Method for determining content of sulfur in sulfonated polyether ether ketone
By using a releasing agent to cover the surface and bottom surface of the sulfonated polyether etherketone sample in the infrared absorption method of the resistance furnace, the problems of incomplete combustion and low signal strength caused by small sample density and loose aggregation state are solved, and sulfur is achieved The accurate and stable measurement of content improves the testing accuracy.
Patent Information
- Application Number
- CN202411576236.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-11-06
AI Technical Summary
The existing high-frequency combustion infrared absorption method and resistance furnace combustion infrared absorption method have problems such as large data fluctuations, inaccurate and incomplete combustion of samples with low sulfur content, especially due to the sample The density is small and the aggregation state is loose, resulting in incomplete sulfur release and low signal strength, affecting the test accuracy.
In the infrared absorption method of the resistance furnace combustion, a release promoter is used to cover the sample surface and bottom surface, and materials such as tungsten trioxide, calcium oxide, tin, nickel, etc. are selected as the release promoter. By adjusting its mass and melting point, it ensures that it is in the resistance furnace. It effectively promotes the complete combustion and centralized release of sulfur elements at temperature to avoid tailing and the sample being blown away by carrier gas.
It improves the stability and accuracy of the test, ensures the accurate determination of sulfur content, especially the detection accuracy of low sulfur content samples, and reduces the phenomenon of misalignment of the integral curve and low test results.
Smart Images

Figure CN119086479A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for determining the sulfur content in sulfonated polyetheretherketone, and belongs to the field of material analysis. Background Art
[0002] Sulfonated polyetheretherketone is a modified polymer material and a raw material for making proton exchange membranes, dialysis membranes, nanofiltration membranes, and ultrafiltration membranes with various functions. It is widely used in fuel cells, vanadium batteries, and wastewater treatment. Sulfonated polyetheretherketone is a sulfonic acid compound obtained by reacting polyetheretherketone with a sulfonating agent such as sulfuric acid or chlorosulfonic acid, and introducing a sulfonic acid group into the carbon atom in polyetheretherketone or connecting it with the sulfur atom in the sulfonating agent.
[0003] The sulfonation degree of sulfonated polyetheretherketone has an important influence on the performance of the material, and the sulfur content is the main parameter that determines its sulfonation degree. Therefore, it is very important to determine the sulfur content in sulfonated polyetheretherketone. At present, there are many methods for testing sulfur in materials, such as X-ray fluorescence spectroscopy, heating method, melting method, combustion method, etc. Among them, high-frequency combustion infrared absorption method is fast and accurate in detecting sulfur content.
[0004] The high-frequency combustion infrared absorption method is based on infrared absorption spectroscopy technology. The sample is placed in a high-frequency induction furnace for heating (magnetic conductive materials are added and a T-shaped crucible is used). Oxygen is introduced to burn the sulfur in it to generate sulfur dioxide (the carbon in it will burn to generate carbon dioxide). These generated gases form a mixed gas with the carrier gas (oxygen). After being purified by dust collecting tubes, drying tubes, purification tubes, catalytic tubes, etc. to remove dust and water vapor, the mixed gas containing sulfur dioxide enters the infrared absorption cell detection system, and the sulfur content is determined by measuring the change in infrared energy at a specific wavelength. However, due to the small density of sulfonated polyetheretherketone and its loose aggregation state, when tested by the high-frequency combustion infrared absorption method, the powder is easily blown away by the carrier gas, making it difficult to fully burn (it cannot be heated by magnetic conductive materials and remains on the crucible wall, etc.), resulting in large fluctuations and inaccuracies in the sulfur content analysis data. Especially for samples with low sulfur content, the number of powders to be measured is relatively large, which is more likely to cause incomplete combustion of the powder.
[0005] The infrared absorption method of resistance furnace combustion is to push the crucible (boat-type crucible) containing the sample to the combustion zone of the resistance furnace, so that the sample in the crucible burns in the oxygen flow; under the action of high temperature and oxygen flow, the sulfur element in the sample is converted into sulfur dioxide gas, and the mixed gas is purified through dust removal pipes, drying pipes, purification pipes, catalytic furnaces, etc. to remove dust, water vapor, etc., and the mixed gas containing sulfur dioxide is introduced into the infrared absorption cell detection system, and the content of sulfur in organic matter is calculated by measuring the change of infrared energy at a specific wavelength. The infrared absorption method of resistance furnace combustion can make the powder in the furnace burn completely. However, it was found during the test that the sulfur atoms in sulfonated polyetheretherketone were first released quickly and then slowly, which kept the signal intensity of sulfur element at a relatively low level for a long time during the test (tailing phenomenon), which led to large area integration error and inaccurate integral curve; in addition, sulfonated polyetheretherketone has a small density and a relatively loose aggregation state. When it is pushed into the resistance furnace, a very small part of the sample is blown down by the carrier gas at the mouth of the resistance furnace, which makes the sample incompletely burned, resulting in low test results and low test accuracy. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, the present invention provides a method for determining the sulfur content in sulfonated polyetheretherketone, which can make the sulfur element burn completely and release concentratedly in the resistance furnace combustion infrared absorption method, thereby suppressing the tailing phenomenon.
[0007] The technical solution adopted by the present invention to solve its technical problem is: A method for determining the sulfur content in sulfonated polyetheretherketone comprises the following steps: spreading the sample flat in a porcelain boat crucible, pushing the sample into a carbon-sulfur analyzer with a resistance furnace, and detecting the sulfur content by infrared absorption method; in the porcelain boat crucible, the upper surface of the sample is covered with a first release promoter powder, the sulfur content of the first release promoter is less than 0.0005%, and the first release promoter is selected from tungsten trioxide, calcium oxide, silicon dioxide, tin, nickel or iron.
[0008] The method for determining the sulfur content in sulfonated polyetheretherketone provided in the present application lays a layer of release promoter on the surface of the sample, which can prevent the loose sulfonated polyetheretherketone from being blown away by the carrier gas and avoid incomplete combustion of the sample. The release promoter can also promote the release of sulfur element in the sulfonated polyetheretherketone and avoid inaccuracy of the integral curve caused by slow sulfur release, which is beneficial to improving the stability and accuracy of the test.
[0009] Furthermore, the mass of the first release-accelerating agent is equivalent to 1.0 to 9.2 times the mass of the sample.
[0010] Further, when the melting point of the first release accelerator is lower than or equal to the temperature of the resistance furnace, the mass of the first release accelerator is equivalent to 2.3 to 3.2 times the mass of the sample; when the melting point of the first release accelerator is greater than the temperature of the resistance furnace, the mass of the first release accelerator is equivalent to 1.0 to 9.2 times the mass of the sample. Preferably, the first release accelerator is porous tungsten trioxide.
[0011] If the melting point of the first release promoter is lower than or equal to the temperature of the resistance furnace, the first release promoter will change from powder to dense liquid (or solid and liquid coexistence) after melting, which is not conducive to the overflow of sulfur dioxide gas; or the first release promoter has already flowed to the bottom of the crucible or outside the crucible during the experiment, which is not conducive to preventing the loose sulfonated polyetheretherketone sample from being blown away by the carrier gas. Therefore, when the melting point of the first release promoter is lower than or equal to the temperature of the resistance furnace, the amount of the first release promoter should not be too much or too little.
[0012] Furthermore, in the porcelain boat crucible, the lower surface of the sample is padded with a second release promoter powder, the sulfur content of the second release promoter is less than 0.0005%, and the second release promoter is selected from tungsten trioxide, calcium oxide, silicon dioxide, tin, nickel or iron.
[0013] Furthermore, the mass of the second release-accelerating agent is equivalent to 0.1 to 1.6 times the mass of the sample.
[0014] Furthermore, the fineness of the second release enhancer powder is 200-300 mesh.
[0015] Furthermore, the fineness of the first release enhancer powder is 200-300 mesh.
[0016] Furthermore, the temperature of the resistance furnace is stabilized at 1280°C to 1320°C, and the O2 carrying capacity is 180L / h.
[0017] Furthermore, the integration endpoint time of the spectrum curve is 40s~300s. In the test program, the computer determines whether the test is over based on: one is that the change of the curve in the spectrum over time is less than a certain speed, it will automatically end (peak judgment factor); the other is the test time (integration endpoint time). If the test reaches the set minimum test time and does not meet the automatic end condition, it will be forced to end according to the preset test time (maximum test time). If the test time is less than the set minimum test time, the test meets the automatic end condition, and the test will not end until the test time reaches the set minimum test time.
[0018] Furthermore, the carbon-sulfur analyzer is calibrated with a standard substance, and a numerical relationship between the infrared spectrum intensity value and the sulfur content of the standard substance is established. The calibration method can be multi-point calibration or single-point calibration.
[0019] Furthermore, the standard substance is a coal standard.
[0020] The beneficial effects of the present invention are as follows: the method for determining the sulfur content in sulfonated polyetheretherketone of the present invention lays a layer of the first release promoter on the surface of the sample, which can cover the sample, prevent the loose sulfonated polyetheretherketone from being blown away by the carrier gas, and prevent incomplete combustion of the sample; and the release promoter can promote the release of sulfur element in the sulfonated polyetheretherketone, and avoid the inaccuracy of the integral curve caused by the slow release of sulfur from the sulfonated polyetheretherketone, which is beneficial to improving the stability and accuracy of the test. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a comparison diagram of infrared absorption spectra of Example 2 and Comparative Example 1.
[0022] Figure 2 It is a comparison diagram of the infrared absorption spectra of Example 3 and Comparative Example 1.
[0023] Figure 3 It is a comparison diagram of the infrared absorption spectra of Example 4 and Comparative Example 1.
[0024] Figure 4 It is a comparison diagram of the infrared absorption spectra of Example 5 and Comparative Example 1.
[0025] Figure 5 It is a comparison chart of infrared absorption spectra of Example 6 and Comparative Example 1.
[0026] Figure 6 It is a comparison chart of infrared absorption spectra of Example 9 and Comparative Example 1.
[0027] Figure 7 It is a comparison chart of infrared absorption spectra of Example 11, Example 4 and Comparative Example 1.
[0028] Figure 8 It is a comparison chart of infrared absorption spectra of Example 13 and Comparative Example 1.
[0029] Fig. 9 It is a comparison chart of the infrared absorption spectra of Example 21 and Comparative Example 3.
[0030] Fig.10 This is a comparison chart of the crucibles after testing the sulfonated polyetheretherketone SP9 of comparative example 3, the steel standard of comparative example 3, and the sulfonated polyetheretherketone SP9 of example 21. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present disclosure clearer, the technical solution of the embodiments of the present disclosure is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present disclosure, not all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Unless otherwise specified, all technical and scientific terms used herein have the standard meaning in the field to which the claimed subject matter belongs. If there are multiple definitions for a term, the definition herein shall prevail.
[0033] The following lists the materials used in the following embodiments and the precautions in the experiments: (1) A porcelain boat crucible (length × height: 88 mm × 10 mm, sulfur content less than 0.0005%) was placed in a muffle furnace and calcined at 1200°C for 4 hours before use. After being taken out and slightly cooled, it was stored in a desiccator.
[0034] (2) Oxygen: purity is 99.995%.
[0035] (3) Desiccant: anhydrous magnesium perchlorate, particle size 0.7 mm ~ 1.2 mm.
[0036] (4) Purifier: caustic soda asbestos, particle size 0.7mm~1.2mm.
[0037] (5) Release promoter: tungsten trioxide powder (200-300 mesh, porous structure), calcium oxide powder (200-300 mesh), silicon dioxide powder (200-300 mesh), tin powder (200-300 mesh), nickel powder (200-300 mesh), iron powder (200-300 mesh). Sulfur content is less than 0.0005%.
[0038] (6) Standard material: coal standard material (national first-class standard material).
[0039] (7) Before testing, check the carbon and sulfur analyzer for leaks and preheat the resistance furnace and high-frequency induction furnace for more than 3 hours.
[0040] (8) Operate according to the instrument instructions. The instrument will automatically analyze and obtain the test results.
[0041] (9) Calibration test: multi-point calibration or single-point calibration.
[0042] ①Multi-point calibration: Select 4 certified coal standard substances to calibrate the instrument, select one as the verification standard, and the other three as the calibration standards. The sulfur content of the verification standard is between the sulfur content of the three calibration standards. Analyze each calibration standard substance 3 to 5 times on the selected channel, establish a calibration curve, and then verify it with the verification standard. During the sample test, the verification standard is used for verification every 10 measurements. If the test result is out of range, recalibrate.
[0043] ② Single-point calibration: Select two coal standard substances or standard samples. The coal standard substances or standard samples should have a sulfur content close to that of the sample being analyzed. You can also control the mass number of the sample in a single test so that the absolute value of the sulfur content in the tested material is close to the absolute value of the sulfur content in the standard substance. Perform the single-point calibration procedure according to the requirements of the instrument manual. Analyze one of the standard substances / standard samples 3 to 5 times, calculate the average of these results, and perform system calibration. The average value is consistent with the standard value and does not exceed the uncertainty range given in the standard substance / sample certificate. Use another standard substance / standard sample as a sample for analysis to verify the calibration. The analysis result is within the uncertainty range of the standard value of the standard substance / standard sample.
[0044] (10) Before testing the samples, perform a blank value test: During the test, except for not adding samples, the same analytical steps, reagents and dosages are used for the test. The computer performs blank value deduction. During the subsequent sample testing, the computer automatically deducts the blank value. Repeat the test 3 to 5 times, and the computer performs the blank value test. If the blank value is greater than 0.002% and the standard deviation is greater than 0.0005%, find out the cause and take appropriate measures.
[0045] (11) Test process (resistance furnace combustion infrared pool absorption method): The sample is spread flat in a porcelain boat crucible, and then pushed into a resistance furnace (pure oxygen atmosphere) to be burned, so that the sulfur element is converted into a SO2 mixed gas (including CO, CO2 and other gases). The mixed gas then passes through a dust collector, a water removal well test tube, a desiccant reagent tube, a purifier reagent tube, and a catalyst reagent tube for dust removal, drying and purification, and finally enters the sulfur infrared absorption cell detection cell to absorb infrared light of a specific wavelength. By measuring the change in infrared energy of a specific wavelength, information on the S content can be obtained. Each sample is balanced and tested 3 to 5 times, and the relative standard error RSD is ≤4%, and the average value is taken.
[0046] The method of this application can detect sulfonated polyetheretherketone with a minimum sulfur content of 0.0128%. Due to the limited source of sulfonated polyetheretherketone, there is currently no sample with a concentration higher than 1.06%. The test range of sulfur in sulfonated polyetheretherketone in this application is 0.0128%~1.06%. The lower the sulfur content, the more difficult it is to detect. It can be expected that if there is a sample with a concentration higher than 1.06%, the upper limit of the test range of this application can be higher.
[0047] Example 1: Covered with silicon dioxide The temperature of the resistance furnace is stabilized at 1280℃~1320℃, the integral end time is set to 110s~300s, and the O2 flow rate is 180L / h. The multi-point calibration method is adopted. The sulfur content in the coal standard is 0.18%, 0.28%, 0.41%, and 0.76%, the mass number is 90mg~95mg, and the weight is accurate to 0.01mg. The correction factor is determined, and the sample with a sulfur content of 0.41% (mass number is 90mg~95mg, and the weight is accurate to 0.01mg) is used to verify the correction factor. After the calibration is completed, the blank value test and the sulfur content test in sulfonated polyetheretherketone are started.
[0048] Weigh 90mg~95mg (accurate to 0.01mg) of sulfonated polyetheretherketone SP1 and spread it evenly in a porcelain boat crucible, then cover the sample with auxiliary silica, the amount of silica is 3.1 times~3.2 times that of SP1, and then push the sample into the combustion zone of the resistance furnace for testing according to the equipment manual. The test results are calculated by directly deducting the blank value by the software. The test was performed 3 times independently, and the average value of the 3 tests was 0.241%, the RSD was 2.72%, and the average test time was 111s.
[0049] Example 2: Covered with tin The sulfur content in sulfonated polyetheretherketone SP1 was detected after calibrating the instrument and measuring the blank value according to the method and steps of Example 1, wherein the first release promoter was tin powder, and its dosage was 3.1 to 3.2 times that of SP1. The average value of 3 tests was 0.221%, and the RSD was 3.34%.
[0050] Comparative Example 1 The sulfur content in sulfonated polyetheretherketone SP1 was detected after calibrating the instrument and measuring the blank value according to the method and steps of Example 1, without adding a release promoter. The average value of 3 tests was 0.212%, the RSD was 3.76%, and the average test time was 111 s.
[0051] Comparing the infrared absorption spectra of Example 2 and Comparative Example 1, we can obtain Figure 1 . Figure 1In the chart, the vertical axis is the infrared light absorption intensity of a specific wavelength, in volts (V) (the signal intensity is converted into voltage for display); the horizontal axis is the analysis test time, in seconds. Figure 1 It can be seen that the sulfur release in Example 2 and Comparative Example 1 is fast at the beginning of the test, with an obvious intensity peak, and then the sulfur release slows down, and another intensity peak appears at 40-50s. This may be because the sulfur doping in the sulfonated polyetheretherketone SP1 causes different release rates at different positions, and the sulfur release in this part (at 40-50s) is relatively slow. The intensity peak at 40-50s of the test spectrum with the addition of tin release promoter is significantly higher than that of Comparative Example 1, indicating that the sulfur release rate is faster, and the test result is higher than that of Comparative Example 1. This should be that when the release promoter is not added, the sulfur in the sulfonated polyetheretherketone SP1 is first quickly released, and then the remaining part is slowly released, resulting in the signal intensity of the sulfur element being released at a relatively low level for a long time (tailing phenomenon), resulting in inaccurate integral curves and low test results. In Example 2, the sulfur release starts 6-7s slower than that in Comparative Example 1. This may be because the metal tin absorbs heat and melts at the beginning, and then the heat can be conducted to the sample, so the sulfur release will be delayed compared with Comparative Example 1.
[0052] Example 3: Covered with calcium oxide The sulfur content in sulfonated polyetheretherketone SP1 was detected after calibrating the instrument and measuring the blank value according to the method and steps of Example 1, wherein the first release promoter was calcium oxide, and its dosage was 5.5-5.6 times that of SP1. The average value of 3 tests was 0.241%, the RSD was 3.86%, and the average test time was 113s.
[0053] Comparing the test spectrum of Example 3 with that of Comparative Example 1, we obtain Figure 2 It is found that the first intensity peak of Example 3 is significantly delayed and shorter than that of Comparative Example 1, and then the second peak is significantly enhanced and delayed. This should be because calcium oxide absorbs heat at the beginning and causes slow heat transfer, so the first peak is significantly delayed and shorter, but the subsequent sulfur signal intensity is significantly enhanced and then drops rapidly, indicating that sulfur is released faster in the subsequent period, avoiding the tailing phenomenon.
[0054] Example 4: Nickel Covered The sulfur content in sulfonated polyetheretherketone SP1 was detected after calibrating the instrument and measuring the blank value according to the method and steps of Example 1, wherein the first release promoter was nickel powder, and its dosage was 7.4-7.5 times that of SP1. The average value of 3 tests was 0.248%, the RSD was 3.66%, and the average test time was 120s.
[0055] Comparing the test spectrum of Example 4 with that of Comparative Example 1, we obtain Figure 3, it is found that the first intensity peak of Example 4 is significantly delayed and shorter than that of Comparative Example 1, and then the second peak appears and then drops rapidly. This should be because the nickel powder absorbs heat and melts first at the beginning, and then the heat is transferred to the sample, so the first peak is significantly delayed and shorter, but the subsequent sulfur signal intensity is significantly enhanced and then drops rapidly, indicating that sulfur is released relatively quickly in the subsequent period, avoiding the tailing phenomenon. This also shows that the first release promoter cannot be added too much (covering too thickly), otherwise the sulfur release in the sample will be slow.
[0056] Example 5: Covered with tungsten trioxide The sulfur content in sulfonated polyetheretherketone SP1 was detected after calibrating the instrument and measuring the blank value according to the method and steps of Example 1, wherein the first release promoter was tungsten trioxide powder, and its dosage was 5.1-5.2 times that of SP1. The average value of 3 tests was 0.229%, the RSD was 3.81%, and the average test time was 111s.
[0057] Comparing the test spectrum of Example 5 with that of Comparative Example 1, we obtain Figure 4 It is found that the first intensity peak of Example 5 is significantly delayed compared with that of Comparative Example 1, and then the second peak appears and then drops rapidly. This indicates that the sulfur release rate becomes faster, and the test result is higher than that of Comparative Example 1. This should be because when no release promoter is added, a part of sulfur in sulfonated polyetheretherketone SP1 is first released quickly, and then the remaining part is slowly released, resulting in the signal intensity of sulfur element being released at a relatively low level for a long time (tailing phenomenon), resulting in inaccurate integral curve and low test results. In Example 5, the sulfur starts to be released 5 to 6 seconds slower than that of Comparative Example 1. This may be because tungsten trioxide absorbs heat at the beginning and then transfers it to the sample. Therefore, the sulfur starts to be released later than that of Comparative Example 1. The counting intensity of sulfur after the first peak is significantly higher than that of Comparative Example 1, indicating that the addition of tungsten trioxide can promote the release of sulfur, and the test result is higher than that of Comparative Example 1.
[0058] Example 6: Covered with iron powder The sulfur content in sulfonated polyetheretherketone SP1 was detected after calibrating the instrument and measuring the blank value according to the method and steps of Example 1, wherein the first release promoter was iron powder, and its dosage was 4.2 to 4.3 times that of SP1. The average value of 3 tests was 0.223%, the RSD was 3.65%, and the average test time was 111 seconds.
[0059] Comparing the test spectrum of Example 6 with that of Comparative Example 1, we obtain Figure 5 .
[0060] Example 7: Covering with tungsten trioxide on the top + laying tungsten trioxide on the bottom The temperature of the resistance furnace is stabilized at 1280℃~1320℃, the integral end time is set to 80s~300s, and the O2 carrying capacity is 180L / h. First, calibrate the instrument according to the method and steps of Example 1, and then perform blank value test and sample test. Weigh 50~53mg of tungsten trioxide and spread it on the bottom of the porcelain boat crucible as the second release promoter, then weigh 54~57mg (accurate to 0.01mg) of sulfonated polyetheretherketone SP1 and spread it on the upper layer of tungsten trioxide, and then weigh a certain amount of tungsten trioxide to cover the sample. The amount of the first release promoter is 3.2~3.4 times that of SP1, and then push the sample into the combustion zone of the resistance furnace for testing according to the equipment manual. The average value of the three tests is 0.227%, the average test time is 81s, and the RSD is 2.68%. After the test is completed, take the powder at the bottom of the crucible, its color is the same as tungsten trioxide and it is analyzed as tungsten trioxide.
[0061] Example 8: Covering with tin on the top + laying tin on the bottom The instrument was calibrated and the blank value was measured according to the method and steps of Example 7, and then the sulfur content in sulfonated polyetheretherketone SP1 was detected, wherein the amount of tin powder of the bottom release promoter (second release promoter) was 60-62 mg, and the amount of tin powder of the top layer (first release promoter) was 2.3-2.4 times that of SP1. The average value of 3 tests was 0.223%, the RSD was 3.65%, and the average test time was 82 s. After the test was completed, there was a layer of solid at the bottom of the crucible.
[0062] Comparing the test results of Example 8 with those of Example 2 and Comparative Example 1, the test time of Example 8 is significantly shorter than that of Comparative Example 1 and Example 2, and the test results are consistent with those of Example 2, but the second intensity peak is significantly higher than that of Example 2 and Comparative Example 1. This is because the amount of accelerator tin powder (the total amount of the first accelerator and the second accelerator in Example 8) is the same as that in Example 2 (Example 2 only has the first accelerator), but part of it is placed on the bottom and part of it is covered on the sample. The tin powder covered on the sample becomes thinner, the heat required for tin melting becomes less, and the heat transfer is faster, so the sulfur release time of Example 8 is significantly faster than that of Example 2 and slower than that of Comparative Example 1. At the same time, the tin powder on the bottom can increase the contact area between the sample and tin, which helps to promote the release of sulfur, so the sulfur release rate becomes faster.
[0063] Example 9: Tin padding on the bottom + tungsten trioxide covering on the top The instrument was calibrated and the blank value was measured according to the method and steps of Example 7, and then the sulfur content in sulfonated polyetheretherketone SP1 was detected, wherein the amount of tin powder as the bottom release promoter was 80-82 mg, and the amount of tungsten trioxide in the top layer was 2.3-2.4 times that of SP1. The average value of 3 tests was 0.224%, the RSD was 3.65%, and the average test time was 82 s. After the test was completed, there was a layer of powder containing solid tin at the bottom of the crucible.
[0064] Comparing the test spectrum of Example 9 with that of Comparative Example 1, we obtain Figure 6 The test time of Example 9 is significantly shorter than that of Comparative Example 1, and no tailing phenomenon occurs. This is because the contact area between the bottom tin and the sample becomes larger after melting, which promotes the release of S. At the same time, the surface is covered with tungsten trioxide and is not melted, which is conducive to the release of sulfur into the gas. Therefore, the test time is significantly shortened.
[0065] Example 10: Tungsten trioxide padding on the bottom + tin covering on the top The instrument was calibrated and the blank value was measured according to the method and steps of Example 7, and then the sulfur content in sulfonated polyetheretherketone SP1 was detected, wherein the amount of tungsten trioxide as the bottom release promoter was 80-82 mg, and the amount of tin as the top release promoter was 6.7-6.8 times that of SP1. The average value of 3 tests was 0.233%, the RSD was 2.42%, and the average test time was 92 s. After the test, there was a layer of solid and trace powder at the bottom of the crucible.
[0066] Comparing Example 9 with Example 10, it is found that the time when sulfur starts to be released in Example 10 is 3-4 seconds later than that in Example 9. This is because the tin powder covered is thicker and has a dense structure, which causes the heat transfer to the powder to be slightly slower. In addition, after the test, the bottom of the crucible of Example 10 is a layer of solid, which is tin metal containing tungsten trioxide, while the crucible of Example 9 contains a small amount of tungsten trioxide powder with tin. This shows that tungsten trioxide does not melt during the test, but tin melts. Therefore, after the sulfur in the sample of Example 10 is released, it needs to pass through the molten tin layer to be released into the gas, which increases the resistance to sulfur release. Tungsten trioxide has a porous structure, which is conducive to the release of sulfur. Therefore, the test time of Example 10 is also longer. During the test, a slight tailing phenomenon was observed in Example 10, and the test result was slightly higher.
[0067] Comparing Example 8 with Example 10, the test time is shorter than that of Example 10, and no tailing phenomenon occurs. This is probably because the covering tin layer is thinner, and the sulfur in the sample can be quickly released into the gas through the molten tin layer after being released, so the test time does not become longer.
[0068] Example 11: Nickel padding on the bottom + tungsten trioxide covering on the top The instrument was calibrated and the blank value was measured according to the method and steps of Example 7, and then the sulfur content in sulfonated polyetheretherketone SP1 was detected, wherein the amount of nickel powder used as the bottom release promoter was 51-52 mg, and the amount of tungsten trioxide used in the top layer was 9.1-9.2 times that of SP1. The average value of 3 tests was 0.226%, the RSD was 1.99%, and the average test time was 92 s.
[0069] Comparing the test spectra of Example 11 with Example 4 and Comparative Example 1, we can obtain Figure 7The test time of Example 11 is the shortest, and the sulfur starts to be released slower than that of Comparative Example 1, but faster than that of Example 4. This is because tungsten trioxide has a porous structure and does not melt, which can reduce the resistance of sulfur being released into the mixed gas. Therefore, sulfur in Example 11 is released faster than that in Example 4, and the test time is shortened.
[0070] Example 12: Tungsten trioxide padding on the bottom + tungsten trioxide covering on the top According to the method and steps of Example 7, the instrument was calibrated and the blank value was measured, and then the sulfur content in the sample was detected. The integral end time was set to 70-300s. First, 50-53mg of tungsten trioxide was weighed and spread on the bottom of the porcelain boat crucible, and then 54-59mg of sulfonated polyetheretherketone SP1 (accurate to 0.01mg) was weighed and spread on the upper layer of tungsten trioxide (the second release promoter), and then a certain amount of tungsten trioxide was weighed to cover the sample, and the amount was 7.0-7.1 times that of SP1, and then the sample was pushed into the combustion zone of the resistance furnace for testing according to the equipment manual. The average value of the three tests was 0.225%, the RSD was 1.61%, and the average test time was 83s.
[0071] Comparative Example 2 The instrument was calibrated and the blank value was measured according to the method and steps of Example 12, and then the sulfur content in sulfonated polyetheretherketone SP1 was detected without adding a release promoter. The average value of 3 tests was 0.209%, the RSD was 3.67%, and the average test time was 98 seconds.
[0072] Comparing the tests of Example 7, Example 12, Example 5 and Comparative Example 2, the test time of Example 7 and Example 12 is basically the same, and their test results are basically consistent with the test result of Example 5. The test result of Comparative Example 2 is low, and the test time is obviously longer. This is because the release of S is relatively slow, which causes the system to judge that the test is over, but in fact the test is not over, so the test result is low. This shows that adding tungsten trioxide release promoter can accelerate sulfur release and avoid integral inaccuracy.
[0073] Example 13: Silicon dioxide on the bottom and tungsten trioxide on the top The instrument was calibrated and the blank value was measured according to the method and steps of Example 12, and then the sulfur content in sulfonated polyetheretherketone SP1 was detected, wherein the amount of silica as the bottom release promoter was 56-57 mg, and the amount of tungsten trioxide in the top layer was 7.0-7.1 times that of SP1. The average value of 3 tests was 0.222%, the RSD was 2.38%, and the average test time was 81 s.
[0074] Comparing the test spectra of Example 13 with those of Comparative Example 1, we obtain Figure 8The test time of Example 13 is significantly shorter, and the initial release of sulfur is slower than that of Comparative Example 1, but the subsequent spectral intensity of S increases significantly, indicating that the release promoter can promote the release of sulfur.
[0075] Example 14: Silicon dioxide on the bottom and tungsten trioxide on the top The temperature of the resistance furnace is stable at 1280℃~1320℃, the integral end time is set to 40s~300s, and the O2 flow rate is 180L / h. The single-point calibration method is adopted. The sulfur content in the coal standard is 0.76%, and the mass number is 40~53mg (accurate to 0.01mg when weighing and recording). The standard with a sulfur content of 1.46% is used for verification and calibration, and its mass number is 21~28mg (accurate to 0.01mg when weighing and recording). After the blank value is determined, 26~27mg of silicon dioxide is first weighed and spread on the bottom of the porcelain boat crucible, and then 29~39mg of sulfonated polyetheretherketone SP2 is weighed (accurate to 0.01mg) and spread on the upper layer of silicon dioxide, and then a certain amount of tungsten trioxide is weighed to cover the sample, and the amount is 4.0~4.1 times that of SP2, and then the sample is pushed into the combustion zone of the resistance furnace for testing according to the equipment manual. In the four tests, 29.73 mg, 29.15 mg, 31.14 mg and 38.56 mg of sulfonated polyetheretherketone SP2 were weighed respectively. The sulfur content test results were 1.06%, 1.08%, 1.01% and 1.03% respectively. The average value was 1.05%, the RSD was 2.57%, and the average test time was 44 s.
[0076] Example 15: Tin padding on the bottom + tungsten trioxide covering on the top The sulfur content in sulfonated polyetheretherketone SP3 was detected according to the method and steps of Example 14, wherein when the instrument was calibrated at a single point, the sulfur content in the coal standard was 0.28%, and the mass number was 90-120 mg (accurate to 0.01 mg), and the standard with a sulfur content of 0.41% was used for verification and calibration, and its mass number was 21-30 mg (accurate to 0.01 mg). The amount of tin powder used as the bottom release promoter was 31-32 mg, and the amount of tungsten trioxide used in the top layer was 1.1-1.2 times that of SP3. During the 4 tests, sulfonated polyetheretherketone SP3 was weighed as 403.42 mg, 356.33 mg, 432.42 mg, and 501.73 mg, respectively. The sulfur content test results were 0.067%, 0.070%, 0.075%, and 0.066%, respectively, with an average value of 0.069%, an RSD of 3.34%, and an average test time of 88 s.
[0077] Example 16: Nickel padding on the bottom + tungsten trioxide covering on the top After calibrating the instrument and measuring the blank value according to the method in Example 1, the sulfur content in sulfonated polyetheretherketone SP4 was detected according to the method and steps in Example 14, wherein the amount of nickel powder used as the bottom release promoter was 21-22 mg, and the amount of tungsten trioxide used in the top layer was 2.5-2.5 times that of SP4. During the 4 tests, 29.05 mg, 30.52 mg, 45.17 mg, and 38.22 mg of sulfonated polyetheretherketone SP4 were weighed respectively, and the sulfur content test results were 0.471%, 0.462%, 0.459%, and 0.473%, respectively, with an average value of 0.466%, an RSD of 1.46%, and an average test time of 53 s.
[0078] Example 17: Silicon dioxide on the bottom and tungsten trioxide on the top The sulfur content in sulfonated polyetheretherketone SP5 was detected according to the method and steps of Example 14, wherein during single-point calibration, the sulfur content in the coal standard was 0.18%, and the mass number was 61-69 mg (accurate to 0.01 mg), and the standard with a sulfur content of 0.28% was used for verification and calibration, and its mass number was 39-44 mg (accurate to 0.01 mg). The amount of silica as the bottom release promoter was 21-22 mg, and the amount of tungsten trioxide in the top layer was 2.1-2.2 times that of SP5. When sulfonated polyetheretherketone SP5 was weighed as 98.92 mg, 98.10 mg, 100.26 mg, and 88.73 mg in 4 tests, the sulfur content test results were 0.130%, 0.123%, 0.125%, and 0.122%, respectively, with an average value of 0.125%, an RSD of 2.84%, and an average test time of 52 s.
[0079] Example 18: Covered with silicon dioxide The temperature of the resistance furnace is stable at 1280℃~1320℃, the integral end time is set to 40s~300s, and the O2 flow rate is 180L / h. The instrument is calibrated by multi-point calibration method. The sulfur content in the coal standard is 0.28%, 0.76%, and 1.46%, and the mass number is 90~100mg (accurate to 0.01mg). The standard with a sulfur content of 0.41% is used for verification and calibration, and its mass number is 90~100mg (accurate to 0.01mg). After the blank value test, 90~100mg (accurate to 0.01mg) of sulfonated polyetheretherketone SP6 is weighed and spread in a porcelain boat crucible, and then the release promoter silica is covered on the sample. The amount of silica is 1.5~1.6 times that of SP6, and then the sample is pushed into the combustion zone of the resistance furnace for testing according to the equipment manual. The test results are directly calculated by the software. During the four tests, 95.72 mg, 99.38 mg, 92.33 mg and 91.59 mg of sulfonated polyetheretherketone SP6 were weighed respectively. The sulfur content test results were 0.618%, 0.616%, 0.625% and 0.622% respectively. The average value was 0.620%, the RSD was 0.65%, and the average test time was 58 s.
[0080] Example 19: Covered with silicon dioxide The temperature of the resistance furnace is stable at 1280~1320℃, the integral end time is set to 40s~300s, and the O2 flow rate is 180L / h. The instrument is calibrated by the single-point calibration method. The sulfur content in the coal standard is 0.18%, and the mass number is 280~290mg (accurate to 0.01mg). The standard with a sulfur content of 0.28% is used for verification and calibration, and its mass number is 180~190mg (accurate to 0.01mg). After the blank value test, 280~300mg (accurate to 0.01mg) of sulfonated polyetheretherketone SP7 is weighed and spread in a porcelain boat crucible, and then the release promoter silica is covered on the sample. The amount of silica is 1.0~1.1 times that of SP7, and then the sample is pushed into the combustion zone of the resistance furnace for testing according to the equipment manual. The test results are directly calculated by the software. During the three tests, 283.61 mg, 290.95 mg and 292.84 mg of sulfonated polyetheretherketone SP7 were weighed respectively. The sulfur content test results were 0.192%, 0.197% and 0.194% respectively. The average value was 0.194%, the RSD was 1.29%, and the average test time was 50 s.
[0081] Example 20: Tin padding on the bottom + tungsten trioxide covering on the top The sulfur content in sulfonated polyetheretherketone SP8 was detected according to the method and steps of Example 14, wherein during single-point calibration, the sulfur content in the coal standard was 0.18%, and the mass number was 55-70 mg (accurate to 0.01 mg), and the standard with a sulfur content of 0.28% was used for verification and calibration, and its mass number was 40-45 mg (accurate to 0.01 mg). The amount of tin powder used as the bottom release promoter was 31-32 mg, and the amount of tungsten trioxide used in the top layer was 1.1-1.2 times that of SP8. During the 4 tests, sulfonated polyetheretherketone SP8 was weighed as 812.36 mg, 857.99 mg, 900.54 mg, and 985.30 mg, respectively. The sulfur content test results were 0.0131%, 0.0129%, 0.0125%, and 0.0135%, respectively, with an average value of 0.0128%, an RSD of 2.38%, and an average test time of 88 s.
[0082] Example 21: Tungsten trioxide is laid on the bottom and silicon dioxide is covered on the top The temperature of the resistance furnace is stable at 1280℃~1320℃, the integral end time is set to 120s~300s, and the O2 flow rate is 180L / h. The instrument is calibrated by the single-point calibration method. The sulfur content in the coal standard is 0.18%, and the mass number is 110~123mg (accurate to 0.01mg). The standard with a sulfur content of 0.28% is used for verification and calibration, and its mass number is 80~90mg (accurate to 0.01mg). The amount of tungsten trioxide used as the bottom release promoter is 30~32mg, and the amount of silica used in the top layer is 1.0~1.1 times that of sulfonated polyetheretherketone SP9. Sample testing is carried out after the blank value test. In the four tests, sulfonated polyetheretherketone SP9 was weighed as 180.53 mg, 184.12 mg, 175.19 mg and 156.32 mg respectively. The sulfur content test results were 0.121%, 0.120%, 0.125% and 0.118% respectively. The average value was 0.121%, the RSD was 2.98%, and the average test time was 120 s.
[0083] Comparative Example 3: High-frequency induction furnace test: Tungsten iron additives are laid on the sample The operating power is 100%, the power duration is 100s, the integral end time is 100s~200s, and the O2 flow rate is 180L / h. The instrument is calibrated by the single-point calibration method. The sulfur content in the steel standard material is 0.127%, and the mass number is 110~120mg (accurate to 0.01mg). The standard material with a sulfur content of 0.097% is used for verification and calibration (the standard material is covered with 0.60g iron and 2.00g tungsten particles during the test), and its mass number is 140~150mg (accurate to 0.01mg). After the blank value test, 100~160mg of sulfonated polyetheretherketone SP9 is weighed in a crucible, and then 0.60g iron and 2.00g tungsten particles are weighed to cover the surface of the sample, and then the sample is pushed into the high-frequency induction furnace for combustion according to the equipment manual for testing. The test results are directly calculated by the software. During the four tests, 152.95 mg, 119.76 mg, 100.61 mg and 105.81 mg of sulfonated polyetheretherketone SP9 were weighed respectively. The sulfur content test results were 0.0096%, 0.0208%, 0.0124% and 0.0121% respectively. The average value was 0.0114%, the RSD was 13.52%, and the average test time was 100 s.
[0084] Compare Example 21 with Comparative Example 3. Fig. 9 The test of comparative example 3 is unstable, and the test result is obviously low. The crucible after the sulfonated polyetheretherketone SP9 test in comparative example 3, the crucible after the steel standard test in comparative example 3, and the crucible tested by sulfonated polyetheretherketone SP9 in Example 21 are compared. Fig.10 , a is the porcelain boat crucible after the test of Example 21; c is the crucible of Comparative Example 3 after the instrument was calibrated with steel standards; b is the crucible of Comparative Example 3 after the test was completed. Fig.10 It can be seen that the crucible of Example 21 (the powders in the crucible in the figure are tungsten trioxide and silicon dioxide; if the sulfonated polyetheretherketone is tested without adding a release promoter, the crucible after the test is very clean and free of any powder) and the crucible wall of Comparative Example 3 after the steel standard test are basically kept clean, and the samples are completely burned or melted, while the surface of the crucible wall of Comparative Example 3 sulfonated polyetheretherketone SP9 after the test is covered with gray powder, which is the sulfonated polyetheretherketone SP9 that is not completely burned. This shows that when using a high-frequency induction furnace for testing, the powder is easily blown everywhere by the carrier gas, making it difficult for the sample to fully burn (remaining on the crucible wall and the combustion chamber, etc.), resulting in large fluctuations in the sulfur content analysis data. In particular, for samples with low sulfur content, the amount of powder required for the test is relatively large, which is more likely to cause incomplete combustion of the powder, resulting in a large test error.
[0085] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0086] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.
Claims
1. A method for determining the sulfur content in sulfonated polyetheretherketone, comprising the steps of spreading the sample in a porcelain boat crucible, pushing the sample into a carbon-sulfur analyzer with a resistance furnace, and detecting the sulfur content by infrared absorption method, characterized in that: In the porcelain boat crucible, the upper surface of the sample is covered with a first release promoter powder, the sulfur content in the first release promoter is less than 0.0005%, and the first release promoter is selected from tungsten trioxide, calcium oxide, silicon dioxide, tin, nickel or iron.
2. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 1, characterized in that: The mass of the first release-promoting agent is equivalent to 1.0 to 9.2 times the mass of the sample.
3. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 2, characterized in that: When the melting point of the first release accelerator is lower than or equal to the temperature of the resistance furnace, the mass of the first release accelerator is equivalent to 2.3 to 3.2 times the mass of the sample.
4. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 1, characterized in that: In the porcelain boat crucible, the lower surface of the sample is padded with second release promoter powder, the sulfur content in the second release promoter is less than 0.0005%, and the second release promoter is selected from tungsten trioxide, calcium oxide, silicon dioxide, tin, nickel or iron.
5. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 4, characterized in that: The mass of the second release-promoting agent is equivalent to 0.1 to 1.6 times the mass of the sample.
6. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 4, characterized in that: The fineness of the second release-promoting agent powder is 200-300 meshes.
7. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 1, characterized in that: The fineness of the first release-promoting agent powder is 200-300 meshes.
8. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 1, characterized in that: The temperature of the resistance furnace is stabilized at 1280°C to 1320°C, and the O2 carrying capacity is 180L / h.
9. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 8, characterized in that: The end point time of spectrum curve integration is 40s~300s.
10. The method for determining the sulfur content in sulfonated polyetheretherketone according to claim 1, characterized in that: The carbon-sulfur analyzer is calibrated with a standard substance, and a numerical relationship between the infrared spectrum intensity value and the sulfur content of the standard substance is established; the standard substance is a coal standard.
Citation Information
Patent Citations
Method for determining contents of carbon and sulfur in iron-containing dust mud
CN104483286A
Method for measuring contents of carbon and sulfur in thorium tetrafluoride
CN106932356A
Determination method and device of low sulfur content
CN108717058A
Method for detecting sulfur and carbon in steel
CN112326584A
Preparation method of sulfonated polyetheretherketone, sulfonated polyetheretherketone membrane and application
CN115260422A