify toxic substances; finally, by improving the surface properties of the protective clothing, the clothing is easier to clean and the toxic substances are easier to be stripped from the fabric matrix. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 is a cross-sectional view of a double-layer fabric of the present invention;

[0043] Figure 2 is a cross-sectional view of a double-layer fabric of the present invention. DETAILED DESCRIPTION

[0044] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0045] The present invention will be described in detail below with reference to the embodiments.

[0046] Example 1

[0047] 1. Preparation of double-layer fabric

[0048] The double-layer fabric consists of a surface yarn 1 and an inner yarn 2, such as Figure 1 and Figure 2 As shown, the surface yarn includes aramid 1313, aramid 1414, conductive fiber, and nylon, wherein the mass fraction of aramid 1313 is 60 parts, the mass fraction of aramid 1414 is 12 parts, the mass fraction of conductive fiber is 2 parts, and the mass fraction of nylon is 12 parts; the inner layer yarn includes aramid 1313, flame retardant viscose, and lyocell fiber, wherein the mass fraction of aramid 1313 is 30 parts, the mass fraction of flame retardant viscose is 40 parts, and the mass fraction of lyocell fiber is 20 parts.

[0049] In the surface yarn, aramid 1313, aramid 1414 and conductive fiber are evenly mixed and then core-wrapped with nylon filament 40D, and the yarn count is 42s / 2; the inner yarn is mixed with aramid 1313, flame-retardant viscose and Lyocell fiber, and the single yarn twist coefficient of the yarn is set to 280, the ply twist coefficient is 390, and the yarn count is 48s / 2. The warp yarn density of the surface yarn and the inner yarn is configured as 2.3:1, and the weft density is configured as 2:1; the surface warp yarn 11 and the inner warp yarn 21 are arranged at 1.9:1, and the surface weft yarn 12 and the inner weft yarn 22 are arranged at 1.9:1; when reeding, the surface yarn and the inner yarn are cycled every 1.2 cm, and the surface yarn and the inner yarn are arranged with 3 insertions between 0.8 cm, and the remaining reed tooth width is pressed into 1 reed tooth with 2 surface yarns and 3 inner yarns; the surface yarn and the inner yarn are connected in the warp and weft directions with an additional binding yarn 3, and the binding yarn 3 structure is 1 / 2 and 1 / 3, and the binding yarn 3 uses the surface yarn to avoid the inner yarn being exposed from the surface layer, and the size of the surface and inner layer gap formed by the binding yarn 3 is 1 cm×1 cm.

[0050] A double-beam loom is used to weave double-layer fabrics, with the upper shaft being the inner yarn and the lower shaft being the surface yarn, and the tension of the inner and outer layers being controlled at 1.5:1; the surface yarn in the double-layer fabric is 2 / 1 variable twill plaid cloth, and the inner yarn is plain weave.

[0051] The double-layer fabric is finished by finishing and tentering the grey cloth after weaving, and then pre-shrunk after high-temperature baking at 180℃ for 90s to form a finished product.

[0052] The double-layer fabric prepared in this embodiment has a mass per unit area of ​​240 gsm.

[0053] 2. Preparation of functional particles

[0054] (a) Dissolve 12g of hexadecylamine in 500ml of anhydrous ethanol, add 0.1mol of potassium chloride solution, and stir on a magnetic stirring device for 15min. Add 10.8ml of titanium isopropoxide to the mixed solution, stir for 60min, and place at room temperature for 24h. Then wash repeatedly with anhydrous ethanol for 3 to 5 times, centrifugally dry, and calcine in a muffle furnace at 650℃ for 2h. After grinding, spherical anatase phase TiO2 can be obtained.

[0055] (b) Melamine is placed in a crucible, and the crucible cover is placed in a muffle furnace at 650°C for 2 hours. After cooling, the crucible is ground to obtain pale yellow powdered graphite carbon nitride (CN compound).

[0056] The separately synthesized TiO2 and CN compounds are dispersed in a polydimethylsiloxane solvent at a mass ratio of 1:1, and then physically assembled by mechanical stirring and ultrasound to obtain TiO2-CN liquid, and the TiO2-CN liquid is dried to obtain TiO2-CN.

[0057] (c) Dissolve 5 g of zirconium chloride in 100 mL of deionized water, and slowly add ammonia water until the solution turns into a white precipitate. Filter the precipitate and wash it three times with deionized water until the pH of the washing solution is close to neutral. Re-disperse the white precipitate in anhydrous ethanol and stir it ultrasonically to form a uniform ZrO2 sol.

[0058] TiO2-CN was added to the ZrO2 sol and stirred for 30 minutes to ensure uniform attachment to obtain a first mixed solution. Ultrasonic waves were used to further disperse the particles. The mass percentage of TiO2-CN particles in the first mixed solution was 5wt%. The coated mixture was placed in a vacuum oven and dried at 80°C for 12 hours. The dried powder was moved into a muffle furnace and sintered at 400°C for 3 hours to ensure the formation of a high temperature resistant protective layer of ZrO2, thereby obtaining a high temperature resistant modified TiO2-CN catalyst.

[0059] Zirconium hydroxide was added to the ZrO2 sol and stirred for 30 minutes to ensure uniform attachment to obtain a second mixed solution. Ultrasonic waves were used to further disperse the particles. The mass percentage of zirconium hydroxide particles in the second mixed solution was 5wt%. The coated mixture was placed in a vacuum oven and dried at 80°C for 12 hours. The dried powder was moved into a muffle furnace and sintered at 400°C for 3 hours to ensure the formation of a high temperature resistant protective layer of ZrO2, thereby obtaining a high temperature resistant modified zirconium hydroxide.

[0060] 3. Preparation of composite fabrics

[0061] Dissolve 15g PDMS and 1.5g curing agent in 50mL n-heptane and stir for 2h to fully mix and dissolve. Take 10g high temperature resistant modified TiO2 / CN catalyst and 4g high temperature resistant modified zirconium hydroxide particles and add them to the mixed solution, ultrasonically disperse for 15min, stir for 2h to obtain the impregnation solution. Put the double-layer fabric into the impregnation solution, use a horizontal rolling mill, dip and roll three times to obtain the coated fabric. Then, put it in an 80℃ oven and dry it for 6h to obtain the composite fabric.

[0062] Example 2

[0063] The preparation method of the composite fabric of this embodiment is basically the same as that of embodiment 1, except that:

[0064] 3. Preparation of composite fabrics

[0065] Add 10g PDMS and 1g curing agent to 100ml n-heptane, stir for 1h, then spray the fabric with a spray gun pressure of 0.5bar and a distance of 20cm from the fabric. Then put it in an 80℃ oven and pre-bake for 20min. Disperse the mixture of high temperature resistant modified TiO2 / CN catalyst and high temperature resistant modified zirconium hydroxide particles in 100ml ethanol, ultrasonicate for 15min, then spray it on the fabric. After coating, put the fabric in a 100℃ oven and dry it for 30min. The amount of TiO2 / CN is 5wt%, and the amount of high temperature resistant modified zirconium hydroxide is 2wt%.

[0066] Example 3

[0067] The preparation method of the composite fabric of this embodiment is basically the same as that of Embodiment 1, except that the mass percentage of TiO2-CN particles in the first mixed solution is 20wt%.

[0068] Example 4

[0069] The preparation method of the composite fabric of this embodiment is basically the same as that of Embodiment 1, except that the mass percentage of the zirconium hydroxide particles in the second mixed solution is 20 wt %.

[0070] Example 5

[0071] The preparation method of the composite fabric of this embodiment is basically the same as that of Embodiment 1, except that the mass percentage of TiO2-CN particles in the first mixed solution is 10 wt%.

[0072] Example 6

[0073] The preparation method of the composite fabric of this embodiment is basically the same as that of Embodiment 1, except that the mass percentage of the zirconium hydroxide particles in the second mixed solution is 15 wt %.

[0074] Comparative Example 1

[0075] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that a single-layer fabric is used. The preparation method of the single-layer fabric is as follows:

[0076] Aramid 1313, aramid 1414 and conductive fiber are preferably used as the base material of the fabric, and a single-layer fabric structure is adopted in the structural design, and the organization structure is a plain woven structure, wherein aramid 1313 accounts for 93%, aramid 1414 accounts for 5%, and conductive fiber accounts for 2%, 2 / 2 square, 750 twist / m, and yarn weaving is 38s / 2.

[0077] The single-layer fabric is finished by finishing and tentering the finished grey cloth, and then pre-shrunk after being baked at 180°C for 90s to form a finished product.

[0078] Comparative Example 2

[0079] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that: no high temperature modified zirconium hydroxide is added to the impregnation solution.

[0080] Comparative Example 3

[0081] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that zirconium hydroxide is used in the impregnation liquid to replace the high-temperature modified zirconium hydroxide.

[0082] Comparative Example 4

[0083] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that: no high temperature modified TiO2-CN catalyst is added to the impregnation liquid.

[0084] Comparative Example 5

[0085] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that: the high temperature modified TiO2-CN catalyst is replaced by TiO2-CN catalyst in the impregnation liquid.

[0086] Comparative Example 6

[0087] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that the mass percentage of TiO2-CN particles in the first mixed solution is 4wt%.

[0088] Comparative Example 7

[0089] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that the mass percentage of TiO2-CN particles in the first mixed solution is 21wt%.

[0090] Comparative Example 8

[0091] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that the mass percentage of the zirconium hydroxide particles in the second mixed solution is 4 wt %.

[0092] Comparative Example 9

[0093] The preparation method of the composite fabric of this comparative example is basically the same as that of Example 1, except that the mass percentage of the zirconium hydroxide particles in the second mixed solution is 21 wt %.

[0094] Test Case

[0095] Fabric air permeability test: Tested in accordance with GB / T5453 "Determination of air permeability of textile fabrics" standard;

[0096] Fabric surface water level test: Test according to GB / T 4745 "Test method for surface moisture resistance of textile fabrics - Water test method";

[0097] Fabric filtration efficiency test: According to GB2626-2019 "Respiratory Protection Self-priming Filter-type Anti-particulate Respirator" standard, the flow rate is 15L / min and the test is carried out under saline medium conditions;

[0098] PAH interception rate test: First, place the multi-layer fabric sample of the fire-fighting protective clothing in a smoke environment for pollution. According to GB / T 28189-2011 "Determination of Polycyclic Aromatic Hydrocarbons in Textiles", the PAHs content of each layer in the multi-layer composite structure of the fire-fighting protective clothing is tested, and then the interception rate is calculated according to the following formula:

[0099] PAHs interception rate of outer fabric = [(M0+I0)-(M X +I X )] / (M0+I0);

[0100] M: PAH content in the middle layer fabric, M X represents the developed sample, and M0 represents the control sample;

[0101] I: PAH content in the inner layer fabric, I X represents the developed sample, and I0 represents the control sample;

[0102] The PAHs decomposition rate test of the outer fabric is carried out 2 hours after the sample is contaminated. The specific calculation method is as follows:

[0103] PAHs decomposition rate of outer fabric = (O0-O X ) / O0;

[0104] O: PAH content in outer fabric, O X represents the developed sample, and O0 represents the control sample;

[0105] Table 1 Test results

[0106]

[0107]

[0108] It can be seen from the above table that the composite fabric prepared by the present invention achieves the barrier and efficient decomposition of PAHs smoke in a high temperature environment, and is suitable for the protection of workers in a toxic environment with PAHs smoke. The protective clothing has the barrier and decomposition capabilities, and at the same time solves the cleaning needs of rapid decontamination.

[0109] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite fabric having the function of blocking and decomposing PAHs smoke, characterized in that: The composite fabric is a double-layer fabric composited with functional particles, wherein the functional particles include a high temperature resistant modified TiO2-CN catalyst and a high temperature resistant modified zirconium hydroxide; The preparation method of the high temperature resistant modified TiO2-CN catalyst is: TiO2-CN is added to ZrO2 sol and stirred to obtain a first mixed solution, and the particles are dispersed by ultrasonic wave, and the powder after the particles are dried is transferred into a muffle furnace and sintered at 350-650° C. for 1-3 hours to obtain a high temperature resistant modified TiO2-CN catalyst; The preparation method of the high temperature resistant modified zirconium hydroxide is: Zirconium hydroxide is added to the ZrO2 sol and stirred evenly to obtain a second mixed solution, and then the solution is dispersed by ultrasonic wave and dried. The dried powder is transferred into a muffle furnace and sintered at 350-650° C. for 1-3 hours to obtain high temperature resistant modified zirconium hydroxide.

2. The composite fabric according to claim 1, characterized in that: The mass percentage of TiO2-CN particles in the first mixed solution is 5-20wt%; preferably, the mass percentage of zirconium hydroxide particles in the second mixed solution is 5-20wt%.

3. The composite fabric according to claim 1, characterized in that: The preparation method of TiO2-CN is as follows: TiO2 and CN compounds are dispersed in a polydimethylsiloxane solvent at a mass ratio of 1:1, and then physically assembled by mechanical stirring and ultrasound to obtain TiO2-CN liquid, and the TiO2-CN liquid is dried to obtain TiO2-CN; Preferably, the preparation method of TiO2 is: dissolving hexadecylamine in anhydrous ethanol, adding potassium chloride solution, adding titanium isopropoxide under stirring, stirring evenly and placing at room temperature for 12-24 hours, then repeatedly washing with anhydrous ethanol for 3-5 times, centrifugally drying, calcining in a muffle furnace at 400-650°C for 1.5-3 hours, and grinding to obtain spherical anatase phase TiO2; Preferably, the preparation method of the CN compound is: placing melamine in a crucible, placing the crucible in a muffle furnace, calcining at 450-650° C. for 1.5-2.5 h, and grinding after cooling to obtain the CN compound; Preferably, the preparation method of the ZrO2 sol is: dissolving zirconium chloride in deionized water, adding ammonia water until the solution becomes a white precipitate, filtering out the precipitate and washing it with deionized water for 3-5 times until the pH of the washing solution is close to neutral, re-dispersing the white precipitate in anhydrous ethanol, and ultrasonically stirring to form a uniform ZrO2 sol.

4. The composite fabric according to claim 1, characterized in that: The double-layer fabric includes a surface yarn and an inner yarn, wherein the surface yarn includes aramid 1313, aramid 1414, conductive fiber, and nylon, wherein the mass fraction of aramid 1313 is 50-70 parts, the mass fraction of aramid 1414 is 5-15 parts, the mass fraction of conductive fiber is 1-3 parts, and the mass fraction of nylon is 10-15 parts; the inner yarn includes aramid 1313, flame-retardant viscose, and lyocell fiber, wherein the mass fraction of aramid 1313 is 20-40 parts, the mass fraction of flame-retardant viscose is 35-45 parts, and the mass fraction of lyocell fiber is 15-25 parts.

5. The composite fabric according to claim 1, characterized in that: The surface yarn is made by mixing aramid 1313, aramid 1414 and conductive fiber evenly, and then core-wrapping with nylon filament 40D, with a yarn count of 40s / 2-45s / 2; the inner yarn is made by mixing aramid 1313, flame-retardant viscose and lyocell fiber, setting the single yarn twist coefficient of the yarn to 280, the ply twist coefficient to 390, and the yarn count to 45s / 2-60s / 2; Preferably, the double-layer fabric has a mass per unit area of ​​200-280 gsm; Preferably, the surface yarn of the double-layer fabric adopts 2 / 1 variable twill checkered cloth, and the inner yarn adopts plain weave; Preferably, the warp yarn density of the surface yarn and the inner yarn is configured as (2.2-2.5):1, and the weft density is configured as (1.8-2.2):1; wherein the surface warp yarn and the inner warp yarn are arranged at 1.7-2.1, and the surface weft yarn and the inner weft yarn are arranged at 1.7-2.1; when reeding, the surface yarn and the inner yarn are cycled every 1.2 cm, and the surface yarn and the inner yarn are arranged at 0.7-1 cm and 3 are inserted, and the remaining reed tooth width is pressed into 1 reed tooth by 2 surface yarns and 3 inner yarns; Preferably, the surface yarn and the inner yarn are connected in the warp and weft directions by using additional binding yarns, the binding yarn structure is 1 / 2, 1 / 3, the binding yarn is the surface yarn, and the size of the gap between the surface and the inner layer formed by the binding yarn is (0.8cm-1.2cm)×(0.8cm-1.2cm); Preferably, the double-layer fabric is woven using a double-weaving-shaft loom, the upper shaft is the inner yarn, the lower shaft is the surface yarn, and the tension of the surface yarn and the inner yarn is controlled to be 1.5:1; Preferably, the double-layer fabric is post-finished and tentered after the woven grey cloth is baked at 175° C.-185° C. for 80-100 seconds and then pre-shrunk to form a finished product.

6. A method for preparing the composite fabric according to any one of claims 1 to 5, characterized in that: The steps include: Dissolve polydimethylsiloxane and curing agent in n-heptane, stir to fully mix and dissolve, add high temperature resistant modified TiO2 / CN catalyst and high temperature resistant modified zirconium hydroxide respectively, ultrasonically disperse for 5-15 minutes, stir for 0.5-2 hours to obtain an impregnation solution, immerse the double-layer fabric in the impregnation solution to obtain a coated fabric, and then put it in a 60-80°C oven to dry for 3-6 hours to obtain a composite fabric.

7. The method for preparing a composite fabric according to claim 6, characterized in that: The mass ratio of the PDMS, curing agent, high temperature resistant modified TiO2 / CN catalyst and high temperature resistant modified zirconium hydroxide is (1-15): (0.1-1.5): (1-10): (1-4), wherein the amount of n-heptane is 10-50 mL of n-heptane per 1-15 g of PDMS dissolved.

8. A method for preparing the composite fabric according to any one of claims 1 to 5, characterized in that: The steps include: Add PDMS and curing agent to n-heptane, stir to mix and dissolve them thoroughly, then spray the double-layer fabric with a spray gun pressure of 0.3-0.5 bar and a distance of 10-20 cm from the fabric, then put it in a 60-80°C oven and pre-bake for 20-60 minutes. Disperse the mixture of high-temperature resistant modified TiO2 / CN and high-temperature resistant modified zirconium hydroxide particles in ethanol and ultrasonicate for 5-15 minutes, then spray it onto the double-layer fabric. After spraying, put the double-layer fabric in an 80-100°C oven and dry it for 5-30 minutes to obtain a composite fabric.

9. The method for preparing the composite fabric according to claim 8, characterized in that: The dosage of the high temperature resistant modified TiO2 / CN catalyst is 1-5wt%, and the dosage of the high temperature resistant modified zirconium hydroxide is 1-2wt%.

10. Use of the composite fabric according to any one of claims 1 to 5 in preparing outer fabrics of protective clothing.