Co-assembled nano-array surface enhanced Raman scattering substrate as well as preparation method and application thereof

Through the co-assembly and pH adjustment of gold nanoparticles at different scales, the problem of poor detection performance of self-assembled nanoarrays enhanced Raman scattering substrates is solved, and the high sensitivity detection of malachite green is realized, providing a fast and simple field detection. method.

CN119086523AActive Publication Date: 2024-12-06OCEAN UNIV OF CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411210773.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

Smart Images

  • Figure CN119086523A_ABST
    Figure CN119086523A_ABST
Patent Text Reader

Abstract

The invention discloses a co-assembled nano-array surface enhanced Raman scattering substrate, and relates to the technical field of biological detection.The co-assembled nano-array surface enhanced Raman scattering substrate is characterized in that first nano-gold particles are assembled to gaps of a second nano-gold particle array, so that the hot spot and sensitivity of the surface enhanced Raman scattering substrate are improved; and transferring the gold film onto a substrate to obtain the gold film. The particle size of the first gold nanoparticles ranges from 20 nm to 35 nm. The particle size of the second nano gold particles ranges from 150 nm to 200 nm. According to the surface enhanced Raman scattering substrate and the preparation method thereof disclosed by the invention, the two kinds of gold nanoparticles with obvious particle size difference are co-assembled to obtain more surface enhanced Raman scattering hot spots, so that the sensitivity of the co-assembled nano array surface enhanced Raman scattering substrate and the adsorption of malachite green on the surface of the co-assembled nano array surface enhanced Raman scattering substrate are improved; the higher-sensitivity surface enhanced Raman scattering detection of the malachite green is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biological detection technology, and in particular to a co-assembled nanoarray surface enhanced Raman scattering substrate, a preparation method and an application thereof. Background Art

[0002] Aquatic products are one of the important sources of high-protein food in the human diet, but they are susceptible to harmful microorganisms and thus infected with diseases. They need to be treated with fungicides to reduce economic losses and increase the output of aquatic products. Malachite green is a commonly used fungicide with the advantages of high efficiency and low cost. However, long-term intake of malachite green and its metabolites can cause serious harm to human health, including teratogenicity, carcinogenicity, mutagenicity, immunotoxicity, reproductive toxicity, etc. Therefore, malachite green has been banned by many countries and regions, but due to its low cost, unscrupulous vendors still illegally add malachite green to aquatic products, bringing potential health risks to consumers.

[0003] Malachite green is referred to as MG. Common analytical techniques for its detection include high performance liquid chromatography, spray mass spectrometry, LC-tandem mass spectrometry, enzyme-linked immunosorbent assay and colloidal gold immunochromatography. However, traditional analytical techniques based on chromatography and mass spectrometry have the disadvantages of high cost, complex operation and inability to achieve rapid on-site detection. The test performance of enzyme-linked immunosorbent assay and colloidal gold immunochromatography depends on antibodies, and the detection sensitivity is often poor and the cost is high.

[0004] Surface-enhanced Raman scattering is a fingerprint vibrational spectrum with the advantages of high sensitivity, fast detection speed, and label-free detection. It has shown great potential in various fields such as analytical chemistry, food science, and biology. The surface-enhanced Raman scattering method relies on the strong local electric field generated by plasma metal nanoparticles under laser excitation, which can amplify the Raman signal of the analyte by many orders of magnitude. If the plasma metal nanoparticles are close enough to each other, that is, a few nanometers apart, hot spots will be generated between the nanoparticles, which can further amplify the surface-enhanced Raman scattering signal. The surface-enhanced Raman scattering substrate construction methods include liquid-liquid interface self-assembly method, flexible substrate method, solid substrate method, liquid substrate method, etc. Compared with other assembly methods, liquid-liquid interface self-assembly has the advantages of precisely controlling the morphology, lateral spacing and uniformity of nanoparticles, and can form large-area nanoarrays. It has been used to construct a variety of surface-enhanced Raman scattering substrates for rapid detection of drug residues.

[0005] Although there have been studies using nanoparticles of different morphologies to construct self-assembled nanoarray surface-enhanced Raman scattering substrates, the self-assembled nanoarray surface-enhanced Raman scattering substrates mainly use single-scale nanoparticles for self-assembly in the detection of malachite green, so that the obtained self-assembled nanoarray surface-enhanced Raman scattering substrates have more gaps and unassembled areas, resulting in poor detection performance of the prepared self-assembled nanoarray surface-enhanced Raman scattering substrates, and more ligands remain on the surface of the self-assembled nanoarray surface-enhanced Raman scattering substrates, and the Raman background signal is high, which is not conducive to the adsorption of malachite green on the surface of the substrate, resulting in poor detection sensitivity of malachite green.

[0006] Therefore, it is necessary to prepare a surface enhanced Raman scattering substrate with good detection performance and high detection sensitivity. Summary of the invention

[0007] In order to solve the problem that a self-assembled nanoarray surface-enhanced Raman scattering substrate obtained by using single-scale nanoparticles in the prior art has a large number of gaps and unassembled areas, and thus has poor detection performance and high Raman background signals during the detection of malachite, the present invention provides a co-assembled nanoarray surface-enhanced Raman scattering substrate and a preparation method and application thereof.

[0008] The present invention uses gold nanoparticles of different particle sizes for liquid-liquid interface self-assembly, and through the co-assembly of two nanogolds with significant particle size differences, the nanogold with small particle size is assembled into the gap of the nanogold array with large particle size, thereby obtaining more surface enhanced Raman scattering hotspot areas, further improving the sensitivity of the co-assembled nanoarray surface enhanced Raman scattering substrate, and by adjusting the pH of the malachite green test liquid, promoting the adsorption of malachite green on the surface of the co-assembled nanoarray surface enhanced Raman scattering substrate, achieving more sensitive malachite green surface enhanced Raman scattering detection, and providing a reliable means for rapid detection of aquatic product quality and safety. The present invention effectively solves the defects of the preparation of the existing self-assembled nanoarray surface enhanced Raman scattering substrate and the detection of malachite green.

[0009] To achieve the above objectives, the specific technical solutions of the present invention are as follows.

[0010] The first aspect of the present invention provides a method for preparing a co-assembled nanoarray surface enhanced Raman scattering substrate, wherein the co-assembled nanoarray surface enhanced Raman scattering substrate is the co-assembled nanoarray surface enhanced Raman scattering substrate provided by the first aspect of the present invention, comprising the following steps:

[0011] Sodium citrate solution and chloroauric acid solution are added into water to carry out reduction reaction, thereby obtaining nano-gold solution No. 1;

[0012] A gold seed solution, a sodium citrate solution, a hydroxylamine hydrochloride solution and a chloroauric acid solution are mixed to obtain an intermediate, and the intermediate is mixed with a reducing agent and a chloroauric acid solution to obtain a No. 2 nanogold solution; since the particle size of the No. 2 nanogold particles is relatively large, it is necessary to first use the gold seed solution to obtain the intermediate during the preparation process, and then prepare the No. 2 nanogold particles through the intermediate.

[0013] A No. 1 nanogold solution and a No. 2 nanogold solution are co-assembled in a water-organic solvent system, so that the No. 1 nanogold particle group is assembled into the gaps of the No. 2 nanogold particle array to obtain a gold film, and the gold film is arranged on a substrate to obtain a co-assembled nanoarray surface enhanced Raman scattering substrate; the substrate is a silicon wafer.

[0014] The particle size of the No. 1 nano-gold particles is 20nm to 35nm;

[0015] The particle size of the No. 2 nano-gold particles is 150nm to 200nm.

[0016] The present invention obtains gold nanoparticles of different particle sizes by using the prepared No. 1 nanogold solution and No. 2 nanogold solution, and then performs liquid-liquid interface self-assembly on the gold nanoparticles of different particle sizes, and assembles the nanogold of small particle size into the gap of the nanogold array of large particle size by co-assembly of two nanogolds with significant particle size differences, thereby obtaining more surface enhanced Raman scattering hotspot areas, and improving the sensitivity and detection performance of the surface enhanced Raman scattering substrate of the co-assembled nanoarray. Wherein, the Raman enhancement effect of the co-assembled substrate will be weakened if the particle size difference of the two nanogold particles is small or large. Therefore, the present invention makes the co-assembled substrate enhancement effect better by controlling the particle size of the two nanogolds.

[0017] In another preferred embodiment, the mass percentage concentration of the sodium citrate solution is 0.8% to 1.2%, and the mass percentage concentration of the chloroauric acid solution is 0.8% to 1.2%.

[0018] In another preferred embodiment, during the preparation of nanogold No. 1, the volume ratio of the sodium citrate solution, the chloroauric acid solution and water is 9-11:1:90-110.

[0019] In another preferred embodiment, the specific preparation process of the gold seed solution is as follows:

[0020] Sodium citrate solution and chloroauric acid solution are added into water and mixed and stirred to obtain a gold seed solution; the volume ratio of the sodium citrate solution, chloroauric acid solution and water is 1.15-1.17:1:100-102.

[0021] In another preferred embodiment, in the process of preparing the No. 2 nanogold solution, the reducing agent is a hydroxylamine hydrochloride solution, and the concentration of the hydroxylamine hydrochloride solution is 0.005 mol / L to 0.015 mol / L;

[0022] The volume ratio of the gold seed solution, the hydroxylamine hydrochloride solution, the chloroauric acid solution and the sodium citrate solution is 30-35:10-20:1:2.

[0023] In another preferred embodiment, the volume ratio of the No. 1 nanogold solution to the No. 2 nanogold solution is 50-500:500.

[0024] In another preferred embodiment, in the water-organic solvent system, the organic solvent is dichloromethane and n-hexane;

[0025] In the water-organic solvent system, the volume ratio of dichloromethane, n-hexane and water is 2:1:0.8-1.1.

[0026] The second aspect of the present invention provides a co-assembled nanoarray surface enhanced Raman scattering substrate, which is prepared by the preparation method of the co-assembled nanoarray surface enhanced Raman scattering substrate provided by the first aspect of the present invention.

[0027] The co-assembled nanoarray surface enhanced Raman scattering substrate is composed of No. 1 nanogold particles in No. 1 nanogold solution, assembled into the gap of No. 2 nanogold particle array in No. 2 nanogold solution, so as to improve the hot spots and sensitivity of the surface enhanced Raman scattering substrate, obtain a gold film, and configure the gold film on the substrate to obtain. The difference in the particle size of the two nanogold particles is small, which may weaken the Raman enhancement effect of the co-assembled substrate. If the difference is too large, the Raman enhancement effect of the co-assembled substrate may also be weakened. Therefore, the present invention makes the co-assembled substrate enhancement effect better by controlling the particle size of the two nanogolds.

[0028] The third aspect of the present invention provides a method for detecting malachite green, comprising soaking the co-assembled nanoarray surface enhanced Raman scattering substrate provided by the first aspect of the present invention for 28 to 32 minutes, taking it out, drying it, and then detecting the surface enhanced Raman scattering signal to obtain the Raman intensity of the malachite green solution to be detected;

[0029] The Raman intensity of the malachite green solution to be detected is substituted into the standard curve of malachite green solution concentration-Raman intensity to obtain the concentration of the malachite green solution to be detected.

[0030] The standard curve of malachite green solution concentration-Raman intensity is obtained by the following method:

[0031] Accurately weigh the malachite green standard and prepare a solution with a concentration of 1000 ppm. Use 1 mol / L HCl to adjust the pH to 4.0 and dilute the concentration to 10 -6 ppb~100ppb, and obtain malachite green solutions of different concentrations. Take 500μL of malachite green solutions of different concentrations, soak the co-assembled nanoarray surface enhanced Raman scattering substrate in malachite green solutions of different concentrations, take them out and dry them after 30 minutes, aim the Raman probe at the surface of the co-assembled nanoarray surface enhanced Raman scattering substrate, and collect Raman intensity; according to the collected Raman intensity and the corresponding malachite green solution concentration, obtain the malachite green solution concentration-Raman intensity standard curve.

[0032] In another preferred embodiment, the pH value of the malachite green solution to be detected is 3-5.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The present invention utilizes two types of nanogold with significant differences in particle size to co-assemble simultaneously, so that the small-sized nanogold particles No. 1 are assembled into the gaps of the large-sized nanogold particles No. 2 array, thereby obtaining more surface-enhanced Raman scattering hotspots, effectively improving the sensitivity of the co-assembled nanoarray surface-enhanced Raman scattering substrate. The method is easy to operate, does not require the use of complex and expensive equipment, and can achieve high-throughput preparation of large quantities of high-performance surface-enhanced Raman scattering substrates. The prepared co-assembled nanoarray surface-enhanced Raman scattering substrate has a higher sensitivity than the existing self-assembled nanoarray surface-enhanced Raman scattering substrate.

[0035] (2) The detection method of the present invention effectively improves the adsorption of malachite green on the surface of the co-assembled nanoarray surface-enhanced Raman scattering substrate, and realizes surface-enhanced Raman scattering detection of malachite green with higher sensitivity. Compared with the traditional malachite green detection method based on chromatography and mass spectrometry technology, the detection speed of the present invention is faster and easier to operate, and rapid on-site detection can be achieved by hand-held. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The Raman spectra of malachite green solutions of different concentrations detected by the co-assembled nanoarray surface enhanced Raman scattering substrate in Example 1 of the present invention are shown in Figure 1. A is the Raman spectra of malachite green solutions with a concentration of 100 ppb to 0.000001 ppb detected by the co-assembled nanoarray surface enhanced Raman scattering substrate at a pH of 4.0; B is the Raman spectra of malachite green solutions with a concentration of 1 ppb to 0.000001 ppb detected by the co-assembled nanoarray surface enhanced Raman scattering substrate at a pH of 4.0; C is 1609 cm -1The linear relationship between the signal intensity of surface enhanced Raman scattering at 1170 cm and the concentration of malachite green solution; D is 1170 cm -1 The linear relationship between the signal intensity of surface enhanced Raman scattering and the concentration of malachite green solution.

[0037] Figure 2 These are Raman spectra of malachite green powder, 0.1 ppb malachite green sea bass spiked sample and 0.1 ppb malachite green solution in the embodiments of the present invention.

[0038] Figure 3 The figures are electron microscope images of different Raman scattering substrates in the embodiments of the present invention; wherein A is an electron microscope image of a single-scale Raman scattering substrate of a self-assembled array of a No. 2 nanogold solution; B is an electron microscope image of a single-scale Raman scattering substrate of a self-assembled array of a No. 1 nanogold solution; C is an electron microscope image of a co-assembly of a No. 2 nanogold solution and 200 μL of a No. 1 nanogold solution; and D is an electron microscope image of a co-assembly of a No. 2 nanogold solution and 100 μL of a No. 1 nanogold solution.

[0039] Figure 4 Figures are Raman spectra and signal enhancement ratio diagrams of different Raman scattering substrates in the embodiments of the present invention; A is a Raman spectrum diagram of 4-mercaptobenzoic acid after incubation with different Raman scattering substrates; B is a Raman spectrum diagram of 4-mercaptobenzoic acid incubated with 0μL, 50μL, 100μL, 200μL, 300μL, 400μL, and 500μL of No. 1 nanogold solution co-assembled with a surface enhanced Raman scattering substrate; C is a signal enhancement ratio diagram of 4-mercaptobenzoic acid incubated with a surface enhanced Raman scattering substrate co-assembled with 0μL, 50μL, 100μL, 200μL, 300μL, 400μL, and 500μL of No. 1 nanogold solution.

[0040] Figure 5 In the embodiment of the present invention, the No. 1 nano-gold solution and the No. 2 nano-gold solution are co-assembled on the substrate and incubated with 4-mercaptobenzoic acid at 1072 cm -1 The Raman signal changes with the storage time.

[0041] Figure 6 The co-assembled surface enhanced Raman scattering substrate in the embodiment of the present invention was incubated with malachite green at different pH values ​​at 1609 cm -1 Raman signal enhancement ratio diagram. DETAILED DESCRIPTION

[0042] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0043] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.

[0044] The handheld Raman spectrometer detector model in the following embodiments is RMS1000 produced by Ruhai Optoelectronics.

[0045] Example 1

[0046] A method for preparing a co-assembled nanoarray surface enhanced Raman scattering substrate comprises the following steps:

[0047] S1. Measure 62.5 mL of ultrapure water into a conical flask, heat and boil it at 280°C on a magnetic stirrer, then add 625 μL of 1% chloroauric acid solution, mix well, add 6.25 mL of 1% sodium citrate solution, and react at 280°C for 25 minutes. After cooling to room temperature, store it in a refrigerator at 4°C to obtain No. 1 nanogold solution, i.e., small-sized nanogold particles for co-assembly. The particle size of No. 1 nanogold particles is about 30 nm.

[0048] S2. Measure 60 mL of ultrapure water into a conical flask, place it on a magnetic stirrer and heat it to boil at 280°C, then add 600 μL of 1% chloroauric acid solution, mix well, add 700 μL of 1% sodium citrate solution, react at 280°C for 30 minutes, and after cooling to room temperature, store it in a refrigerator at 4°C to obtain a gold seed solution.

[0049] S3. Take 2 mL of gold seed solution and mix it with 5 mL of ultrapure water, then add 840 μL of 0.01 mol / L hydroxylamine hydrochloride solution, then add 60 μL of 1% chloroauric acid solution and 100 μL of 1% sodium citrate solution, stir for 30 min at room temperature to obtain an intermediate, then take 800 μL of the intermediate and mix it with 5 mL of ultrapure water, then add 1200 μL of 0.01 mol / L hydroxylamine hydrochloride solution, 120 μL of 1% chloroauric acid solution and 100 μL of 1% sodium citrate solution, finally stir for 30 min at room temperature to obtain No. 2 nanogold solution, i.e., large-size nanogold particles for co-assembly, and the particle size of No. 2 nanogold particles is about 190 nm.

[0050] S4. Wash the No. 1 nanogold solution and the No. 2 nanogold solution, remove the unreacted reducing agent, and then concentrate. The specific method is as follows: take 10mL of the No. 1 nanogold solution and the No. 2 nanogold solution in a centrifuge tube, add 1mL, 0.1% SDS solution and 1mL, 0.01% Twen20 solution, and mix thoroughly; centrifuge at 9000rpm for 10min, and discard the supernatant; first add 1mL, 1% PVP solution to the centrifuge tube, mix well, and then add 10mL ultrapure water; after mixing again, add 1mL, 0.1% SDS solution and 1mL, 0.01% Twen20 solution; centrifuge at 9000rpm for 10min, and discard the supernatant; redissolve the precipitate in 1mL of anhydrous ethanol to complete the washing and concentration.

[0051] Take 500 μL of the washed and concentrated No. 2 nanogold solution and mix it with 100 μL of the No. 1 nanogold solution, then add 2 mL of dichloromethane, 1 mL of ultrapure water and 1 mL of n-hexane in sequence, mix them evenly to achieve the co-assembly of gold nanoparticles of different sizes, and after the organic phase evaporates, transfer the assembled gold film to a silicon wafer and dry it at room temperature to obtain a co-assembled nanoarray surface enhanced Raman scattering substrate.

[0052] Example 2

[0053] A method for preparing a co-assembled nanoarray surface enhanced Raman scattering substrate. Compared with the method for preparing a co-assembled nanoarray surface enhanced Raman scattering substrate in Example 1, this embodiment only changes the amount of the added nanogold solution No. 1, and the remaining steps are the same. The specific operations are as follows:

[0054] Take 500 μL of the washed No. 2 nanogold solution and mix them with 0 μL, 50 μL, 100 μL, 200 μL, 300 μL, 400 μL, and 500 μL of No. 1 nanogold solution, respectively, and then perform co-assembly. Soak the prepared surface enhanced Raman scattering substrate in 500 μL, 100 μL, 200 μL, 300 μL, 400 μL, and 500 μL of the No. 1 nanogold solution, respectively. -4 The samples were incubated in 4-mercaptobenzoic acid for 30 min, taken out, dried, and then the surface enhanced Raman scattering signal was detected. Figure 4 As shown in the figure, when the addition amount of No. 1 nanogold solution was 50μL and 100μL, the Raman signal of the co-assembled surface enhanced Raman scattering substrate gradually increased. When the addition amount was 100μL, 200μL, 300μL, 400μL, and 500μL, as the addition amount of No. 1 nanogold solution gradually increased, the Raman signal of the co-assembled surface enhanced Raman scattering substrate showed a downward trend. Through significance analysis, the co-assembled surface enhanced Raman scattering substrate with the addition amount of No. 1 nanogold solution of 100μL had the best enhancement effect, and its enhancement ratio reached 228.38%±4.86% relative to the absence of No. 1 nanogold solution.

[0055] In order to illustrate the detection effect of the co-assembled nanoarray surface-enhanced Raman scattering substrate on malachite green in the present invention, we conducted the following experiment.

[0056] 1. Establishment of standard curve

[0057] Accurately weigh the malachite green standard and prepare a solution with a concentration of 1000 ppm. Use 1 mol / L HCl to adjust the pH to 4.0 and finally dilute the concentration to 10 -6 ppb~100ppb. Take 500 μL of the above malachite green solutions with different concentration gradients, immerse the co-assembled nanoarray surface enhanced Raman scattering substrate in Example 1 in it, take it out and dry it after 30 minutes, aim the Raman probe of the Raman spectrometer detector at the surface of the co-assembled nanoarray surface enhanced Raman scattering substrate, and collect the Raman intensity.

[0058] With malachite green at 1609cm -1 and 1170cm -1 The Raman intensity at the position is taken as the ordinate, and the concentration of the malachite green solution is taken as the abscissa. A malachite green standard curve is established. The results are shown in Figure 1 As shown. A handheld Raman spectrometer was used to detect the Raman signal, with an excitation wavelength of 785nm, an excitation power of 60mW, and an excitation time of 2s. Figure 1 A and Figure 1 As can be seen in B, in the range of 10 -6 ppb~100ppb, with the increase of malachite green concentration, 1609cm -1 and 1170cm -1 The Raman signal intensity also gradually increased, so the Origin software was used to fit the linear equation and establish a standard curve. The results are as follows: Figure 1 As shown in C, the characteristic peak of malachite green is 1609cm -1 The Raman signal intensity at 10 -6 The concentration range of ppb to 1 ppb shows a good linear relationship, and the linear regression equation is y=2997.23+372.02x, where y is the Raman signal intensity, x is the logarithm of the malachite green concentration, and R 2 The detection limit was 0.85×10 -6 ppb.

[0059] like Figure 1 As shown in D, the characteristic peak of malachite green is 1170cm -1 The Raman signal intensity at 10 -3A good linear relationship is shown in the range of ppb to 5 ppb, and a linear regression equation y=2355.48+550.51x is established, where y is the Raman signal intensity, x is the logarithm of the malachite green concentration, and R 2 The detection limit was 0.13×10 -3 ppb, which is lower than the detection limit of 0.5ppb for malachite green by high performance liquid chromatography in GB / T19857-2005. This shows that this method has extremely high sensitivity for the detection of malachite green, is easy to operate, does not require the use of large instruments and equipment, and can achieve rapid on-site detection.

[0060] 2. Detection effect

[0061] Sea bass was selected as the actual test object. First, the sea bass meat was crushed into fish paste with a crusher. 2g of fish paste was weighed and malachite green solution was added to make the malachite green spiked concentration in the fish meat 0.1ppb. Then 2mL of ultrapure water was added to mix, vortexed for 3min, and allowed to stand for 30min; then 8mL of 0.1% formic acid acetonitrile solution was added, vortexed for 3min, and then ultrasonically extracted for 20min. Then 4g of anhydrous sodium sulfate was added to the above sample, vortexed for 3min, ultrasonicated for 5min, centrifuged at 5000r / min for 5min, and the supernatant was taken and the centrifugation operation was repeated again. The obtained supernatant was placed in a 10mL centrifuge tube and blown to dryness with nitrogen at 50℃. Finally, 1mL of ultrapure water was used for re-dissolution, vortexed for 5min, filtered through a 0.22μm filter membrane, and the pH of the test solution was adjusted to 4.0 to obtain a sea bass extract re-solution.

[0062] The co-assembled nanoarray surface enhanced Raman scattering substrate was immersed in 500 μL sea bass extract solution for 30 min, then taken out and dried and the Raman signal was detected by a handheld Raman spectrometer. The results are as follows: Figure 2 The malachite green content in the actual food samples was analyzed using the standard curve established in 1, with malachite green at 1609cm -1 The quantitative analysis of the characteristic peak at 1170 cm-1 was performed, and the overall recovery of the spiked detection was 89.31% to 101.06%, with a relative standard deviation of 4.10% to 8.83%. -1 The characteristic peaks at the 400 nm were quantitatively analyzed, and the overall recovery rates were between 79.33% and 111.27%, with relative standard deviations between 3.71% and 8.15%.

[0063] 3. Comparison of the surface-enhanced Raman scattering substrate of nanoarrays constructed by co-assembly of gold nanoparticles of different scales and the surface-enhanced Raman scattering substrate of nanoarrays constructed by self-assembly of gold nanoparticles of a single scale

[0064] The scanning electron microscope images of the co-assembled nanoarray surface enhanced Raman scattering substrate in Example 1 and the traditional single-scale nanogold self-assembled nanoarray surface enhanced Raman scattering substrate are as follows: Figure 3 As shown in the figure, compared with the single-scale nano-gold self-assembled nano-array surface-enhanced Raman scattering substrate, the small-sized No. 1 nano-gold particles in the different-scale nano-gold co-assembled nano-array surface-enhanced Raman scattering substrate are filled between the large-sized No. 2 nano-gold particles, thereby forming more surface-enhanced Raman scattering hotspot areas, which can improve the surface-enhanced Raman scattering enhancement signal of the material.

[0065] In this embodiment, 4-mercaptobenzoic acid is used as a surface enhanced Raman scattering detection probe molecule. The surface enhanced Raman scattering substrate is immersed in a 10 -4 M of 4-mercaptobenzoic acid solution for 30 min, and then the enhancement effect of different surface enhanced Raman scattering substrates on the Raman signal of 4-mercaptobenzoic acid was detected, such as Figure 4 As shown. The experimental results show that the Raman signal detected by the nanoarray surface-enhanced Raman scattering substrate co-assembled by the No. 1 nanogold solution and the No. 2 nanogold solution is 1422% ± 6.52% stronger than the surface-enhanced Raman scattering substrate self-assembled by the No. 1 nanogold solution alone, and 52% ± 0.19% stronger than the surface-enhanced Raman scattering substrate self-assembled by the No. 2 nanogold solution alone. It can be seen that the surface-enhanced Raman scattering substrate co-assembled by nanogold of different sizes has more hot spots and can achieve a stronger surface-enhanced Raman scattering enhancement effect.

[0066] 4. Effect of different addition amounts of No. 1 nanogold solution

[0067] Take 500 μL of washed No. 2 nanogold and mix them with 0 μL, 50 μL, 100 μL, 200 μL, 300 μL, 400 μL, and 500 μL of No. 1 nanogold solution, respectively, and then perform co-assembly. Soak the prepared surface enhanced Raman scattering substrate in 500 μL, 100 μL, 200 μL, 300 μL, 400 μL, and 500 μL of the No. 1 nanogold solution, respectively. -4 The samples were incubated in 4-mercaptobenzoic acid for 30 min, taken out, dried, and then the surface enhanced Raman scattering signal was detected. Figure 4 As shown in the figure, when the addition amount of No. 1 nanogold solution is 50μL and 100μL, the Raman signal of the co-assembled surface enhanced Raman scattering substrate gradually increases. When the addition amount is 100μL, 200μL, 300μL, 400μL, and 500μL, as the addition amount of No. 1 nanogold solution gradually increases, the Raman signal of the co-assembled surface enhanced Raman scattering substrate shows a downward trend. Through significance analysis, the co-assembled surface enhanced Raman scattering substrate has the best enhancement effect when the addition amount of No. 1 nanogold solution is 100μL, and its enhancement ratio reaches 228.38%±4.86% relative to the case without adding No. 1 nanogold solution.

[0068] 5. Storage stability evaluation

[0069] The co-assembled nanoarray surface enhanced Raman scattering substrate prepared in Example 1 was -4 The Raman signal of 4-mercaptobenzoic acid on the surface enhanced Raman scattering substrate was tested after drying, and the change of the Raman signal of 4-mercaptobenzoic acid on the surface enhanced Raman scattering substrate was recorded within 18 days of storage. The results are shown in Figure 5 As shown, during the storage period of 18 days, the Raman signal of 4-mercaptobenzoic acid did not decrease significantly, indicating that the co-assembled nanoarray surface-enhanced Raman scattering substrate prepared by the method of the present invention has good storage stability.

[0070] 6. Detection of malachite green at different pH

[0071] The co-assembled nanoarray surface enhanced Raman scattering substrate prepared in Example 1 was used to prepare malachite green solutions of different pH values. The malachite green solutions were adjusted to pH values ​​of 2, 3, 4, 5, 6, 7, 8, 9, and 10 using 1 mol / L hydrochloric acid and 1 mol / L sodium hydroxide. The prepared co-assembled nanoarray surface enhanced Raman scattering substrate was incubated in 500 μL malachite green solutions of different pH values, and the concentrations of malachite green were 10 ppb and 1 ppm, respectively. The co-assembled nanoarray surface enhanced Raman scattering substrate was incubated in malachite green solutions of the same pH and different concentrations, first incubating 10 ppb malachite green and then incubating 1 ppm malachite green solution. Raman spectroscopy was then performed to extract malachite green 1609 cm -1 The intensity of the Raman characteristic peak signal at 1609cm -1 The ratio of the Raman signal intensity of 1ppm malachite green to 10ppb malachite green was used to analyze the effect of different pH on the detection of malachite green. The results are as follows Figure 6 As shown, in the pH range of 3 to 5, the Raman signal enhancement effect of malachite green is better, among which when the pH is 4, the effect of enhancing the Raman signal of the co-assembled nanoarray SERS substrate is optimal.

[0072] The present invention utilizes two kinds of nano-gold particles with significant differences in particle size to co-assemble simultaneously, so that the nano-gold particles of the small particle size are assembled into the gaps of the nano-gold particle array of the large particle size, so that the co-assembled nano-array surface-enhanced Raman scattering substrate has more surface-enhanced Raman scattering hotspot areas compared with a single-scale self-assembled nano-array surface-enhanced Raman scattering substrate, and effectively improves the sensitivity of the co-assembled nano-array surface-enhanced Raman scattering substrate to malachite green detection. The method of the present invention is easy to operate, does not require the use of complex and expensive equipment, can achieve high-throughput preparation of large quantities of high-performance surface-enhanced Raman scattering substrates, and the prepared co-assembled nano-array surface-enhanced Raman scattering substrate has higher sensitivity than the existing self-assembled nano-array surface-enhanced Raman scattering substrate. In addition, the detection method of the present invention effectively improves the adsorption of malachite green drugs on the surface of the co-assembled nanoarray surface-enhanced Raman scattering substrate, and realizes surface-enhanced Raman scattering detection of malachite green with higher sensitivity. Compared with the traditional malachite green detection method based on chromatography and mass spectrometry technology, the detection speed of the present invention is faster and the operation is simpler. The on-site rapid detection of malachite green can be achieved through handheld Raman spectroscopy, and the detection limit is far lower than the limit requirement in the national standard. It can be used to develop malachite green surface-enhanced Raman scattering non-labeling detection related products.

[0073] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the scope of protection of the invention. Obviously, the described embodiments are only some embodiments of the present invention, rather than all embodiments. Based on these embodiments, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field can still combine, add, delete or make other adjustments to the features in the various embodiments of the present invention according to the circumstances without conflict, without making creative work, so as to obtain different other technical solutions that do not deviate from the concept of the present invention in essence, and these technical solutions also belong to the scope of protection of the present invention.

Claims

1. A method for preparing a co-assembled nanoarray surface enhanced Raman scattering substrate, It is characterized in that The following steps are involved: Sodium citrate solution and chloroauric acid solution are added into water to carry out reduction reaction, thereby obtaining nano-gold solution No. 1; Mixing a gold seed solution, a sodium citrate solution, a hydroxylamine hydrochloride solution and a chloroauric acid solution to obtain an intermediate, and mixing the intermediate with a reducing agent and a chloroauric acid solution to obtain a No. 2 nanogold solution; Co-assembling the No. 1 nanogold solution and the No. 2 nanogold solution in a water-organic solvent system, assembling the No. 1 nanogold particles into the gaps of the No. 2 nanogold particle array to obtain a gold film, and configuring the gold film on a substrate to obtain a co-assembled nanoarray surface enhanced Raman scattering substrate; The particle size of the No. 1 nano-gold particles is 20nm to 35nm; The particle size of the No. 2 nano-gold particles is 150nm to 200nm.

2. The co-assembled nanoarray surface enhanced Raman scattering substrate according to claim 1, It is characterized in that The mass percentage concentration of the sodium citrate solution is 0.8% to 1.2%, and the mass percentage concentration of the chloroauric acid solution is 0.8% to 1.2%.

3. The co-assembled nanoarray surface enhanced Raman scattering substrate according to claim 2, It is characterized in that In the process of preparing No. 1 nano-gold, the volume ratio of the sodium citrate solution, the chloroauric acid solution and water is 9-11:1:90-110.

4. The co-assembled nanoarray surface enhanced Raman scattering substrate according to claim 2, It is characterized in that The specific preparation process of the gold seed solution is as follows: Add sodium citrate solution and chloroauric acid solution into water to obtain a gold seed solution; The volume ratio of the sodium citrate solution, the chloroauric acid solution and water is 1.15-1.17:1:100-102.

5. The co-assembled nanoarray surface enhanced Raman scattering substrate according to claim 3, It is characterized in that In the process of preparing the No. 2 nanogold solution, the reducing agent is a hydroxylamine hydrochloride solution; The concentration of the hydroxylamine hydrochloride solution is 0.005 mol / L to 0.015 mol / L; The volume ratio of the gold seed solution, hydroxylamine hydrochloride solution, chloroauric acid solution and sodium citrate solution is 30-35:10-20:1:2 。 6. The co-assembled nanoarray surface enhanced Raman scattering substrate according to claim 1, It is characterized in that The volume ratio of the No. 1 nano-gold solution to the No. 2 nano-gold solution is 50-500:

500.

7. The co-assembled nanoarray surface enhanced Raman scattering substrate according to claim 1, It is characterized in that In the water-organic solvent system, the organic solvents are dichloromethane and n-hexane; In the water-organic solvent system, the volume ratio of dichloromethane, n-hexane and water is 2:1:0.8-1.

1.

8. A co-assembled nanoarray surface-enhanced Raman scattering substrate prepared by the method for preparing a co-assembled nanoarray surface-enhanced Raman scattering substrate according to any one of claims 1 to 7.

9. A method for detecting malachite green, It is characterized in that The following steps are involved: The co-assembled nanoarray surface enhanced Raman scattering substrate of claim 8 is placed in a malachite green solution to be detected and immersed for 28 to 32 minutes, taken out, dried, and then the surface enhanced Raman scattering signal is detected to obtain the Raman intensity of the malachite green solution to be detected; The Raman intensity of the malachite green solution to be detected is substituted into the standard curve of malachite green solution concentration-Raman intensity to obtain the concentration of the malachite green solution to be detected.

10. The method for detecting malachite green according to claim 9, It is characterized in that The pH value of the malachite green solution to be detected is 3-5.

Citation Information

Patent Citations

  • Method for preparing size-controlled gold nanostars with surface Raman enhanced activity

    CN102837005A

  • Method for detecting MG based on Au-Ag NPs composite material

    CN107389655A

  • Surface enhanced Raman scattering nano-probe taking polystyrene as wrapping shell layer, and preparation method of surface enhanced Raman scattering nano-probe

    CN109342392A

  • Construction method of algae toxin ratio Raman sensor based on gold-silver nano assembly body

    CN110308137A

  • Surface-enhanced Raman scattering substrate and preparation method thereof and in-situ rapid detection method

    CN110790220A