Dyeing method of regenerated polyester air layer fabric containing disperse turquoise blue and active turquoise blue series
By adding Setamo LD in two steps and controlling the heating curve during the dyeing process, and pre-adding alkali treatment, the color stain problem easily caused by the recycled polyester fabric, the color stain problem is solved, and the fabric quality and corporate efficiency are significantly improved.
Patent Information
- Application Number
- CN202411230101.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-12-06
AI Technical Summary
Recycled polyester fabrics are prone to adsorption and aggregation of dyes, resulting in fabric quality problems such as color stains, due to their high oil content and rapid dyeing.
The method of adding the high-temperature resistant dispersant Setamo LD in two steps and controlling the dyeing and detergent heating curve is adopted. The alkali treatment is pre-added to adjust the pH of the dye solution to ensure that the dispersed and active turtle is uniformly dyed and avoiding local aggregation.
It effectively avoids the occurrence of color stain problems on the cloth, greatly improves the quality of the cloth, basically eliminates color stain remediation and scrapping, and improves corporate efficiency.
Smart Images

Figure CN119083199A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dyeing and finishing, and relates to a dyeing method for a regenerated polyester air layer fabric containing dispersed turquoise and active turquoise. Background Art
[0002] In an era of increasingly scarce resources and people's growing awareness of environmental protection, recycled polyester fabrics, as a new type of environmentally friendly recycled fabric, are increasingly favored by China and European and American countries. The research and development of recycled polyester fabrics has great environmental significance. Recycled polyester fabric yarn is extracted from waste mineral water bottles and cola bottles, and is also commonly known as cola bottle environmentally friendly fabric. It is widely used in tank tops, skirts, children's clothing, pajamas, cheongsams, home textiles, etc. The use of recycled polyester fabrics has important positive significance for the low-carbon emission reduction and sustainable development advocated by my country. The production method of recycled polyester fabrics determines that its oil content is higher than that of ordinary polyester. Different batches of recycled polyester fabrics have certain differences in performance and color. If the oil is not removed cleanly during dyeing, dye adsorption and aggregation are likely to occur. Especially when there is turquoise dye, due to the fast dyeing speed of turquoise, dye adsorption and aggregation are more likely to occur, resulting in color stains, and even color flowers and other fabric quality problems.
[0003] The reason for the above problems is that the recycled polyester fabric has a high oil content and the turquoise dye is dyed quickly, which can easily lead to rapid adsorption and aggregation of the dye, resulting in color stains and other fabric quality problems. Summary of the invention
[0004] The purpose of the present invention is to provide a dyeing method for recycled polyester air layer fabric containing dispersed turquoise and active turquoise in order to address the above-mentioned problems existing in the prior art. The technical problem to be solved by the invention is how to improve the quality of the recycled polyester fabric which is prone to color stains when dyed with turquoise dye.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] The composition of the recycled polyester fabric is 75D / 36F semi-gloss recycled polyester DTY (surface) + 50D / 36F semi-gloss recycled polyester DTY (middle) + 40S / 1 cotton (lining) + 30D spandex air layer (full lining) CSQ00202. This fabric is an elastic air layer blended with recycled polyester and cotton. First, the recycled polyester air layer fabric is subjected to conventional oxygen bleaching using a Nisaka dyeing machine. The oxygen bleaching temperature is between 95-100℃, and then it is first dyed and washed. The dyeing and washing bath ratio is 1:14. In the first step of dyeing and washing, 2g / l color light stabilizer AD, 3g / l acid chelating dispersant HS, 2g / l dispersing and leveling agent RM-7025, and 0.7% of Setamo LD are added. In the second step, 1.5g / l glacial acetic acid and 0.15g / l sodium acetate are added, and the machine is run for 6 minutes after the addition. The third step is to add 0.3% Setamo LD, 0.4-0.5% Xialiling (yellow 6G-LS), 0.004-0.005% Xialiling (golden SWF-N), and 0.9-1.2% Xialiling (turquoise SWF). After adding the dye, run for 5 minutes to enter the heating stage. Raise to 80 degrees at a rate of 2 degrees / minute, and from 80 degrees to 100 degrees at a rate of 1 degree / minute, and keep warm at 100 degrees for 10 minutes. Raise from 100 degrees to 115 degrees at 0.7 degrees / minute, and keep warm at 115 degrees for 10 minutes. Then raise from 115 degrees to 128 degrees at a rate of 0.7 degrees / minute, and keep warm at 128 degrees for 45 minutes. Cool down to 100 degrees at a rate of 1 degree / minute, and then cool down to 70 degrees at a rate of 1.5 degrees / minute and drain. Then perform two reduction cleanings at 85 degrees.
[0007] After the above steps are completed, use the Bazzoni dyeing machine to dye the cotton. The bath ratio of cotton dyeing is 1:12. In the first step of dyeing, add 3g / l acid chelating dispersant HS and 0.6% Setamo LD. In the second step, add 40-70g / l of sodium sulfate, and pre-add alkali, add 2.0-4.0g / l soda ash, and measure the pH after running for 5 minutes, which is between 10.3-10.5. In the third step, add 1.0%-1.4% Yingcai Clone Yellow 4GL, 0.06-0.1% Yingcai Clone Blue BF, and 1.5-2.0% Yingcai Clone Turquoise. Heat up after running for 10 minutes. After rising to 80 degrees at 1 degree / minute, soda ash is added three times, each time linearly for 20 minutes, 2g / l soda ash is added for the first time, 5g / l soda ash is added for the second time, and 11g / l soda ash is added for the third time. Then keep warm for 30-50 minutes and drain. After drainage, enter post-treatment and color fixation.
[0008] 1. Add the high temperature resistant dispersant Setamol LD in two steps during dyeing and washing. Add a certain amount of Setamol LD before adding the dye, and then add a certain amount of Setamol LD when dispersing the turquoise blue dye, so that the dye is evenly dispersed and dyed evenly to avoid local aggregation of the dye. The conventional process is not to add Setamol LD or only add it before adding the dye, and not to add Setamol LD when dispersing the turquoise blue dye.
[0009] 2. Control the dyeing and washing temperature rise curve. Heat up slowly and control the heating rate between 0.7 degrees / minute and 2 degrees / minute. When the temperature reaches a certain temperature of 100 degrees and 115 degrees, keep it warm for 10 minutes before continuing to heat up. This dyeing temperature rise curve is specifically formulated for dyeing turquoise blue dyes.
[0010] 3. When dyeing cotton, use the pre-alkali process. Before adding the active turquoise dye, add some alkali to the Bazzoni dyeing machine to adjust the pH of the dye solution to between 10.3-10.5 and reduce the generation of foam in the dye solution. This process not only adds soda ash three times at 80 degrees after adding the dye, but also adds a certain amount of soda ash before adding the dye.
[0011] 4. Setamol LD is also added in the first step of cotton coating. Setamol LD is not added during the general process of cotton coating. The purpose of the above production process is to make dispersed turquoise and active turquoise dye the fabric evenly, avoid local rapid adsorption and aggregation of dyes, and thus avoid the problem of color stains on the fabric. Before this process was formulated, when dyeing the recycled polyester air layer fabric containing dispersed turquoise and active turquoise, color stains would appear on both the recycled polyester surface and the cotton surface of each cylinder of cloth. After using this dyeing processing method, after dyeing the recycled polyester fabric containing dispersed turquoise and active turquoise, no color stains were produced on the fabric surface, which greatly improved the quality of the fabric surface, basically eliminated the color stain repair and scrapping, and improved the company's benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a flow chart of dyeing and washing process.
[0013] Figure 2 This is the process flow chart of cotton coating. DETAILED DESCRIPTION
[0014] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0015] The composition of recycled polyester fabric is 75D / 36F semi-gloss recycled polyester DTY (surface) + 50D / 36F semi-gloss recycled polyester DTY (middle) + 40S / 1 cotton (lining) + 30D spandex air layer (full lining) CSQ00202. This fabric is an elastic air layer blended with recycled polyester and cotton. Figure 1As shown, the recycled polyester air layer fabric is first subjected to conventional oxygen bleaching with a Nisaka dyeing machine, and the oxygen bleaching temperature is between 95-100°C. After oxygen bleaching, it is first dyed and washed. The dyeing and washing bath ratio is 1:14. In the first step of dyeing and washing, 2g / l color light stabilizer AD, 3g / l acid chelating dispersant HS, 2g / l dispersing leveling agent RM-7025, and 0.7% of Setamo LD are added. In the second step, 1.5g / l glacial acetic acid and 0.15g / l sodium acetate are added, and the machine is run for 6 minutes after the addition. In the third step, 0.3% Setamo LD, 0.4-0.5% Xialiling (yellow 6G-LS), 0.004-0.005% Xialiling (golden SWF-N), and 0.9-1.2% Xialiling (turquoise blue SWF) are added. After the dye is added, the machine is run for 5 minutes to enter the heating stage. Raise the temperature to 80 degrees at a rate of 2 degrees / min, and from 80 degrees to 100 degrees at a rate of 1 degree / min, and keep it at 100 degrees for 10 minutes. Raise the temperature from 100 degrees to 115 degrees at a rate of 0.7 degrees / min, and keep it at 115 degrees for 10 minutes. Then raise the temperature from 115 degrees to 128 degrees at a rate of 0.7 degrees / min, and keep it at 128 degrees for 45 minutes. Cool down to 100 degrees at a rate of 1 degree / min, and then cool down to 70 degrees at a rate of 1.5 degrees / min and drain. Then perform two reduction cleanings at 85 degrees.
[0016] After the above process is completed, the cotton is covered with a Bazzoni dyeing machine. Figure 2 As shown, the bath ratio of cotton coating is 1:12. In the first step of cotton coating, 3g / l acid chelating dispersant HS and 0.6% Setamo LD are added. In the second step, 40-70g / l of sodium sulfate is added, and alkali is pre-added. 2.0-4.0g / l soda ash is added. After running for 5 minutes, the pH is measured, which is between 10.3-10.5. In the third step, 1.0%-1.4% Yingcai Clone Yellow 4GL, 0.06-0.1% Yingcai Clone Blue BF, and 1.5-2.0% Yingcai Clone Turquoise are added. The temperature is raised after running for 10 minutes. After rising to 80 degrees at 1 degree / minute, soda ash is added three times, each time linearly for 20 minutes, 2g / l soda ash is added for the first time, 5g / l soda ash is added for the second time, and 11g / l soda ash is added for the third time. Then keep warm for 30-50 minutes and drain. After drainage, enter post-treatment and color fixation.
[0017] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A dyeing method for a regenerated polyester air layer fabric containing dispersed turquoise and active turquoise, characterized in that: The composition of the recycled polyester air layer fabric is 75D / 36F semi-gloss recycled polyester DTY surface layer, 50D / 36F semi-gloss recycled polyester DTY middle layer, 40S / 1 cotton lining layer and 30D spandex air layer CSQ00202 full lining; firstly, the recycled polyester air layer fabric is subjected to conventional oxygen bleaching using a Nisaka dyeing machine, and the oxygen bleaching temperature is between 95-100℃; After oxygen bleaching, dyeing and washing are performed first. The steps of dyeing and washing include: 1) adding 2g / l color light stabilizer AD, 3g / l acid chelating dispersant HS, 2g / l dispersing and leveling agent RM-7025, and 0.7% of Setamo LD; 2) adding 1.5g / l glacial acetic acid and 0.15g / l sodium acetate, and running for 6 minutes after adding; 3) adding 0.3% Setamo LD, 0.4-0.5% Xialiling (yellow 6G-LS), 0.004-0.005% Xialiling (golden SWF-N), and 0.9-1.2% Xialiling (turquoise blue SWF), and adding After the dye is run for 5 minutes, it enters the heating stage; 4) Raise to 80°C at a rate of 2 degrees / min, and from 80°C to 100°C at a rate of 1°C / min, and then keep warm at 100°C for 10 minutes; 5) Raise from 100°C to 115°C at 0.7°C / min, and keep warm at 115°C for 10 minutes; 6) Raise from 115°C to 128°C at a rate of 0.7°C / min, and keep warm at 128°C for 45 minutes; 7) Cool down to 100°C at a rate of 1°C / min, and then cool down to 70°C at a rate of 1.5°C / min and then drain; 8) Then perform two reduction cleanings at 85°C; After dyeing and washing, cotton is applied. The steps of applying cotton are as follows: The cotton bath ratio is 1:12; 1), add 3g / l acid chelating dispersant HS, 0.6% Setamo LD; 2), add 40-70g / l sodium sulfate, and pre-add alkali, add 2.0-4.0g / l soda ash, and measure the pH after running for 5 minutes, which is between 10.3-10.5; 3), add 1.0%-1.4% Yingcai clone (yellow 4GL), 0.06-0.1% Yingcai clone (blue BF), 1.5-2.0% Yingcai clone (turquoise blue); 4), after running for 10 minutes, heat up to 80℃ at 1℃ / min, and then add soda ash three times, each time linearly for 20 minutes, add 2g / l soda ash for the first time, 5g / l soda ash for the second time, and 11g / l soda ash for the third time; 5), keep warm for 30-50 minutes and then drain, and then enter post-treatment and color fixation.