PHA coated paper

By using blends of crystalline PHA and amorphous PHA in PHA coating materials and other additives, the process conditions are optimized, and the melting pressure instability and adhesion problems during coating processes are solved, and the film and paper are improved. Adhesion and slurry recovery rate improve the quality and environmental protection of the product.

CN119083242APending Publication Date: 2024-12-06BEIJING PHABUILDER BIOTECHNOLOGY CO LTD +1

Patent Information

Application Number
CN202410972084.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing PHA coating materials have problems such as unstable melting pressure, leakage of film, sticky rollers during coating, resulting in poor adhesion between the film and paper and low pulp recovery rate, affecting the quality and environmental protection of the product. .

Method used

A blend of crystalline PHA and amorphous PHA is used as the main material, and heat stabilizers, antioxidants, melt enhancers, nucleating agents and surfactants are added to optimize formula and process conditions and improve adhesion of film paper. and resorption rate.

Benefits of technology

It effectively solves the problems of melting pressure instability and adhesion in the coating process, improves the adhesion and slurry recovery rate between the film and paper, and enhances the use value and environmental protection of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides PHA (Polyhydroxyalkanoate) coated paper, the PHA coated paper comprises backing paper and a PHA film, and raw materials for preparing the PHA film comprise a blend of crystalline PHA and amorphous PHA; in the blend of the crystalline PHA and the amorphous PHA, the weight ratio of the crystalline PHA to the amorphous PHA is (40 / 60)-(95 / 5); the preferable weight ratio is 70 / 30 to 90 / 10; the pulp return rate of the coated paper is not lower than 75%. By optimizing the raw material formula of the PHA lamination material, the problems of unstable melt pressure, film leakage and roller adhesion in the lamination process are effectively solved, the balance between the adhesion and separation of film paper is effectively adjusted, the adhesion and pulp return rate of the film and the paper are improved, and the PHA lamination material has excellent market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a PHA coated paper. Background Art

[0002] At present, the degradable material polylactic acid (PLA) has become a hot topic in coating research, but PLA can only be degraded under industrial composting conditions. Polyhydroxyalkanoates (PHA) are a pure bio-source, 100% degradable emerging material. Compared with degradable materials such as PLA, polybutylene succinate (PBS), polybutylene adipate / terephthalate (PBAT), and polypropylene carbonate (PPC), the production, purification, and application process of PHA is greener and more bio-friendly. It does not require petroleum-based industrial products as a synthetic source. In addition, the degradation environment requirements are lower, and natural degradation can be achieved without composting. The paper-plastic composite material made of PHA will not cause environmental pollution.

[0003] However, PHA materials also have many disadvantages: ① The processing window is narrow, the heat resistance is poor, and the thermal decomposition temperature is close to the melting temperature. The pyrolysis is violent above 170°C, close to the melting temperature (Tm=165°C). ② The crystallization rate is low, the post-crystallization cycle is long, the product is easy to become brittle due to post-crystallization, and PHA in a viscous state is easy to stick to the roller. ③ The melt strength is low, and defects such as fracture and bubbles are prone to occur during lamination, affecting the appearance and performance of the product. ④ PHA has a high degree of crystallinity, the molecular chains are difficult to diffuse and entangle with each other, the surface tension is small, and the adhesion to paper is small, which is not conducive to the molding of laminated paper cups; ⑤ Because PHA is a hydrophobic substance, PHA laminated paper is not easy to re-slurry.

[0004] Chinese application CN114960278A discloses a method for preparing a plant fiber coated PHA oil-proof material, which includes the preparation of nanocellulose, modification of nanocellulose, modification of PHA, and coating the modified nanocellulose and PHA to obtain the PHA oil-proof material. The method esterifies the nanocellulose and compounds the modified PHA. Although the degradable oil-proof PHA coating material can be obtained while ensuring the performance of PHA, it still cannot solve at least the following problems: 1. The adhesion between PHA film and paper is poor, resulting in poor forming of paper cups and side seepage and leakage problems; 2. PHA coated paper cannot meet the needs of paper-plastic re-pulping, which greatly reduces its use value and environmental friendliness.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first object of the present invention is to provide a PHA coated paper to solve the problems of unstable melt pressure, film leakage, and sticking to rollers in the coating process of the existing PHA coated materials, thereby affecting the quality of the PHA coated paper, especially the adhesion between the film and the paper and the re-slurry rate.

[0007] As one of the technical solutions, the PHA coated paper provided by the present invention comprises a base paper and a PHA film, wherein the raw materials for preparing the PHA film include a blend of crystalline PHA and amorphous PHA; in the blend of crystalline PHA and amorphous PHA, the weight ratio of crystalline PHA to amorphous PHA is 40 / 60 to 95 / 5; preferably, the weight ratio is 70 / 30 to 90 / 10; The re-slurry rate of the coated paper is not less than 75%, preferably not less than 80%, 85%, 90% or even 95%.

[0008] As the second technical solution, the coated paper provided by the present invention includes a base paper and a PHA film, and the PHA film is made of a PHA coating material. The raw materials of the PHA coating material include the following components by weight: the raw materials for preparing the PHA film include the following components: 65~100 parts of a blend of crystalline PHA and amorphous PHA, 0.1~2 parts of a heat stabilizer, 0.1~2 parts of an antioxidant, 0.2~2 parts of a melt enhancer, 0.2~2 parts of a nucleating agent, and 0-2 parts of a surfactant.

[0009] Preferably, the raw materials include the following components: 80-100 parts of a blend of crystalline PHA and amorphous PHA, 0.2-1 parts of a heat stabilizer, 0.2-1 parts of an antioxidant, 0.2-1 parts of a melt enhancer, 0.2-1 parts of a nucleating agent, and 0.2-1 parts of a surfactant.

[0010] The present invention selects a blend of crystalline PHA (high strength) and amorphous PHA (high toughness, high elasticity) as the main material, which can ensure that the main material has the dual properties of high strength and high toughness.

[0011] Preferably, in the blend of crystalline PHA and amorphous PHA, the weight ratio of crystalline PHA to amorphous PHA is 40 / 60 to 95 / 5, and a more suitable weight ratio is 70 / 30 to 90 / 10.

[0012] In some embodiments provided by the present invention, the blend of crystalline PHA and amorphous PHA comprises 60 to 95 parts of at least one crystalline PHA and 5 to 40 parts of at least one amorphous PHA; the dosage ratio of the two is preferably 3 to 4:1; more preferably, the dosage of the blend of crystalline PHA and amorphous PHA in the raw material is 65 to 100 parts, and the suitable dosage is 65 parts, 80 parts, 85 parts, 90 parts, 95 parts, 100 parts, etc.

[0013] The PHA described in the present invention includes but is not limited to one or a combination of two or more of polyhydroxybutyrate (PHB), poly 3-hydroxybutyrate / 3-hydroxyvalerate (PHBV), poly 3-hydroxybutyrate / 3-hydroxyhexanoate (PHBHHx), poly-3-hydroxyoctanoate (PHO), poly-3-hydroxydecanoate (PHD), poly-3-hydroxydodecanoate (PHDD), and poly 3-hydroxybutyrate / 4-hydroxybutyrate copolymer (P34HB).

[0014] Preferably, the crystalline PHA is selected from one or a combination of two or more of PHB, PHBV, PHBHHx, PHO, PHD, PHDD, and P34HB; and the amorphous PHA is selected from PHBHHx and / or P34HB.

[0015] As a preferred embodiment of the present invention, the blend of crystalline PHA and amorphous PHA is obtained by physically blending crystalline PHB and amorphous P34HB or PHBHHx in a ratio of 3 to 4:1, or crystalline PHBV and amorphous P34HB or PHBHHx in a ratio of 3 to 4:1, or crystalline PHBHHx and amorphous P34HB or PHBHHx in a ratio of 3 to 4:1, or crystalline P34HB and amorphous P34HB or PHBHHx in a ratio of 3 to 4:1. The above blends particularly exhibit excellent film-forming properties during the coating process, forming a PHA-based coating modified material with both strength and toughness.

[0016] In some embodiments of the present invention, the PDI of the amorphous PHA is 1.5-3.0, a suitable range is, for example, 1.5-2.5, preferably 1.6-2.1, etc.

[0017] In some embodiments of the present invention, the PDI of the PHBHHx is ≤3, and more preferably the PDI is 1.6-2.0.

[0018] In some specific embodiments of the present invention, the PDI of the PHBHHx is 1.6, 1.7, 1.8, 1.9 or 2.0.

[0019] In some embodiments of the present invention, the PDI of the P34HB is ≤2.5, preferably the PDI is 1.6-2.1.

[0020] In some specific embodiments of the present invention, the PDI of the P34HB is 1.6, 1.7, 1.8, 1.9, 2.0 or 2.1.

[0021] The PHA coated paper provided by the present invention, the heat stabilizer in the PHA coated material is selected from one or more of zinc stearate, calcium stearate, calcium ricinoleate, phosphite, dibasic lead phthalate, epoxide, glyceride and zinc ricinoleate, preferably zinc stearate, which can effectively stabilize the state of the material system during the coating process.

[0022] The PHA coated paper provided by the present invention, wherein the antioxidant in the PHA coated material is one or a combination of two or more of antioxidant 1010, antioxidant 1076, thioester (preferably antioxidant DLTDP, antioxidant DSTDP) and phosphite (preferably antioxidant 168), preferably a combination of two antioxidants, such as antioxidant 1010+antioxidant 168 in a weight ratio of 1:2 to 1:1, antioxidant 1076+antioxidant DLTDP in a weight ratio of 1:1 to 1:2, etc.

[0023] The PHA coated paper provided by the present invention comprises a nucleating agent in the PHA coated material, which comprises one or a combination of two or more of boron nitride (BN), sorbitol, aromatic phosphate salts, sodium cinnamate, phosphate metal salts, phosphate basic metals, and sorbitol benzyl derivatives.

[0024] The PHA coated paper provided by the present invention, the melt enhancer in the PHA coated material is selected from one or more combinations of Joncryl ADR-4368, BASF ADR 4400, BASF ADR 4468, chain extender DX-5, chain extender 6901, chain extender MSA7200, and chain extender HER. In the PHA coated material provided by the present invention, the surfactant is selected from one or more combinations of polyethylene glycol octadecyl ether, polysorbate, aromatic polyethylene oxide, sorbitan derivatives, block copolymers of polyethylene oxide and polypropylene oxide, polyethylene glycol ether, polyvinyl alcohol, alkyl sulfates, alkyl phosphates, stearates, and alkylphenol polyether phosphates, preferably one or more combinations of polyethylene glycol octadecyl ether and alkylphenol polyether phosphate TXP-10.

[0025] The PHA coated paper provided by the present invention comprises, in addition to the above raw materials, a wetting and dispersing agent. The weight amount of the wetting and dispersing agent in the above raw materials is 0-2 parts, preferably 0.1-1 parts, especially 0.2-0.5 parts.

[0026] The wetting and dispersing agent is selected from one or a combination of two or more of sulfonated oil, soap, pull-opening powder BX, soybean lecithin, mercaptans, hydrazides, mercaptan acetals, and polyoxyethylene alkylated ethers.

[0027] The present invention adds a proper amount of surfactant and wetting dispersant to the PHA coating material, which can effectively adjust the balance between the adhesion and separation of the film paper.

[0028] The PHA coating material provided by the present invention has a melt index of 2-8 g / 10 min.

[0029] The present invention optimizes the raw materials of PHA coating materials, effectively solves the problems of unstable melt pressure, film leakage and roller sticking in the coating process; effectively adjusts the balance between film-paper adhesion and separation, thereby improving the adhesion between the film and paper and the re-slurry rate.

[0030] The PHA coated paper provided by the present invention, the base paper can be conventional paper in the art, such as white cardboard, gray board, coated paper, offset paper, corrugated paper, writing paper, kraft paper, newsprint, etc. In the embodiment of the present invention, the paper used is white cardboard, and more preferably the base paper has a grammage of 20g / m 2 ~350g / m 2 .

[0031] Preferably, the gram weight of the PHA film is 5g / m 2 ~30g / m 2 .

[0032] The second object of the present invention is to provide a method for preparing the above-mentioned PHA coated paper, the method comprising the following steps: S1, mix all raw materials evenly to obtain a raw material mixture; S2, adding the raw material mixture into an extruder, melting, extruding and granulating to obtain a PHA coating material; S3, adding the PHA coating material into a coating extruder, and coating the base paper with an extrusion die.

[0033] In the preparation method provided by the present invention, in step S2: Preferably, the extruder is a twin-screw extruder, and the temperature settings of each section are: 110-130°C for the feeding section, 130-150°C for the compression section, 140-160°C for the homogenization section, and 150-165°C for the die head.

[0034] It is worth noting that the temperature of each section mentioned above is preferably increased gradually.

[0035] Preferably, the main engine speed is 180-220 rpm and the feeding speed is 8-12 Hz.

[0036] Preferably, the twin-screw processing temperature is 120-160°C, the screw speed is 150-300 rpm, and the wind blowing temperature is 30-60°C.

[0037] In step S2, the PHA coating material is prepared by granulating the strands through an air-blown conveyor belt.

[0038] In the preparation method provided by the present invention, in step S3: Preferably, the temperature settings of each section of the laminating extruder are: 150-170°C for the feeding section, 160-180°C for the compression section, 160-180°C for the homogenization section, and 170-180°C for the die head.

[0039] It is worth noting that the temperature of each section mentioned above is preferably increased gradually.

[0040] Preferably, the main machine speed is 15-25 rpm, the metering pump speed is 8-12 rpm, and the melt pressure is 5-8 MPa.

[0041] Preferably, the temperature of the traction rollers 1 and 2 is set between 50-100° C., the extrusion die is between the traction rollers 1 and 2, and the material flows out of the die and is compounded with paper to prepare a paper-plastic composite material.

[0042] Beneficial effects brought by the technical solution of the present invention: 1. Enhanced adhesion between PHA film and paper and higher peeling force; 2. PHA coated paper can be re-pulped and recycled, with a re-pulping rate of >90%; 3. The adhesion between PHA film and paper and the resizing property of PHA coated paper can be balanced by adjusting the modified formula; 4. The production process is simple, the cost is low, and it has broad application prospects. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0044] All raw materials involved in the following examples are known commercially available products, such as Joncryl ADR-4368 purchased from BASF (food grade), antioxidant 1010 purchased from Lianlong Supply Chain Management Co., Ltd., antioxidant DLTDP purchased from Songyuan Baifu Chemical (Tangshan) Co., Ltd., alkylphenol polyether phosphate TXP-10 purchased from Hai'an Petrochemical Plant, Jiangsu Province, and nucleating agent BN purchased from Liaoning Borda Technology Co., Ltd.

[0045] In the following examples, the base paper used in preparing the laminated paper was conventional white cardboard.

[0046] Example 1

[0047] This embodiment provides a PHA coating material, which includes, by weight, 80 parts of PHB, 20 parts of amorphous P34HB (PDI is 1.8), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTDP, and 0.5 parts of nucleating agent BN.

[0048] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: 60 parts of PHB, 40 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, and 0.5 parts of nucleating agent were weighed by mass and physically mixed for 25 minutes using a high-speed mixer.

[0049] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature of each section is set as follows: 120°C for the feeding section, 140°C for the compression section, 150°C for the homogenization section, and 155°C for the die head. The main engine speed is 200rpm, and the feeding speed is 10Hz. The PHA coating material is obtained by pulling and granulating the strips through a wind-blown conveyor belt. Preferably, the twin-screw processing temperature is 150°C, the screw speed is 250 rpm, and the wind blowing temperature is 45°C.

[0050] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 70℃ for traction roller 1 and 2, and the extrusion die head is between traction roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0051] This embodiment also provides a method for calculating the pulping rate of coated paper (the same below): specifically, the coated paper is cut into pieces, and then the sample is dissociated, the pulp is homogenized, and sieved, and finally the pulping rate of the coated paper is calculated.

[0052] Example 2

[0053] This embodiment provides a PHA coating material, which includes, by weight, 70 parts of PHB, 30 parts of amorphous P34HB (PDI is 1.7), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTDP, and 0.5 parts of nucleating agent BN.

[0054] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: 80 parts of PHB, 20 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, and 0.5 parts of nucleating agent were weighed by mass and physically mixed for 20 minutes using a high-speed mixer.

[0055] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature of each section is set as follows: 120°C for the feeding section, 140°C for the compression section, 150°C for the homogenization section, and 155°C for the die head. The main engine speed is 200rpm, and the feeding speed is 10Hz. The PHA coating material is obtained by granulating the strands through a wind-blown conveyor belt. Preferably, the twin-screw processing temperature is 120°C, the screw speed is 300 rpm, and the wind blowing temperature is 30°C.

[0056] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 50℃ for traction roller 1 and 2, and the extrusion die head is between traction roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0057] Example 3

[0058] This embodiment provides a PHA coating material, which includes, by weight, 80 parts of PHB, 20 parts of amorphous P34HB (PDI is 1.6), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTDP, and 0.5 parts of nucleating agent BN.

[0059] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: 80 parts of PHB, 20 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, and 0.5 parts of nucleating agent were weighed by mass and physically mixed for 30 minutes using a high-speed mixer.

[0060] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature settings of each section are: feeding section 120°C, compression section 140°C, homogenization section 150°C, die head 155°C, main engine speed is 200rpm, feeding speed is 10Hz, and granulation is performed by wind-blown conveyor belt drawing to obtain PHA coating special material. Preferably, the twin-screw processing temperature is 160°C, the screw speed is 150rpm, and the wind blowing temperature is 60°C.

[0061] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 100℃ for pulling roller 1 and 2, and the extrusion die head is between pulling roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0062] Example 4

[0063] This embodiment provides a PHA coating material, which includes, by weight, 90 parts of PHB, 10 parts of amorphous P34HB (PDI is 1.8), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTDP, and 0.5 parts of nucleating agent BN.

[0064] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: 80 parts of PHB, 20 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, and 0.5 parts of nucleating agent were weighed by mass and physically mixed for 25 minutes using a high-speed mixer.

[0065] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature of each section is set as follows: 120°C for the feeding section, 140°C for the compression section, 150°C for the homogenization section, and 155°C for the die head. The main engine speed is 200rpm, and the feeding speed is 10Hz. The PHA coating material is obtained by granulating the strips through a wind-blown conveyor belt. Preferably, the twin-screw processing temperature is 130°C, the screw speed is 250 rpm, and the wind blowing temperature is 50°C.

[0066] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 80℃ for traction roller 1 and 2, and the extrusion die head is between traction roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0067] This embodiment also provides a method for calculating the pulping rate of coated paper (the same below): specifically, the coated paper is cut into pieces, and then the sample is dissociated, the pulp is homogenized, and sieved, and finally the pulping rate of the coated paper is calculated.

[0068] Example 5

[0069] This embodiment provides a PHA coating material, which includes, by weight, 80 parts of PHB, 20 parts of P34HB (PDI is 1.9), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, 0.5 parts of nucleating agent, and 0.2 parts of alkylphenol polyether phosphate (TXP-10).

[0070] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: 80 parts of PHB, 20 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, 0.5 parts of nucleating agent, and 0.2 parts of alkylphenol polyether phosphate (TXP-10) were weighed by mass and physically mixed for 20-30 minutes using a high-speed mixer.

[0071] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature settings of each section are: 120°C for the feeding section, 140°C for the compression section, 150°C for the homogenization section, and 155°C for the die head. The main engine speed is 200rpm, and the feeding speed is 10Hz. The PHA coating material is obtained by pulling and granulating with a wind-blown conveyor belt. Preferably, the twin-screw processing temperature is 145°C, the screw speed is 220 rpm, and the wind blowing temperature is 40°C.

[0072] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 90℃ for traction roller 1 and 2, and the extrusion die head is between traction roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0073] Example 6

[0074] This embodiment provides a PHA coating material, which includes, by weight, 80 parts of PHB, 20 parts of P34HB (PDI is 2.0), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, 0.5 parts of nucleating agent, and 0.3 parts of polyethylene glycol octadecyl ether.

[0075] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: 80 parts of PHB, 20 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, 0.5 parts of nucleating agent, and 0.3 parts of polyethylene glycol octadecyl ether were weighed by mass and physically mixed for 20 minutes using a high-speed mixer.

[0076] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature of each section is set as follows: 120°C for the feeding section, 140°C for the compression section, 150°C for the homogenization section, and 155°C for the die head. The main engine speed is 200rpm, and the feeding speed is 10Hz. The PHA coating material is obtained by pulling and granulating the strips through a wind-blown conveyor belt. Preferably, the twin-screw processing temperature is 120°C, the screw speed is 200 rpm, and the wind blowing temperature is 40°C.

[0077] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 60℃ for pulling roller 1 and 2, and the extrusion die head is between pulling roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0078] Example 7

[0079] This embodiment provides a PHA coating material, which includes, by weight, 80 parts of PHB, 20 parts of P34HB (PDI is 1.8), 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, 0.5 parts of nucleating agent, 0.2 parts of alkylphenol polyether phosphate (TXP-10), and 0.3 parts of polyethylene glycol octadecyl ether.

[0080] This embodiment also provides a PHA coated paper and a preparation method thereof, and the preparation method specifically includes: S1: By mass, weigh 80 parts of PHB, 20 parts of P34HB, 0.3 parts of zinc stearate, 0.4 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.2 parts of antioxidant DLTP, 0.5 parts of nucleating agent, 0.2 parts of alkylphenol polyether phosphate (TXP-10), and 0.3 parts of polyethylene glycol octadecyl ether, and physically mix them for 30 minutes using a high-speed mixer.

[0081] S2: The mixed material is melt-extruded through a twin-screw extruder, and the temperature settings of each section are: 120°C for the feeding section, 140°C for the compression section, 150°C for the homogenization section, and 155°C for the die head. The main engine speed is 200rpm, and the feeding speed is 10Hz. The PHA coating material is obtained by granulating the strands through a wind-blown conveyor belt. Preferably, the twin-screw processing temperature is 160°C, the screw speed is 300 rpm, and the wind blowing temperature is 60°C.

[0082] S3: PHA coating material is added into the coating extruder, and the temperature of each section is set as follows: 160℃ for feeding section, 170℃ for compression section, 170℃ for homogenization section, 175℃ for die head, 20rpm for main engine, 10rpm for metering pump, 6MPa for melt pressure, 90℃ for traction roller 1 and 2, and the extrusion die head is between traction roller 1 and 2. The material flows out of the die head and is compounded with paper to prepare paper-plastic composite material, namely PHA coating paper.

[0083] Example 8

[0084] This embodiment provides a PHA coating material. Compared with Example 1, the only difference is the formula. Specifically, it includes 60 parts of PHB, 20 parts of amorphous PHBHHx (PDI is 1.8), 0.1 parts of zinc stearate, 0.1 parts of Joncryl ADR-4368, 0.1 parts of antioxidant 1010, 0.1 parts of antioxidant DLTDP, and 0.2 parts of nucleating agent BN.

[0085] Example 9

[0086] This embodiment provides a PHA coating material. Compared with Example 1, the only difference is the formula. Specifically, it includes 80 parts of PHD, 40 parts of amorphous PHBHHx (PDI is 1.6), 1 part of zinc stearate, 1 part of JoncrylADR-4368, 1 part of antioxidant 1010, 0.5 antioxidant DLTDP, and 1 part of nucleating agent BN, in parts by mass.

[0087] Example 10

[0088] This embodiment provides a PHA coating material. Compared with Example 1, the only difference is the formula. Specifically, it includes 96 parts of PHB, 24 parts of amorphous PHBHHx (PDI is 1.9), 2 parts of zinc stearate, 2 parts of JoncrylADR-4368, 1 part of antioxidant 1010, 1 antioxidant DLTDP, 2 parts of nucleating agent BN, and 0.3 parts of polyethylene glycol octadecyl ether in parts by mass.

[0089] Embodiment 11

[0090] This embodiment provides a PHA coating material. Compared with Example 1, the only difference is that the formula is different. Specifically, it includes 60 parts of PHBV, 20 parts of amorphous P34HB (PDI is 1.7), 0.5 parts of zinc stearate, 0.5 parts of Joncryl ADR-4368, 0.2 parts of antioxidant 1010, 0.3 parts of antioxidant DLTDP, 1 part of nucleating agent BN, and 0.2 parts of alkylphenol polyether phosphate (TXP-10) in parts by mass.

[0091] Test Example 1

[0092] This test example provides the performance indicators of various film-coated modified materials prepared in the present invention, and the test results are shown in Table 1 for details.

[0093] Table 1

[0094] This test example also provides the performance indicators of each coated paper prepared by the present invention, and the test results are shown in Table 2 for details.

[0095] Table 2

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A PHA coated paper, comprising a base paper and a PHA film, characterized in that: The raw materials for preparing the PHA film include a blend of crystalline PHA and amorphous PHA; in the blend of crystalline PHA and amorphous PHA, the weight ratio of crystalline PHA to amorphous PHA is 40 / 60 to 95 / 5; preferably, the weight ratio is 70 / 30 to 90 / 10; The re-slurry rate of the coated paper is not less than 75%.

2. A PHA coated paper, comprising a base paper and a PHA film, characterized in that: The PHA film is made of a PHA coating material. The raw materials of the PHA coating material include the following components by weight: 65-120 parts of a blend of crystalline PHA and amorphous PHA, 0.1-2 parts of a heat stabilizer, 0.1-2 parts of an antioxidant, 0.2-2 parts of a melt enhancer, 0.2-2 parts of a nucleating agent, and 0-2 parts of a surfactant.

3. The PHA coated paper according to claim 1 or 2, characterized in that: In the blend of crystalline PHA and amorphous PHA, the weight ratio of crystalline PHA to amorphous PHA is 40 / 60 to 95 / 5, preferably 70 / 30 to 90 / 10; And / or, the blend of crystalline PHA and amorphous PHA comprises 60 to 95 parts of at least one crystalline PHA and 5 to 40 parts of at least one amorphous PHA.

4. The PHA coated paper according to claim 1 or 2, characterized in that: The PHA includes one or a combination of two or more of PHB, PHBV, PHBHHx, PHO, PHD, PHDD, and P34HB; Preferably, the crystalline PHA is selected from one or a combination of two or more of PHB, PHBV, PHBHHx, PHO, PHD, PHDD, and P34HB; the amorphous PHA is selected from PHBHHx and / or P34HB; More preferably, the PDI of the amorphous PHA is 1.5 to 3.0; The PDI of the PHBHHx is ≤3, preferably 1.6-2.0; The PDI of the P34HB is ≤2.5, and preferably the PDI is 1.6-2.

1.

5. The PHA coated paper according to any one of claims 2 to 4, characterized in that: The heat stabilizer is selected from one or more of zinc stearate, calcium stearate, calcium ricinoleate, phosphite, dibasic lead phthalate, epoxide, glyceride and zinc ricinoleate; And / or, the antioxidant is one or a combination of two or more of antioxidant 1010, antioxidant 1076, thioester and phosphite.

6. The PHA coated paper according to any one of claims 2 to 5, characterized in that: The nucleating agent includes one or a combination of two or more of boron nitride, sorbitol, TMC-306, aromatic phosphate salts, sodium cinnamate, phosphate metal salts, phosphate basic metals, and sorbitol benzyl derivatives; And / or, the melt enhancer is selected from one or a combination of two or more of Joncryl ADR-4368, BASF ADR 4400, BASF ADR 4468, chain extender DX-5, chain extender 6901, chain extender MSA7200, and chain extender HER; And / or, the surfactant is selected from one or a combination of two or more of polyethylene glycol octadecyl ether, polysorbate, aromatic polyethylene oxide, sorbitan derivatives, block copolymers of polyethylene oxide and polypropylene oxide, polyethylene glycol ether, polyvinyl alcohol, alkyl sulfates, alkyl phosphates, stearates, and alkylphenol polyether phosphates.

7. The PHA coated paper according to any one of claims 2 to 6, characterized in that: The raw materials also include a wetting and dispersing agent; The wetting and dispersing agent is selected from one or a combination of two or more of sulfonated oil, soap, pull-opening powder BX, soybean lecithin, mercaptans, hydrazides, mercaptan acetals, and polyoxyethylene alkylated ethers.

8. The PHA coated paper according to any one of claims 1 to 7, characterized in that: The base paper is selected from white cardboard, grey board, coated paper, offset paper, corrugated paper, writing paper, kraft paper and newsprint.

9. The PHA coated paper according to any one of claims 1 to 8, characterized in that: The base paper has a grammage of 20 g / cm 2 ~350g / cm 2 , and / or, the gram weight of the PHA film is 5g / m 2 ~30g / m 2 .

10. The method for preparing the PHA coated paper according to any one of claims 1 to 9, characterized in that: The steps include: S1, mix all raw materials evenly to obtain a raw material mixture; S2, adding the raw material mixture into an extruder, melting, extruding and granulating to obtain a PHA coating material; S3, adding the PHA coating material into a coating extruder, and coating the base paper with an extrusion die.

Citation Information

Patent Citations

  • Preparation method of plant fiber coated PHA oil-proof material

    CN114960278A

  • Foaming material and preparation method thereof

    CN115785637A

  • Degradable full-bio-based coated paper for food as well as preparation method and application of degradable full-bio-based coated paper

    CN117364539A

  • Composition for biodegradable fiber and biodegradable fiber manufactured using the same

    CN117881820A

  • Special polyhydroxyalkanoate film blowing material and film

    CN118222074A

Cited By

  • High-bio-based biodegradable paper-plastic composite film and preparation method thereof

    CN120003135A