Micro-swelling graft modified self-lubricating fabric liner as well as preparation method and application thereof

By performing microswelling graft modification in the self-lubricating fabric liner, combining graphene oxide or carboxylated carbon nanotubes with impregnated resin, the large overflow loss of lubricating filler and insufficient adhesion of aramid fiber to resin in the prior art is solved. The problem of improving the lubrication efficiency and friction performance of the pad.

CN119083159APending Publication Date: 2024-12-06NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411435060.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing self-lubricating fabric liners have large overflow loss during the friction process, and the adhesion between aramid fiber and resin is insufficient, which limits the tribological properties and adhesion of the liners.

Method used

Using the microswelling graft modification technology, the fibers are reinforced by grafting graphene oxide or carboxylated carbon nanotubes in the woven fabric of aramid fiber and PTFE fiber, and impregnating resins with phenolic resins, modified epoxy resins and other impregnation resins. The bonding strength and adhesion of the resin.

Benefits of technology

It significantly reduces the loss of lubricating filler during friction, improves the lubrication efficiency and friction wear performance of the liner, enhances the adhesion to the steel substrate, and improves the load-bearing capacity under high shear stress friction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083159A_ABST
    Figure CN119083159A_ABST
Patent Text Reader

Abstract

The invention discloses a micro-swelling graft modified self-lubricating fabric liner as well as a preparation method and application thereof, and relates to the technical field of self-lubricating composite materials. The micro-swelling graft modified self-lubricating fabric liner comprises a modified hybrid fiber fabric and impregnating resin loaded on the modified hybrid fiber fabric, the modified hybrid fiber fabric is a micro-swelling hybrid fiber fabric grafted with a micro-nano filler, and the micro-nano filler comprises graphene oxide or carboxylated carbon nanotubes. According to the micro-swelling grafting modified self-lubricating fabric liner disclosed by the invention, the micro-nano filler is grafted on the hybrid fiber fabric, so that the lubricating efficiency of the micro-nano filler is improved, and the frictional wear performance of the self-lubricating fabric liner is improved. The roughness of the surface skin layer of the aramid fiber in the micro-swelled hybrid fiber fabric is increased, the bonding strength between the hybrid fiber fabric and the impregnated resin is improved, and meanwhile, the adhesion of the self-lubricating fabric liner and a steel substrate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of self-lubricating composite materials, and in particular relates to a slightly swellable graft-modified self-lubricating fabric liner and a preparation method and application thereof. Background Art

[0002] The spherical plain bearing structure includes an outer ring with an inner spherical surface and an inner ring with an outer spherical surface. It can bear radial load, axial load or combined radial and axial load. The lubrication between the inner and outer rings during the load-bearing process is mainly guaranteed by the lubricating oil filled between the two. Self-lubricating spherical plain bearings refer to the use of certain solid self-lubricating materials inlaid or bonded between the inner and outer rings, so that no additional lubricating materials are required during the use of the bearings, which reduces maintenance costs and meets the use requirements of special operation scenarios such as vacuum and seawater. Among them, the self-lubricating spherical plain bearings with self-lubricating fabric pads bonded between the inner and outer rings are a type of self-lubricating bearings that are currently widely used in deep space exploration, space flight, and deep-sea shipping.

[0003] Self-lubricating fabric pads are usually made of high-performance fibers and polytetrafluoroethylene fibers, which are woven into a mixed fiber fabric with warp and weft threads, and then impregnated with a specific resin and hot-pressed to shape. Among them, polytetrafluoroethylene fiber, as a lubricating phase, forms a transfer film during the friction process to reduce wear. However, due to the low strength and extremely strong inertness of polytetrafluoroethylene fibers, it cannot independently bear the wear-reducing and anti-wear effects of the pad. High-performance fibers make up for this shortcoming on the other hand, and improve the mechanical properties of the pad through their own high strength and high modulus characteristics, and improve the anti-wear performance of the pad. Aramid fiber is a choice among high-performance fibers in the composition of fabric pads. Its smooth surface has a strong inertness and cannot form a strong adhesion with the resin, which limits its development as a reinforcing phase in fabric pads. Summary of the invention

[0004] In order to solve the above problems existing in the prior art, the present invention provides a micro-swelling grafted modified self-lubricating fabric liner and its preparation method and application. The technical problem to be solved by the present invention is achieved by the following technical solutions:

[0005] The invention provides a slightly swollen grafted modified self-lubricating fabric liner, comprising: a modified mixed fiber fabric and an impregnated resin loaded on the modified mixed fiber fabric; the modified mixed fiber fabric is a slightly swollen mixed fiber fabric grafted with a micro-nano filler, and the micro-nano filler comprises graphene oxide or carboxylated carbon nanotubes.

[0006] In one embodiment of the present invention, the mixed fiber fabric is a woven fabric of aramid fiber and PTFE fiber, and the woven fabric is a plain fabric, a twill fabric or a satin fabric;

[0007] The surface density of the mixed fiber fabric is 180-360g / m 2 The diameter of the aramid fiber is 200D-1000D, and the diameter of the PTFE fiber is 200D-1000D.

[0008] In one embodiment of the present invention, 3-amino-1,2,4-triazole is used as an interface hydrogen bond structure grafting bridge to connect the micro-nano filler and the slightly swollen aramid fiber.

[0009] In one embodiment of the present invention, the impregnating resin includes at least one of phenolic resin, modified epoxy resin, bismaleimide resin and modified cyanate resin.

[0010] In one embodiment of the present invention, the mass fraction of the impregnating resin in the slightly swellable graft-modified self-lubricating fabric liner is 25%-35%.

[0011] The present invention provides a method for preparing a slightly swellable graft modified self-lubricating fabric liner, which is applicable to the slightly swellable graft modified self-lubricating fabric liner described in any one of the above embodiments. The preparation method comprises:

[0012] Cleaning of mixed fiber fabrics;

[0013] Adding micro-nano fillers, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 3-amino-1,2,4-triazole into pure water for modification reaction to obtain a modified solution, and sequentially washing the modified solution with alcohol, centrifuging and drying to obtain a modified micro-nano filler;

[0014] Adding N,N-dimethylacetamide and the modified micro-nano filler into pure water and mixing them to obtain a slightly swollen grafting solution;

[0015] The mixed fiber fabric after cleaning is immersed in the slightly swellable grafting solution, and a grafting reaction is performed by infrared heating, and the mixed fiber fabric after the slightly swellable grafting is subjected to ultrasonic cleaning and drying in sequence to obtain a modified mixed fiber fabric;

[0016] placing the modified mixed fiber fabric in an impregnation solution containing an impregnation resin, and subjecting the impregnation solution to multiple ultrasonic, rolling and drying cycles to obtain a composite modified mixed fiber fabric;

[0017] The composite modified mixed fiber fabric is solidified and formed to obtain a slightly swellable grafted modified self-lubricating fabric liner.

[0018] In one embodiment of the present invention, the mass ratio of the micro-nano filler, the 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and the 3-amino-1,2,4-triazole is (1-3):(10-15):(3-5);

[0019] The reaction temperature of the modification reaction is 60-80° C., and the reaction time is 1-3 h.

[0020] In one embodiment of the present invention, the mass fraction of N,N-dimethylacetamide in the slightly swelling grafting solution is 10%-20%, and the mass fraction of the modified micro-nano filler in the slightly swelling grafting solution is 0.1%-0.5%.

[0021] In one embodiment of the present invention, the volume ratio of the washed mixed fiber fabric to the slightly swellable grafting solution is 1:(20-25); the reaction temperature of the grafting reaction is 80-100° C., and the reaction time is 1-3 hours.

[0022] The present invention provides an application of the slightly swellable grafted modified self-lubricating fabric liner as described in any one of the above embodiments in a self-lubricating spherical bearing.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The micro-swelling grafted modified self-lubricating fabric liner of the present invention comprises a modified mixed fiber fabric and an impregnating resin loaded on the modified mixed fiber fabric, wherein the modified mixed fiber fabric is a mixed fiber fabric grafted with micro-nano fillers, and the micro-nano fillers include graphene oxide or carboxylated carbon nanotubes. The present invention minimizes the overflow loss of the lubricating filler due to the high-speed movement of the friction pair during the friction process of the micro-swelling grafted modified self-lubricating fabric liner, thereby improving the lubrication efficiency of the micro-nano filler and improving the tribological performance of the self-lubricating fabric liner.

[0025] 2. The slightly swellable grafted modified self-lubricating fabric liner of the present invention has partially broken hydrogen bonds in the surface cortex of the aramid fibers in the mixed fiber fabric after slight swelling, which increases the roughness and specific surface area, thereby increasing the actual contact area between the impregnated resin and the mixed fiber fabric, enhancing the mechanical locking effect between the impregnated resin and the aramid fibers in the mixed fiber fabric, improving the bonding strength between the mixed fiber fabric and the impregnated resin, and improving the adhesion between the self-lubricating fabric liner and the steel substrate, so that the slightly swellable grafted modified self-lubricating fabric liner exhibits better load-bearing capacity in high shear stress friction conditions.

[0026] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the following specifically cites a preferred embodiment and describes it in detail with the accompanying drawings as follows. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a SEM (scanning electron microscope) image of aramid fiber in a modified mixed fiber fabric provided by an embodiment of the present invention;

[0028] Figure 2 is a SEM image of aramid fiber in an unmodified mixed fiber fabric provided in an embodiment of the present invention;

[0029] Figure 3 Schematic diagram of a method for preparing a slightly swellable graft-modified self-lubricating fabric liner provided by an embodiment of the present invention;

[0030] Figure 4 This is a SEM image of the wear scar of the slightly swellable grafted modified self-lubricating fabric liner prepared in Example 1 after the friction test;

[0031] Figure 5 This is a SEM image of the wear scar of the self-lubricating fabric pad prepared in Example 1 after the friction test. DETAILED DESCRIPTION

[0032] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the following is a detailed description of a slightly swelling grafted modified self-lubricating fabric liner and its preparation method and application proposed in accordance with the present invention in combination with the accompanying drawings and specific implementation methods.

[0033] The above and other technical contents, features and effects of the present invention are clearly presented in the following detailed description of the specific implementation modes in conjunction with the accompanying drawings. Through the description of the specific implementation modes, the technical means and effects adopted by the present invention to achieve the predetermined purpose can be more deeply and specifically understood. However, the attached drawings are only for reference and explanation purposes and are not used to limit the technical solutions of the present invention.

[0034] In a first aspect, an embodiment of the present invention provides a slightly swollen grafted modified self-lubricating fabric liner comprising: a modified mixed fiber fabric and an impregnated resin loaded on the modified mixed fiber fabric. The modified mixed fiber fabric is a slightly swollen mixed fiber fabric grafted with micro-nano fillers, and the micro-nano fillers include graphene oxide or carboxylated carbon nanotubes.

[0035] In an optional embodiment, the mixed fiber fabric is a woven fabric of aramid fiber and PTFE (polytetrafluoroethylene) fiber. Wherein, the woven fabric can be a plain fabric, a twill fabric or a satin fabric.

[0036] Optionally, the surface density of the mixed fiber fabric is 180-360g / m 2 , wherein the diameter of the aramid fiber can be 200D-1000D, and the diameter of the PTFE fiber can be 200D-1000D.

[0037] Optionally, the mixed fiber fabric has a thickness of 0.25-0.35 mm.

[0038] In an optional embodiment, 3-amino-1,2,4-triazole can be used as an interface hydrogen bond structure grafting bridge to connect the micro-nano filler and the slightly swollen aramid fiber.

[0039] In an optional embodiment, N,N-dimethylacetamide can be used as a hydrogen bond regulator between aramid fiber macromolecules in mixed fiber fabrics. Under infrared irradiation conditions, the hydrogen bonds between the cortical layers of the aramid fibers are broken, and the surface is slightly swollen. Aramid belongs to aromatic polyamides, and its macromolecules are orderly bonded by dense hydrogen bonds. DMAc (N,N-dimethylacetamide) is a strong polar solvent that can destroy the hydrogen bond forces between the macromolecular chains of aramid fibers, partially break to achieve microswelling, increase porosity, and make the original hydrogen bond structural units vacant, providing connection points for subsequent grafting of micro-nano fillers. The epoxy and carboxyl groups on the surface of graphene oxide can undergo nucleophilic substitution and amidation reactions with the amino groups of 3-amino-1,2,4-triazole, respectively, so that 3-amino-1,2,4-triazole is grafted on the surface of graphene oxide and hydrogen bond structural units (amide and triazole groups, the number of hydrogen bond donors is 2, and the number of hydrogen bond acceptors is 3) are introduced. Since both the modified graphene oxide and the slightly swollen aramid contain N and O atoms that can act as hydrogen bond receptors to interact with adjacent H atoms, multiple hydrogen bond structures are formed between the modified graphene oxide and the surface of the aramid fiber under infrared heating conditions. In the subsequent washing and drying process, the aramid macromolecules absorb energy, release the free water in the fiber, reduce the gaps between the macromolecules, and restore the regular arrangement. The larger m-GO nanosheets with hydrogen bond structural units are combined with the axial arrangement of the fiber macromolecules, thereby being fixed between the fiber macromolecules, and the smaller DMAc molecules escape due to heat.

[0040] In this embodiment, since the micro-nano filler is grafted onto the aramid fiber through the interfacial hydrogen bond structure, during the friction process of the micro-swelling grafted modified self-lubricating fabric liner, the micro-nano filler is not easy to overflow the friction area with the movement of the friction pair due to the presence of a large number of hydrogen bonds, thereby improving the lubrication efficiency of the micro-nano filler, thereby forming a more stable and dense lubrication transfer film, and effectively improving the friction and wear performance of the self-lubricating fabric liner.

[0041] In an optional embodiment, the impregnating resin includes at least one of phenolic resin, modified epoxy resin, bismaleimide resin and modified cyanate resin.

[0042] Optionally, the mass fraction of the impregnated resin in the slightly swellable graft modified self-lubricating fabric liner is 25%-35%.

[0043] In this embodiment, the hydrogen bonds in the surface cortex of the aramid fibers in the mixed fiber fabric after slight swelling are partially broken, the roughness increases, and the specific surface area increases, so that the actual contact area between the impregnating resin and the mixed fiber fabric increases, and a stronger mechanical locking effect is produced between the impregnating resin and the aramid fibers in the mixed fiber fabric, thereby improving the bonding strength between the mixed fiber fabric and the impregnating resin, and at the same time, it can also improve the bonding strength between the self-lubricating fabric liner and the steel substrate, so that the slightly swelled grafted modified self-lubricating fabric liner exhibits better load-bearing capacity in high shear stress friction conditions.

[0044] See also Figure 1 and Figure 2 , Figure 1 is a SEM image of aramid fiber in a modified mixed fiber fabric provided by an embodiment of the present invention; Figure 2 This is a SEM image of an unmodified aramid fiber in a mixed fiber fabric provided by an embodiment of the present invention. The micro-nano filler is graphene oxide. It can be seen from the figure that the graphene oxide in the modified mixed fiber fabric is connected to the slightly swollen aramid fiber, and compared with the aramid fiber in the unmodified mixed fiber fabric, the surface cortical hydrogen bonds of the aramid fiber in the slightly swollen mixed fiber fabric are partially broken, and the roughness is significantly increased.

[0045] In a second aspect, the present invention provides a method for preparing a slightly swellable graft-modified self-lubricating fabric liner, which is applicable to the slightly swellable graft-modified self-lubricating fabric liner provided in the first aspect. Figure 3 , Figure 3 It is a schematic diagram of a method for preparing a slightly swelling grafted modified self-lubricating fabric liner provided in an embodiment of the present invention.

[0046] like Figure 3 As shown, the preparation method of the slightly swellable graft modified self-lubricating fabric liner of this embodiment comprises the following steps:

[0047] Step 1: Clean the mixed fiber fabric.

[0048] In an optional embodiment, the mixed fiber fabric may be ultrasonically cleaned for 6-12 hours using acetone and petroleum ether respectively.

[0049] Step 2: Add the micro-nano filler, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 3-amino-1,2,4-triazole into pure water for modification reaction to obtain a modified solution, and sequentially perform alcohol washing, centrifugation and drying on the modified solution to obtain a modified micro-nano filler.

[0050] In an optional embodiment, the mass ratio of the micro-nano filler, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 3-amino-1,2,4-triazole is (1-3):(10-15):(3-5).

[0051] In an optional embodiment, the reaction temperature of the modification reaction is 60-80° C., and the reaction time is 1-3 h.

[0052] Optionally, the micro-nano filler is graphene oxide or carboxylated carbon nanotubes.

[0053] Step 3: Add N,N-dimethylacetamide and the modified micro-nano filler into pure water and mix them to obtain a slightly swollen grafting solution.

[0054] In an optional embodiment, the mass fraction of N,N-dimethylacetamide in the slightly swelling grafting solution is 10%-20%, and the mass fraction of the modified micro-nano filler in the slightly swelling grafting solution is 0.1%-0.5%.

[0055] Step 4: soaking the cleaned mixed fiber fabric in a slightly swellable grafting solution, performing a grafting reaction by infrared heating, and performing ultrasonic cleaning and drying treatments on the slightly swellable grafted mixed fiber fabric in sequence to obtain a modified mixed fiber fabric.

[0056] In an optional embodiment, the volume ratio of the mixed fiber fabric after washing to the slightly swelling grafting solution is 1:(20-25).

[0057] In an optional embodiment, the reaction temperature of the grafting reaction is 80-100° C., and the reaction time is 1-3 h.

[0058] In this embodiment, the slightly swollen grafted mixed fiber fabric is placed in an ultrasonic cleaning machine for ultrasonic cleaning, so as to remove the micro-nano fillers deposited on the fabric surface that have not been grafted with the aramid fibers in the slightly swollen mixed fiber fabric.

[0059] Step 5: placing the modified mixed fiber fabric in an impregnation solution containing an impregnation resin, and subjecting the impregnation solution to multiple ultrasonic, rolling and drying cycles to obtain a composite modified mixed fiber fabric.

[0060] In an optional embodiment, the impregnating liquid is a mixed solution of an impregnating resin and a diluent.

[0061] Optionally, the mass fraction of the impregnating resin in the impregnating liquid is 15%-35%, and the diluent is a mixture of anhydrous ethanol and ethyl acetate in a mass ratio of 1:1.

[0062] Optionally, the impregnating resin includes at least one of phenolic resin, modified epoxy resin, bismaleimide resin and modified cyanate resin.

[0063] In this embodiment, ultrasonic vibration is used during the impregnation process to allow the impregnation resin to fully adhere to the modified mixed fiber fabric, and the bubbles generated during the impregnation process can be discharged through roller pressing.

[0064] In an optional embodiment, the modified mixed fiber fabric is placed in an impregnation solution containing an impregnation resin and subjected to 4-6 cycles of ultrasound, rolling and drying until the impregnation resin reaches the corresponding mass fraction requirement, i.e., 25%-35%, to obtain a composite modified mixed fiber fabric.

[0065] Optionally, each ultrasonication time is 10 min-30 min, each rolling number is 4-6 times, each drying temperature is 55° C.-65° C., and the drying time is 10 min-30 min.

[0066] Step 6: Curing and molding the composite modified mixed fiber fabric to obtain a slightly swellable grafted modified self-lubricating fabric liner.

[0067] In an optional embodiment, the composite modified mixed fiber fabric loaded with impregnated resin can be cured and formed by hot pressing, wherein the pressure required to be applied during the curing process is 0.5MPa-2MPa, the hot pressing temperature is 160℃-200℃, and the hot pressing time is 1h-3h.

[0068] Optionally, during hot pressing, a layer of non-stick paper may be placed on the upper and lower surfaces of the composite modified mixed fiber fabric respectively, and then hot pressing and curing are performed on a hot press.

[0069] In this embodiment, the hot pressing pressure of hot pressing curing is 0.5MPa, the heating rate is 3℃ / min, the hot pressing temperature is 180℃, and the holding time is 3h. In other optional embodiments, the hot pressing curing stage can be divided into two stages, wherein the first stage is heated to 80℃-120℃ at a heating rate of 1℃ / min-3℃ / min and maintained for 50min-80min; the second stage is heated to 160℃-200℃ at a heating rate of 1℃ / min-3℃ / min and maintained for 50min-80min.

[0070] In a third aspect, the present invention provides an application of the micro-swelling grafted modified self-lubricating fabric liner provided in the first aspect in a self-lubricating spherical bearing. The present invention does not specifically limit the application method, and any method known in the art can be used. Specifically, the micro-swelling grafted modified self-lubricating fabric liner can be pasted on the inner lining surface of the metal spherical bearing.

[0071] Furthermore, the technical solution of the present invention will be clearly and completely described in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0072] In the following examples, the surface density of the mixed fiber fabric is 300 g / m 2 , thickness is 0.3mm, diameter of aramid fiber is 200D, diameter of PTFE fiber is 200D.

[0073] Example 1

[0074] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0075] Step 2: Add 0.2 g of graphene oxide, 3 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.6 g of 3-amino-1,2,4-triazole into 100 ml of pure water, react at 70°C for 2 h to obtain a modified solution, and wash the modified solution with alcohol, centrifuge and dry it in turn to obtain modified graphene oxide.

[0076] Step 3: Add 100 g of N,N-dimethylacetamide and 2 g of modified graphene oxide into 900 g of pure water and mix to obtain a slightly swollen grafting solution.

[0077] Step 4: Soak the cleaned mixed fiber fabric in a slightly swellable grafting solution, and use infrared heating to react at 90°C for 2 hours to obtain a slightly swellable grafted mixed fiber fabric. The slightly swellable grafted mixed fiber fabric is then ultrasonically cleaned and dried in turn to obtain a modified mixed fiber fabric.

[0078] Step 5: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution, place the modified mixed fiber fabric in the impregnation solution, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite modified mixed fiber fabric.

[0079] Step 6: Place the composite modified mixed fiber fabric on the upper surface of AISI-1045 stainless steel, and place a layer of non-stick paper under the stainless steel and on the fabric respectively, and then perform hot pressing and curing on a hot press, wherein the hot pressing pressure is 0.5 MPa, the heating rate is 3°C / min, the hot pressing temperature is 180°C, and the holding time is 3 hours to obtain a slightly swelling grafted modified self-lubricating fabric liner.

[0080] Example 2

[0081] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a plain weave fabric.

[0082] Step 2: Add 0.2 g of graphene oxide, 3 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.6 g of 3-amino-1,2,4-triazole into 100 ml of pure water, react at 70°C for 2 h to obtain a modified solution, and wash the modified solution with alcohol, centrifuge and dry it in turn to obtain modified graphene oxide.

[0083] Step 3: Add 100 g of N,N-dimethylacetamide and 2 g of modified graphene oxide into 900 g of pure water and mix to obtain a slightly swollen grafting solution.

[0084] Step 4: Soak the cleaned mixed fiber fabric in a slightly swellable grafting solution, and use infrared heating to react at 90°C for 2 hours to obtain a slightly swellable grafted mixed fiber fabric. The slightly swellable grafted mixed fiber fabric is then ultrasonically cleaned and dried in turn to obtain a modified mixed fiber fabric.

[0085] Step 5: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution, place the modified mixed fiber fabric in the impregnation solution, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite modified mixed fiber fabric.

[0086] Step 6: Place the composite modified mixed fiber fabric on the upper surface of AISI-1045 stainless steel, and place a layer of non-stick paper under the stainless steel and on the fabric respectively, and then perform hot pressing and curing on a hot press, wherein the hot pressing pressure is 0.5 MPa, the heating rate is 3°C / min, the hot pressing temperature is 180°C, and the holding time is 3 hours to obtain a slightly swelling grafted modified self-lubricating fabric liner.

[0087] Example 3

[0088] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0089] Step 2: Add 0.2 g of graphene oxide, 3 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.6 g of 3-amino-1,2,4-triazole into 100 ml of pure water, react at 70°C for 2 h to obtain a modified solution, and wash the modified solution with alcohol, centrifuge and dry it in turn to obtain modified graphene oxide.

[0090] Step 3: Add 200 g of N,N-dimethylacetamide and 2 g of modified graphene oxide into 800 g of pure water and mix to obtain a slightly swollen grafting solution.

[0091] Step 4: Soak the cleaned mixed fiber fabric in a slightly swellable grafting solution, and use infrared heating to react at 90°C for 3 hours to obtain a slightly swellable grafted mixed fiber fabric. The slightly swellable grafted mixed fiber fabric is then ultrasonically cleaned and dried in turn to obtain a modified mixed fiber fabric.

[0092] Step 5: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution, place the modified mixed fiber fabric in the impregnation solution, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite modified mixed fiber fabric.

[0093] Step 6: Place the composite modified mixed fiber fabric on the upper surface of AISI-1045 stainless steel, and place a layer of non-stick paper under the stainless steel and on the fabric respectively, and then perform hot pressing and curing on a hot press, wherein the hot pressing pressure is 0.5 MPa, the heating rate is 3°C / min, the hot pressing temperature is 180°C, and the holding time is 3 hours to obtain a slightly swelling grafted modified self-lubricating fabric liner.

[0094] Example 4

[0095] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0096] Step 2: Add 0.2 g of carboxylated carbon nanotubes, 3 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.6 g of 3-amino-1,2,4-triazole into 100 ml of pure water, react at 70°C for 2 hours to obtain a modified solution, and wash the modified solution with alcohol, centrifuge and dry it in turn to obtain modified carboxylated carbon nanotubes.

[0097] Step 3: Add 100 g of N,N-dimethylacetamide and 2 g of modified carboxylated carbon nanotubes into 900 g of pure water and mix them to obtain a slightly swollen grafting solution.

[0098] Step 4: Soak the cleaned mixed fiber fabric in a slightly swellable grafting solution, and use infrared heating to react at 90°C for 2 hours to obtain a slightly swellable grafted mixed fiber fabric. The slightly swellable grafted mixed fiber fabric is then ultrasonically cleaned and dried in turn to obtain a modified mixed fiber fabric.

[0099] Step 5: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution, place the modified mixed fiber fabric in the impregnation solution, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite modified mixed fiber fabric.

[0100] Step 6: Place the composite modified mixed fiber fabric on the upper surface of AISI-1045 stainless steel, and place a layer of non-stick paper under the stainless steel and on the fabric respectively, and then perform hot pressing and curing on a hot press, wherein the hot pressing pressure is 0.5 MPa, the heating rate is 3°C / min, the hot pressing temperature is 180°C, and the holding time is 3 hours to obtain a slightly swelling grafted modified self-lubricating fabric liner.

[0101] Example 5

[0102] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a satin fabric.

[0103] Step 2: Add 0.6 g of graphene oxide, 3 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 1 g of 3-amino-1,2,4-triazole to 100 ml of pure water, react at 70°C for 2 hours to obtain a modified solution, and wash the modified solution with alcohol, centrifuge and dry it in turn to obtain modified graphene oxide.

[0104] Step 3: Add 100 g of N,N-dimethylacetamide and 2 g of modified graphene oxide into 900 g of pure water and mix to obtain a slightly swollen grafting solution.

[0105] Step 4: Soak the cleaned mixed fiber fabric in a slightly swellable grafting solution, and use infrared heating to react at 90°C for 2 hours to obtain a slightly swellable grafted mixed fiber fabric. The slightly swellable grafted mixed fiber fabric is then ultrasonically cleaned and dried in turn to obtain a modified mixed fiber fabric.

[0106] Step 5: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution, place the modified mixed fiber fabric in the impregnation solution, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite modified mixed fiber fabric.

[0107] Step 6: Place the composite modified mixed fiber fabric on the upper surface of AISI-1045 stainless steel, and place a layer of non-stick paper under the stainless steel and on the fabric respectively, and then perform hot pressing and curing on a hot press, wherein the hot pressing pressure is 0.5 MPa, the heating rate is 3°C / min, the hot pressing temperature is 180°C, and the holding time is 3 hours to obtain a slightly swelling grafted modified self-lubricating fabric liner.

[0108] Example 6

[0109] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0110] Step 2: Add 0.4 g of carboxylated carbon nanotubes, 2.4 g of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 0.8 g of 3-amino-1,2,4-triazole into 100 ml of pure water, react at 70°C for 2 hours to obtain a modified solution, and wash the modified solution with alcohol, centrifuge and dry it in turn to obtain modified carboxylated carbon nanotubes.

[0111] Step 3: Add 200 g of N,N-dimethylacetamide and 2 g of modified carboxylated carbon nanotubes into 800 g of pure water and mix them to obtain a slightly swollen grafting solution.

[0112] Step 4: Soak the cleaned mixed fiber fabric in a slightly swellable grafting solution, and use infrared heating to react at 90°C for 3 hours to obtain a slightly swellable grafted mixed fiber fabric. The slightly swellable grafted mixed fiber fabric is then ultrasonically cleaned and dried in turn to obtain a modified mixed fiber fabric.

[0113] Step 5: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution, place the modified mixed fiber fabric in the impregnation solution, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite modified mixed fiber fabric.

[0114] Step 6: Place the composite modified mixed fiber fabric on the upper surface of AISI-1045 stainless steel, and place a layer of non-stick paper under the stainless steel and on the fabric respectively, and then perform hot pressing and curing on a hot press, wherein the hot pressing pressure is 0.5 MPa, the heating rate is 3°C / min, the hot pressing temperature is 180°C, and the holding time is 3 hours to obtain a slightly swelling grafted modified self-lubricating fabric liner.

[0115] Comparative Example 1

[0116] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0117] Step 2: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, and evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution.

[0118] Step 3: placing the cleaned mixed fiber fabric in an impregnating solution, and subjecting the mixed fiber fabric to 4-6 cycles of ultrasonic treatment, rolling and drying, until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite mixed fiber fabric.

[0119] Step 4: Place a layer of non-stick paper on the upper and lower surfaces of the composite mixed fiber fabric respectively, and then perform hot pressing and curing on a hot press. The hot pressing temperature is 180°C, the heating rate is 3°C / min, the pressure is 0.5MPa, and the hot pressing time is 3h to obtain a self-lubricating fabric lining.

[0120] Comparative Example 2

[0121] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a plain fabric.

[0122] Step 2: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, and evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution.

[0123] Step 3: placing the cleaned mixed fiber fabric in an impregnating solution, and subjecting the mixed fiber fabric to 4-6 cycles of ultrasonic treatment, rolling and drying, until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite mixed fiber fabric.

[0124] Step 4: Place a layer of non-stick paper on the upper and lower surfaces of the composite mixed fiber fabric respectively, and then perform hot pressing and curing on a hot press. The hot pressing temperature is 180°C, the heating rate is 3°C / min, the pressure is 0.5MPa, and the hot pressing time is 3h to obtain a self-lubricating fabric lining.

[0125] Comparative Example 3

[0126] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0127] Step 2: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, and evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution.

[0128] Step 3: Add graphene oxide directly into the impregnation solution and stir evenly, the mass of graphene oxide is 10% of the mass of phenolic resin, place the cleaned mixed fiber fabric in the impregnation solution with graphene oxide filler, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of phenolic resin reaches 30%, thereby obtaining a composite mixed fiber fabric.

[0129] Step 4: Place a layer of non-stick paper on the upper and lower surfaces of the composite mixed fiber fabric respectively, and then perform hot pressing and curing on a hot press. The hot pressing temperature is 180°C, the heating rate is 3°C / min, the pressure is 0.5MPa, and the hot pressing time is 3h to obtain a self-lubricating fabric lining.

[0130] Comparative Example 4

[0131] Step 1: using acetone and petroleum ether to perform ultrasonic cleaning on the mixed fiber fabric for 6 hours respectively, wherein the mixed fiber fabric is a twill fabric.

[0132] Step 2: Evenly mix anhydrous ethanol and ethyl acetate in a mass ratio of 1:1 to obtain a diluent, and evenly mix the diluent and phenolic resin in a mass ratio of 1:7 to obtain an impregnation solution.

[0133] Step 3: Add carboxylated carbon nanotubes directly into the impregnation solution and stir evenly, the mass of the carboxylated carbon nanotubes being 10% of the mass of the phenolic resin, and place the cleaned mixed fiber fabric in the impregnation solution containing the carboxylated carbon nanotube filler, and perform 4-6 cycles of ultrasonication, rolling and drying until the mass fraction of the phenolic resin reaches 30%, thereby obtaining a composite mixed fiber fabric.

[0134] Step 4: Place a layer of non-stick paper on the upper and lower surfaces of the composite mixed fiber fabric respectively, and then perform hot pressing and curing on a hot press. The hot pressing temperature is 180°C, the heating rate is 3°C / min, the pressure is 0.5MPa, and the hot pressing time is 3h to obtain a self-lubricating fabric lining.

[0135] The friction coefficients of the slightly swellable grafted modified self-lubricating fabric pads prepared in Examples 1-4 and the self-lubricating fabric pads prepared in Comparative Examples 1-4 were tested, and friction tests were performed respectively. The friction coefficient and wear rate results of each pad are shown in Table 1.

[0136] Table 1

[0137]

[0138] The wear marks of the slightly swellable grafted modified self-lubricating fabric liner prepared in Example 1 after the friction test and the wear marks of the self-lubricating fabric liner prepared in Comparative Example 1 after the friction test were observed by scanning electron microscopy, see Figure 4 and Figure 5 , Figure 4 This is a SEM image of the wear scar of the slightly swellable grafted modified self-lubricating fabric liner prepared in Example 1 after the friction test; Figure 5 This is an SEM image of the wear marks on the self-lubricating fabric pad prepared in Example 1 after the friction test. It can be clearly seen from the image that the wear marks on the slightly swellable grafted modified self-lubricating fabric pad prepared in Example 1 after the friction test are not obvious, while the self-lubricating fabric pad prepared in Example 1 has relatively obvious wear marks after the friction test.

[0139] It should be noted that, in this article, the terms "comprises", "includes" or any other variations are intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also other elements not explicitly listed. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the presence of other identical elements in the article or device including the elements. The orientation or positional relationship indicated by "upper", "lower", "left", "right", etc. is based on the orientation or positional relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0140] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A slightly swellable grafted modified self-lubricating fabric liner, characterized in that: include: A modified mixed fiber fabric and an impregnating resin loaded on the modified mixed fiber fabric; The modified mixed fiber fabric is a slightly swollen mixed fiber fabric grafted with micro-nano fillers, and the micro-nano fillers include graphene oxide or carboxylated carbon nanotubes.

2. The slightly swelling graft modified self-lubricating fabric liner according to claim 1, characterized in that: The mixed fiber fabric is a woven fabric of aramid fiber and PTFE fiber, and the woven fabric is a plain fabric, a twill fabric or a satin fabric; The surface density of the mixed fiber fabric is 180-360g / m 2 The diameter of the aramid fiber is 200D-1000D, and the diameter of the PTFE fiber is 200D-1000D.

3. The slightly swelling graft modified self-lubricating fabric liner according to claim 2, characterized in that: The micro-nano filler and the slightly swollen aramid fiber are connected by using 3-amino-1,2,4-triazole as an interface hydrogen bond structure grafting bridge.

4. The slightly swelling graft modified self-lubricating fabric liner according to claim 1, characterized in that: The impregnating resin includes at least one of phenolic resin, modified epoxy resin, bismaleimide resin and modified cyanate resin.

5. The slightly swelling graft modified self-lubricating fabric liner according to claim 1, characterized in that: The mass fraction of the impregnating resin in the slightly swellable graft-modified self-lubricating fabric liner is 25%-35%.

6. A method for preparing a slightly swellable graft-modified self-lubricating fabric liner, characterized in that: The slightly swelling grafted modified self-lubricating fabric liner according to any one of claims 1 to 5, wherein the preparation method comprises: Cleaning of mixed fiber fabrics; Adding micro-nano fillers, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and 3-amino-1,2,4-triazole into pure water for modification reaction to obtain a modified solution, and sequentially washing the modified solution with alcohol, centrifuging and drying to obtain a modified micro-nano filler; Adding N,N-dimethylacetamide and the modified micro-nano filler into pure water and mixing them to obtain a slightly swollen grafting solution; The mixed fiber fabric after cleaning is immersed in the slightly swellable grafting solution, and a grafting reaction is performed by infrared heating, and the mixed fiber fabric after the slightly swellable grafting is subjected to ultrasonic cleaning and drying in sequence to obtain a modified mixed fiber fabric; placing the modified mixed fiber fabric in an impregnation solution containing an impregnation resin, and subjecting the impregnation solution to multiple ultrasonic, rolling and drying cycles to obtain a composite modified mixed fiber fabric; The composite modified mixed fiber fabric is solidified and formed to obtain a slightly swellable grafted modified self-lubricating fabric liner.

7. The method for preparing the slightly swelling graft modified self-lubricating fabric liner according to claim 6, characterized in that: The mass ratio of the micro-nano filler, the 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and the 3-amino-1,2,4-triazole is (1-3):(10-15):(3-5); The reaction temperature of the modification reaction is 60-80° C., and the reaction time is 1-3 hours.

8. The method for preparing the slightly swelling graft modified self-lubricating fabric liner according to claim 6, characterized in that: The mass fraction of N,N-dimethylacetamide in the slightly swelling grafting solution is 10%-20%, and the mass fraction of the modified micro-nano filler in the slightly swelling grafting solution is 0.1%-0.5%.

9. The method for preparing the slightly swelling graft modified self-lubricating fabric liner according to claim 6, characterized in that: The volume ratio of the mixed fiber fabric after the cleaning treatment to the slightly swollen grafting solution is 1:(20-25); the reaction temperature of the grafting reaction is 80-100° C., and the reaction time is 1-3 hours.

10. Use of the slightly swellable graft-modified self-lubricating fabric liner according to any one of claims 1 to 5 in a self-lubricating spherical bearing.