Rapid determination method for types and contents of inclusions in aluminum alloy melt

The detection of the types and content of inclusions in aluminum alloy melt by microscope with laser-induced breakdown plasma emission spectroscopy has solved the problem of long detection time and low accuracy in the prior art, and achieved rapid and accurate inclusions analyze.

CN119086530APending Publication Date: 2024-12-06CHONGQING NATIONAL INNOVATION INSTITUTE OF LIGHT ALLOYS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210576.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing aluminum alloy melt inclusion detection methods have a long detection time, rely on technical personnel's experience and low accuracy, so it is impossible to accurately identify the content of different inclusion species.

Method used

A microscope with laser-induced breakdown plasma emission spectroscopy was used to count the grid area proportion of inclusions through the microscope mesh ruler, and LIBS was used to detect the inclusion components to quickly calculate the types and content of inclusions.

Benefits of technology

It significantly shortens the detection time, improves the detection efficiency and accuracy, reduces the human eye load, reduces detection errors, and improves the ability to control the melt quality of aluminum alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020212460000081
    Figure BDA0005020212460000081
  • Figure BDA0005020212460000091
    Figure BDA0005020212460000091
  • Figure BDA0005020212460000101
    Figure BDA0005020212460000101
Patent Text Reader

Abstract

The invention relates to the technical field of detection and analysis of non-metallic inclusions in aluminum alloy materials, and discloses a rapid determination method for types and content of aluminum alloy melt inclusions, which comprises the following steps: step S1, cutting an off-line slag measurement aluminum alloy sample to prepare an aluminum alloy sample suitable for inlaying; s2, the embedded sample is subjected to grinding, polishing and cleaning treatment; s3, placing the sample on a microscope objective table with an LIBS function, and adjusting the detection condition of a microscope; s4, opening a netlike scale of the microscope, setting the side length L of a unit grid, moving the visual field along the Y-axis direction, and observing and counting the grid area proportion Pi of each inclusion in a specified detection range; s5, detecting the components of each inclusion by utilizing a microscope LIBS (Laser-induced Breakdown Spectroscopy), and judging the type of the inclusion; and step S6, calculating according to the Pi to obtain the type content N of each inclusion in the sample. According to the scheme, the types and contents of different inclusions are effectively detected, the operation is simple and convenient, the speed is high, and the detection efficiency is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of non-metallic inclusion detection and analysis in aluminum alloy materials, and in particular to a method for quickly determining the types and contents of inclusions in an aluminum alloy melt. Background Art

[0002] The inclusions produced during the aluminum alloy casting process will be inherited into the aluminum alloy products. The inclusions in the aluminum melt are divided into endogenous inclusions and exogenous inclusions. They have a wide range of sources and types, mainly oxides (Al 2 O 3 , MgO), carbides (SiC, AlC), nitrides (AIN) and borides (TiB 2 ) and refractory materials, slag, refiners, etc. remain in the melt during the casting process, thus generating inclusions. Generally, their number is relatively large, the particle size is relatively small and the distribution is relatively uniform. Specifically, most of them are granular or film-like with similar shapes and close grayscale values. Generally speaking, the number, size, composition, distribution, etc. of non-metallic inclusions will have an important influence on the properties of aluminum alloys (such as continuity). At the same time, due to the difference in elastic modulus and expansion coefficient between inclusions and the matrix, severe stress concentration will occur around the inclusions during the deformation process, which will then cause cracks. Therefore, the accurate identification of inclusions in aluminum alloy melts and the rapid determination of their content are of great significance to aluminum processing companies.

[0003] At present, the PoDFA offline slag measurement method proposed by ABB is widely recognized and widely used in the industrial field for the detection of aluminum alloy melt inclusions. This method uses the PoDFA slag measuring instrument to take samples at each stage of melt processing, observes the slag sample with a metallographic microscope, uses the eyepiece micrometer (or square grid micrometer) of the metallographic microscope to measure the length of the filter in the sample detection area, observes the color, morphology and size of the slag under an appropriate magnification, identifies the type of slag with the naked eye, counts the number of grids of different types of inclusions, and quantitatively calculates the number of inclusions in the filter cake and the area of ​​the filter cake to obtain the slag content per unit area. This method can measure the types and contents of inclusions in aluminum alloy melts, but the detection time is too long, it is highly dependent on the experience of technicians, has large human errors, low accuracy, and is prone to eye damage.

[0004] In summary, the existing methods for determining the content and types of inclusions in aluminum alloys focus on the quantitative evaluation of the inclusions as a whole, and cannot truly reflect the content of different types of inclusions in the aluminum alloy melt. Therefore, a simple, fast, and highly accurate method for determining the types and contents of aluminum alloy inclusions is urgently needed. Summary of the invention

[0005] The present invention aims to provide a method for quickly determining the types and contents of inclusions in an aluminum alloy melt, so as to solve the technical problem in the prior art that the quantitative analysis time of inclusions in an aluminum alloy melt is long and leads to low detection efficiency.

[0006] To achieve the above object, the present invention adopts the following technical solution: a method for quickly determining the type and content of inclusions in aluminum alloy melt, comprising the following steps:

[0007] Step S1, test sample preparation: cutting and processing the offline slag test aluminum alloy sample to prepare an aluminum alloy sample suitable for inlaying, and the sample size should meet the size requirements of the inlaying equipment;

[0008] Step S2, sample processing: grinding, polishing and cleaning the mounted samples;

[0009] Step S3, sample loading: placing the sample on a microscope stage with a laser induced breakdown plasma emission spectroscopy (LIBS) function, and adjusting the microscope detection conditions;

[0010] Step S4, preliminarily confirm inclusions: turn on the microscope mesh ruler, set the unit grid side length L, move the field of view along the Y-axis direction, observe and count the grid area proportion Pi of each inclusion within the specified detection range;

[0011] Step S5, detecting and confirming the type of inclusions: using microscope LIBS to detect the composition of each inclusion, and judging the type of inclusions based on the composition results;

[0012] Step S6, calculating the inclusion content: calculating the content N of each type of inclusion in the sample according to the grid area proportion Pi.

[0013] The principles and advantages of this solution are:

[0014] 1. Improve detection efficiency: Compared with the existing technology that uses a metallographic microscope to detect the total content of aluminum alloy inclusions, which is inefficient, this solution can directly count the grid area ratio Pi of different inclusions in the aluminum alloy melt through the microscope mesh scale, and then quickly confirm the inclusion type by detecting the composition of each inclusion through LIBS, and then quickly calculate the content of different inclusions according to the grid area ratio Pi. During the detection process, the operation is simple and fast, which effectively improves the detection efficiency. Specifically, the applicant found through long-term experiments that compared with the existing technology that uses a metallographic microscope to detect the total weight of inclusions in aluminum alloy melts, which takes 2 to 3.5 hours, this solution only takes 0.8 to 1.3 hours to detect the content and type of inclusions in the same sample, significantly shortening the time required for detection and improving detection efficiency.

[0015] 2. Improve detection accuracy: Compared with the existing metallographic microscope, which can only roughly judge the type of inclusions based on the morphology when detecting aluminum alloy inclusions, resulting in low detection accuracy, this solution uses a microscope to preliminarily judge the major types of inclusions and then uses LIBS to sample and detect the composition of inclusions, effectively confirming the specific types of inclusions (such as spinel, magnesia, alumina, TiB 2 ), effectively improving the detection accuracy. Specifically, taking a 2xxx aluminum alloy as an example, comparative example 1 uses a metallographic microscope to determine the types of inclusions, including oxide inclusions and refiner particle inclusions, and can only roughly determine the formation mode of the inclusions, and cannot determine whether it is a specific oxide inclusion or refiner particle inclusion; while Example 1 uses the method of this scheme to detect the same 2xxx aluminum alloy, which can accurately identify the inclusions as spinel, magnesium oxide, aluminum oxide, TiB 2 , the types are clearer, the detection accuracy is higher, it is more instructive for technicians to effectively control the melt quality, and it is also helpful to build an aluminum alloy inclusion database and detection standards.

[0016] 3. Higher safety: Compared with the existing metallographic microscope that requires long-term naked eye observation to detect aluminum alloy inclusions, which is easy to damage the human eye, during the detection process of this solution, there is no need to limit the naked eye to the eyepiece range, but to observe through the connected computer display screen, with a larger and clearer field of view, which not only effectively improves the detection accuracy and efficiency, but also reduces the burden on the human eye and improves the detection safety.

[0017] 4. This scheme can set the appropriate mesh ruler side length L according to the shape and size of different inclusions by setting the unit grid side length L of the microscope mesh ruler, fix the detection area, solve the problem of scattered detection results and poor representativeness, and further improve the detection accuracy.

[0018] 5. This solution uses the LIBS function of the microscope to analyze the composition of each inclusion and determine the type of inclusion based on the results. It can achieve accurate qualitative analysis of the properties of inclusions in the aluminum alloy melt, shorten the detection time, reduce the error of directly judging the type of inclusions in the aluminum alloy melt based on the experience of technicians, and further improve the detection accuracy.

[0019] Preferably, as an improvement, in step S3, the microscope stage position is restored to the default position, the X and Y coordinate axes are restored to the coordinate origin, the Z axis distance is set to 5 mm, the light source is coaxial incident, and the sample is observed under bright field.

[0020] Beneficial effect: The above arrangement facilitates cleaning and observation of inclusions inside aluminum alloy samples. Specifically, the optimal working distance of the microscope stage is 5 mm. The applicant has found through long-term experiments that if the working distance is too long or too short, the sample will be too close or too far from the objective lens, causing the sample to be distorted on the display screen and unclear focus.

[0021] Preferably, as an improvement, in step S4, the unit grid side length L is set in the range of 50 to 500 μm.

[0022] Beneficial effect: The above setting is adopted to facilitate the counting of the area ratio of a single inclusion grid during the detection process. The applicant has found through long-term experiments that if the unit grid side length L is too short (less than 50μm), the grid will be too small to effectively count the area ratio of a single inclusion grid; if the unit grid side length L is too long (greater than 500μm), the grid will be too large to cause a large error in the statistical value of the area ratio of a single inclusion grid, thereby reducing the detection accuracy.

[0023] Preferably, as an improvement, in step S4, the detection range is set to be 0.5 to 1 mm on each side of the interface between the filter layer and the aluminum substrate, and the field of view of a single movement along the Y-axis direction is 0.2 to 1 mm.

[0024] Beneficial effect: The above arrangement is convenient for effectively counting the slag content of the sample. The applicant has found through long-term experiments that if the distance between the filter layer and the aluminum substrate is too short (less than 0.5 mm), the statistical results will be unrepresentative due to the small detection area; if the distance between the filter layer and the aluminum substrate is too long (greater than 1 mm), the detection area will be too large and there will be no slag in some areas, resulting in a long detection time and reduced detection efficiency.

[0025] Preferably, as an improvement, in step S4, the field of view of a single movement along the Y-axis direction is 0.2-1 mm.

[0026] Beneficial effect: The above setting is convenient for quickly counting the sample slag content and concentrating the detection area. The applicant has found through long-term experiments that if the field of view of a single movement is too short (less than 0.2mm), part of the detection area will be repeated in the field of view, which will lead to a long detection time; if the field of view of a single movement is too long (greater than 1mm), part of the detection area cannot be presented in the field of view, resulting in the omission of some areas without detection, affecting the overall detection results.

[0027] Preferably, as an improvement, in the above step S4, a microscope mesh ruler is used to count the grid area proportion Pi of each inclusion within a specified detection range under a field of view of 100 to 500 times, and the value range of Pi is 0.1 to 1.

[0028] Beneficial effect: The above arrangement facilitates clear observation and identification of inclusions (i.e., slag) in the sample. The applicant has found through long-term experiments that if the field of view magnification is too small (less than 100 times), the inclusions will be misidentified due to the small magnification and unclear identification; if the field of view magnification is too large (less than 500 times), the single observable field of view will be reduced due to the large magnification, thereby increasing the detection time and reducing the detection efficiency.

[0029] Preferably, as an improvement, in step S5, the magnification is selected to be 300 to 1000 times when the laser induced breakdown plasma emission spectroscopy is used to detect the inclusion components.

[0030] Beneficial effect: The above setting is used to facilitate clear identification and preliminary judgment of the types of inclusions in the sample. The applicant has found through long-term experiments that if the magnification is too small (less than 300 times), the type of inclusions will be misidentified due to the small magnification and large field of view; if the magnification is too large (such as greater than 1000 times), the field of view that can be analyzed at a time will be reduced, the detection time will be increased, and the detection efficiency will be reduced.

[0031] Preferably, as an improvement, in step S5, the number of single inclusion component analysis detection points is 4 to 25.

[0032] Beneficial effect: The above configuration is used to effectively determine the type of inclusions and improve the accuracy of inclusion type detection. The applicant has found through long-term experiments that if there are too few analysis and detection points (less than 4), the type of inclusions cannot be accurately determined due to the large difference in composition results, and too many detection points will not further improve the detection accuracy, but will reduce the detection efficiency.

[0033] Preferably, as an improvement, in step S6, the calculation formula of the inclusion content in the aluminum alloy melt is as follows: N = [(∑Pi)L 2 ] / M, where i=1, 2, ... n, and M is the filtered weight of the aluminum liquid.

[0034] Beneficial effect: The above-mentioned setting is used to facilitate accurate calculation of the contents of different inclusions in the aluminum alloy melt, thereby accurately evaluating the quality of the batch of aluminum alloy melts.

[0035] Preferably, as an improvement, in step S1, the aluminum alloy inclusion sample is sliced ​​into thin sheet alloy samples of 15-20mm*10-15mm and 10-15mm thick, and the size of the alloy sample to be tested after the thin sheet is inlaid is φ25-φ40mm and the thickness is 20-25mm.

[0036] Preferably, as an improvement, in step S2, the grinding treatment is to use 800-2000 mesh diamond sandpaper and SiC sandpaper for grinding for 5-10 minutes, the polishing treatment is to use 0.05-5μm diamond suspension for polishing for 10-15 minutes, and the cleaning treatment is to use water for cleaning for 0.5-1 minute; the sample after grinding, polishing and cleaning is mirror-like and has no solvent residue.

[0037] Beneficial effect: The above-mentioned setting is adopted to facilitate obtaining aluminum alloy samples that meet the requirements of laser-induced breakdown plasma emission spectroscopy. The applicant has found through long-term experiments that if the grinding (conditions) exceeds the specified range of this scheme, the sample cannot be ground flat due to the mismatch between the hardness of the sandpaper and the sample; if the grinding time is too long, the sample cannot be effectively detected due to cracking at the junction of the sample; if the grinding time is too short, the sample cannot be detected due to unevenness. If the polishing (conditions) exceeds the specified range of this scheme, the sample cannot be mirrored due to the mismatch of the lubricating liquid particle size; if the polishing time is too long, the inclusions cannot be fully counted due to the increase in scratches on the sample surface; if the polishing time is too long, the sample surface will be foggy and the sample cannot be effectively detected. If other solvents are used for cleaning, the sample will be corroded due to solvent reaction; if the cleaning time is too long, the sample will be partially oxidized due to long-term water shock; if the cleaning time is too long, the sample detection result will be incorrect due to residual impurities. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a schematic diagram of the specified detection area of ​​the aluminum alloy sample in the method for rapid determination of the types and contents of inclusions in aluminum alloy melts in Example 1 of the present invention (the black parts on both sides of the figure are filter layers, and the white part in the middle is the aluminum matrix, the same below).

[0039] Figure 2 This is the LIBS composition analysis diagram of TiB2 inclusions in the aluminum alloy sample in Example 1 of the present invention at a 300x field of view.

[0040] Figure 3 This is the LIBS composition analysis diagram of spinel inclusions in the aluminum alloy sample in Example 2 of the present invention at a 300x field of view.

[0041] Figure 4 This is the LIBS composition analysis diagram of alumina inclusions in the aluminum alloy sample in Example 3 of the present invention at a 300x field of view.

[0042] Figure 5 This is the LIBS composition analysis diagram of MgO inclusions in the aluminum alloy sample in Example 4 of the present invention at a 500x field of view.

[0043] Figure 6This is a typical inclusion morphology image of the aluminum alloy sample in Comparative Example 1 of the present invention under a 200x field of view of a metallographic microscope.

[0044] Figure 7 This is a typical inclusion morphology image of the aluminum alloy sample in Comparative Example 2 of the present invention under a 500x field of view of a metallographic microscope (① is inclusion; ② is aluminum alloy phase; ③ is microscopic looseness).

[0045] Figure 8 This is a typical inclusion morphology image of the aluminum alloy sample in Comparative Example 3 of the present invention under a 500x field of view of a metallographic microscope (①②③ are all inclusions).

[0046] Fig. 9 The following are typical inclusion morphology images of the aluminum alloy sample in Comparative Example 4 of the present invention under a metallographic microscope at 200 and 500 times the field of view (① is the inclusion). DETAILED DESCRIPTION

[0047] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.

[0048] Program Overview

[0049] This scheme provides a method for quickly determining the type and content of inclusions in aluminum alloy melt, comprising the following steps:

[0050] Step S1, test sample preparation: cutting and processing the offline slag test aluminum alloy sample to prepare an aluminum alloy sample suitable for inlaying, and the sample size should meet the size requirements of the inlaying equipment;

[0051] As a reference, this scheme slices the aluminum alloy slag sample into thin sheet alloy samples of 15~20mm*10~15mm and 10~15mm thickness. The size of the alloy sample to be tested after the thin slices are inlaid is φ25~φ40mm and the thickness is 20~25mm.

[0052] Step S2, sample processing: grinding, polishing and cleaning the mounted samples;

[0053] As a reference, the grinding treatment is to use 800-2000 mesh diamond sandpaper and SiC sandpaper for 5-10 minutes, the polishing treatment is to use 0.05-5μm diamond suspension for 10-15 minutes, and the cleaning treatment is to use water for 0.5-1 minute; the samples after grinding, polishing and cleaning are mirror-like and have no solvent residue.

[0054] Step S3, sample loading: placing the sample on a microscope stage with a laser induced breakdown plasma emission spectroscopy (LIBS) function, and adjusting the microscope detection conditions;

[0055] As a reference, after the sample is placed on the stage, the X and Y coordinate axes of the microscope stage position are restored to the coordinate origin, the Z axis distance (i.e., the optimal working distance of the microscope stage position) is set to 5 mm, the light source is coaxial incident, and the sample is observed under bright field.

[0056] The microscope of this scheme is easy to operate. After confirming that the stage is restored to the default position (that is, the coordinate axis of the stage is returned to 0, back to the coordinate origin) and adjusting the working distance, the type and content of inclusions in the aluminum alloy sample can be detected without any other additional parameter design.

[0057] Step S4, preliminarily confirm inclusions: turn on the microscope mesh ruler, set the unit grid side length L, move the field of view along the Y-axis direction, observe and count the grid area proportion Pi of each inclusion within the specified detection range;

[0058] As a reference, the unit grid side length L is set in the range of 50 to 500 μm, the specified detection range is 0.5 to 1 mm on both sides of the junction of the filter layer and the aluminum substrate, the field of view of a single movement along the Y-axis direction is 0.2 to 1 mm, and the grid area proportion Pi of each inclusion in the specified detection range is calculated using a microscope mesh ruler under a field of view of 100 to 500 times. After testing, the value range of Pi is 0.1 to 1.

[0059] Step S5, detecting and confirming the type of inclusions: using microscope LIBS to detect the composition of each inclusion, and judging the type of inclusions based on the composition results;

[0060] As a reference, when using laser induced breakdown plasma emission spectroscopy (LIBS) to detect inclusion components, the magnification is selected to be 300 to 1000 times, and 4 to 25 detection points are selected when analyzing a single inclusion component.

[0061] Step S6, calculating the inclusion content: calculating the content N of each type of inclusion in the sample according to the grid area proportion Pi.

[0062] As a reference, the calculation formula for the inclusion content in aluminum alloy melt is as follows: N = [(∑Pi)L 2 ] / M, where i=1, 2, ... n, and M is the filtered weight of the aluminum liquid.

[0063] Example 1

[0064] This solution provides a method for quickly determining the type and content of inclusions in aluminum alloy melts. The offline slag sample selected in this embodiment is a 2xxx aluminum alloy. The method of the present invention is used to detect the type and content of inclusions in the selected sample. The specific steps are as follows:

[0065] (1) Obtain a 2xxx aluminum alloy slag sample using an offline slag meter and record the filtered weight of the aluminum liquid (M = 1.43 kg).

[0066] As a reference, this scheme takes 2A12 aluminum alloy as an example to demonstrate in detail the method for rapid determination of the types and contents of inclusions in aluminum alloy melts.

[0067] (2) Cut the 2xxx aluminum alloy slag sample to prepare an alloy sample suitable for inlay. The sample size should meet the size requirements of the inlay equipment.

[0068] As a reference, this scheme slices the aluminum alloy slag sample into thin sheet alloy samples with a size of 15mm*10mm and a thickness of 10mm. The size of the alloy sample to be tested after the thin slices are inlaid is φ30mm and the thickness is 25mm.

[0069] (3) Use diamond sandpaper and SiC sandpaper to grind the mounted samples, and use diamond polishing agent to polish the grinded samples; wash the polished samples with water, and the samples will be mirror-like and free of solvent residue.

[0070] (4) A microscope with laser-induced breakdown plasma emission spectroscopy (LIBS) function was set up (the X and Y axes of the stage position were restored to the origin, the Z axis distance was set to 5 mm, and the microscope light source was set to coaxial incident light), and the sample was observed under bright field.

[0071] (5) Adjust the magnification to 200 times, turn on the microscope mesh ruler, set the mesh ruler side length L to 100 μm, and the single movement field along the Y axis to 0.5 mm. Use the mesh ruler to observe and count the mesh area proportion of each inclusion in the 0.5 mm area on the left and right of the junction between the filter layer and the aluminum substrate. The complete detection area is as follows: Figure 1 Shown in the red box.

[0072] (6) The microscope mode was switched to LIBS mode, the magnification was adjusted to 300 times, and the laser-induced breakdown plasma emission spectroscopy was used to detect the composition of each inclusion. The number of analysis detection points for a single inclusion composition was greater than 4. The type of inclusion was determined by the composition results and the total grid area proportion ∑Pi of different inclusion types was calculated. The statistical results are shown in Table 1. The typical inclusion types of this sample are as follows: Figure 2 shown.

[0073] Table 1 The proportion of total mesh area of ​​each type of inclusions at 200 times

[0074]

[0075] (7) Using N = [(∑Pi)L 2 ] / M calculates the content of each type of inclusion. Through calculation, the content of each type of inclusion in 2xxx is shown in Table 2.

[0076] Table 2 Content of various inclusion types at 200 times (mm 2 / kg)

[0077] Spinel Alumina Magnesium Oxide <![CDATA[TiB 2 ]]> 0.0069 0.0007 0.0007 0.0259

[0078] Example 2

[0079] The difference between this embodiment and embodiment 1 is that the offline slag test sample is a certain 3xxx aluminum alloy. The method of the present invention is used to detect the type and content of inclusions on the selected sample, and the specific steps are as follows:

[0080] (1) Obtain a 3xxx aluminum alloy slag sample using an offline slag meter and record the filtered aluminum liquid weight M = 1.41 kg.

[0081] (2) Cut the 3xxx aluminum alloy slag sample to prepare an alloy sample suitable for inlay. The sample size should meet the size requirements of the inlay equipment.

[0082] (3) Use diamond sandpaper and SiC sandpaper to grind the mounted samples, and use diamond polishing agent to polish the grinded samples; wash the polished samples with water, and the samples will be mirror-like and free of solvent residue.

[0083] (4) The X and Y coordinate axes of the microscope stage with laser-induced breakdown plasma emission spectroscopy (LIBS) function were restored to the coordinate origin, the Z axis distance was set to 5 mm, the microscope light source was set to coaxial incident light, and the sample was observed under bright field.

[0084] (5) Adjust the magnification to 500 times, turn on the microscope mesh ruler, set the mesh ruler side length L to 100 μm, and the single movement field along the Y axis to 0.5 mm. Observe and count the mesh area proportion of each inclusion in the 0.5 mm area on the left and right of the junction between the filter layer and the aluminum substrate through the mesh ruler.

[0085] (6) The microscope mode was switched to LIBS mode, the magnification was adjusted to 300 times, and the laser induced breakdown plasma emission spectroscopy was used to detect the composition of each inclusion. The number of analysis detection points for a single inclusion component was greater than 4. The type of inclusion was determined by the composition results and the total grid area proportion ∑Pi of different inclusion types was calculated. The statistical results are shown in Table 3. The typical inclusion types of this sample are as follows: Figure 3 shown.

[0086] Table 3 The proportion of total mesh area of ​​each type of inclusions at 500 times

[0087]

[0088] (7) Using N = [(∑Pi)L 2 ] / M calculates the content of each type of inclusion. Through calculation, the content of each type of inclusion in 3xxx is shown in Table 4.

[0089] Table 4 Content of various inclusion types at 500 times (mm 2 / kg)

[0090] Alumina Magnesium Oxide <![CDATA[TiB 2 ]]> Refractory Materials Spinel 0.0085 0.0049 0.0106 0.0028 0.0163

[0091] Example 3

[0092] The difference between this embodiment and embodiment 1 is that the offline slag test sample is a certain 5xxx aluminum alloy. The method of the present invention is used to detect the type and content of inclusions on the selected sample, and the specific steps are as follows:

[0093] (1) Obtain a 5xxx aluminum alloy slag sample using an offline slag meter and record the filtered aluminum liquid weight M = 1.40 kg.

[0094] (2) Cut the 5xxx aluminum alloy slag sample to prepare an alloy sample suitable for inlay. The sample size should meet the size requirements of the inlay equipment.

[0095] (3) Use diamond sandpaper and SiC sandpaper to grind the mounted samples, and use diamond polishing agent to polish the grinded samples; wash the polished samples with water, and the samples will be mirror-like and free of solvent residue.

[0096] (4) The X and Y coordinate axes of the microscope stage with laser-induced breakdown plasma emission spectroscopy (LIBS) function were restored to the coordinate origin, the Z axis distance was set to 5 mm, the microscope light source was set to coaxial incident light, and the sample was observed under bright field.

[0097] (5) Adjust the magnification to 200 times, turn on the microscope mesh ruler, set the mesh ruler side length L to 50 μm, and the single movement field along the Y axis to 1 mm. Observe and count the mesh area proportion of each inclusion in the 0.5 mm area on the left and right of the junction between the filter layer and the aluminum substrate through the mesh ruler.

[0098] (6) The microscope mode was switched to LIBS mode, the magnification was adjusted to 300 times, and the laser induced breakdown plasma emission spectroscopy was used to detect the composition of each inclusion. The number of analysis detection points for a single inclusion component was greater than 4. The type of inclusion was determined by the composition results and the total grid area proportion ∑Pi of different inclusion types was calculated. The statistical results are shown in Table 5. The typical inclusion types of this sample are as follows: Figure 4 shown.

[0099] Table 5 The proportion of total mesh area of ​​each type of inclusions at 200 times

[0100]

[0101] (7) Using N = [(∑Pi)L 2 ] / M calculates the content of each type of inclusions. Through calculation, the content of each type of inclusions in 5xxx is shown in Table 6.

[0102] Table 6 Content of various inclusion types at 200 times (mm 2 / kg)

[0103] Alumina Magnesium Oxide <![CDATA[TiB 2 ]]> Spinel 0.01875 0.0069 0.0093 0.0061

[0104] Example 4

[0105] The difference between this embodiment and embodiment 1 is that the offline slag test sample is a certain 7xxx aluminum alloy. The method of the present invention is used to detect the type and content of inclusions on the selected sample, and the specific steps are as follows:

[0106] (1) Obtain a 7xxx aluminum alloy slag sample using an offline slag meter and record the filtered aluminum liquid weight M = 1.46 kg.

[0107] (2) Cut the 7xxx aluminum alloy slag sample to prepare an alloy sample suitable for inlay. The sample size should meet the size requirements of the inlay equipment.

[0108] (3) Use diamond sandpaper and SiC sandpaper to grind the mounted samples, and use diamond polishing agent to polish the grinded samples; wash the polished samples with water, and the samples will be mirror-like and free of solvent residue.

[0109] (4) The X and Y coordinate axes of the microscope stage with laser-induced breakdown plasma emission spectroscopy (LIBS) function were restored to the coordinate origin, the Z axis distance was set to 5 mm, the microscope light source was set to coaxial incident light, and the sample was observed under bright field.

[0110] (5) Adjust the magnification to 500 times, turn on the microscope mesh ruler, set the mesh ruler side length L to 50 μm, and the single movement field along the Y axis to 1 mm. Observe and count the mesh area proportion of each inclusion in the 0.5 mm area on the left and right of the junction between the filter layer and the aluminum substrate through the mesh ruler.

[0111] (6) The microscope mode was switched to LIBS mode, the magnification was adjusted to 500 times, and the laser induced breakdown plasma emission spectroscopy was used to detect the composition of each inclusion. The number of detection points for a single inclusion composition analysis was greater than 4. The type of inclusion was determined by the composition results and the total grid area proportion ∑Pi of different inclusion types was calculated. The statistical results are shown in Table 7. The typical inclusion types of this sample are as follows: Figure 5 shown.

[0112] Table 7 The proportion of total grid area of ​​each type of inclusions at 500 times

[0113]

[0114] (7) Using N = [(∑Pi)L 2 ] / M calculates the content of each type of inclusion. Through calculation, the content of each type of inclusion in 7xxx is shown in Table 8.

[0115] Table 8 Content of various inclusion types at 500 times (mm 2 / kg)

[0116] Alumina Magnesium Oxide Ti-containing particles Refractory Materials 0.0009 0.0048 0.0005 0.0001

[0117] Comparative Example 1

[0118] This comparative example and Example 1 use the same 2xxx slag sample for analysis, the difference is that the slag sample in Comparative Example 1 uses the traditional metallographic method to detect the type and content of inclusions, and the specific steps are as follows:

[0119] (1) Place the polished sample on the stage of the metallographic microscope.

[0120] (2) Move the field of view at 50 times magnification and use the square grid micrometer of the eyepiece of the metallographic microscope to manually measure and record the filter length of the sample detection area.

[0121] (3) Place the slag in the field of view in the eyepiece grid micrometer at 200 times magnification, and use the grid to estimate the area of ​​different types of inclusions in the 0.5 mm area above and below the interface between the filter and solid aluminum.

[0122] (4) Observe the morphological characteristics of inclusions with a metallographic microscope at 200-500 times magnification, and determine the type of inclusions based on the morphological characteristics.

[0123] Comparative Example 1 Typical inclusion types such as Figure 6 As shown in the figure, it can be seen that the inclusions are light brown and dark brown fine particles gathered into flakes. According to the morphological characteristics, it can only be inferred that the inclusions are MgO or TiB 2 , unable to make an accurate judgment.

[0124] Comparative Example 2

[0125] This comparative example and Example 2 use the same 3xxx slag sample for analysis. The difference is that the slag sample in Comparative Example 2 uses the traditional metallographic method to detect the type and content of inclusions. The steps are the same as those in Comparative Example 1. The results are detailed in Figure 7 ,from Figure 7 It can be seen that the inclusions in the sample are irregular in shape and dark gray to black. Based on the morphological characteristics, it is speculated that the inclusions in the sample are spinel or γ-Al 2 O 3 , unable to make an accurate judgment.

[0126] Specifically, Figure 7 As shown, when making a preliminary judgment, Figure 7 There is an obvious inclusion area in (a). Based on experience, the inclusion at ① is speculated to be spinel or γ-Al 2 O 3 ; Figure 7 There is an obvious inclusion area in (b). Based on experience, the inclusion at ① is speculated to be spinel or γ-Al 2 O 3 However, after LIBS sampling and analysis of this scheme, it was found that the ① in Figure (a) is a spinel inclusion, and the ① in Figure (b) is a γ-Al 2 O 3 Inclusions. It can be seen that compared with the accurate detection of inclusion types and contents by this scheme, when the traditional metallographic method is used to detect inclusion types, it is difficult for experienced technicians to accurately determine the types of inclusions, which affects the judgment of the total amount of inclusions in the entire aluminum alloy sample, reduces the detection accuracy, and further affects the accuracy of its guidance on melt quality control.

[0127] Comparative Example 3

[0128] This comparative example and Example 3 use the same 5xxx slag sample for analysis. The difference is that the slag sample in Comparative Example 3 uses the traditional metallographic method to detect the type and content of inclusions. The steps are the same as those in Comparative Example 1. The results are detailed in Figure 8 ,from Figure 8 It can be seen that the sample is mixed with fine particles that aggregate into flakes and are dark brown. Based on the morphological characteristics, it is speculated that the inclusions in the sample are MgO or TiB 2 , unable to make an accurate judgment.

[0129] Specifically, Figure 8 As shown, when making a preliminary judgment, Figure 8 There are three obvious inclusion areas in (a). Figure 8 There are two obvious inclusion areas in (b). Figure 8 The inclusions at ① in (a) and 8(b) have similar morphologies and are difficult to distinguish. Based on experience, it is speculated that they are MgO or TiB. 2However, after LIBS sampling and analysis of this scheme, it was found that Figure 8 In (a), position ① is MgO inclusion; Figure 8 (b) ① is TiB 2 Inclusion.

[0130] Comparative Example 4

[0131] This comparative example and Example 4 use the same 7xxx slag sample for analysis. The difference is that the slag sample in Comparative Example 4 uses the traditional metallographic method to detect the type and content of inclusions. The steps are the same as those in Comparative Example 1. The results are detailed in Fig. 9 ,from Fig. 9 It can be seen that the sample is irregularly mixed, has no fixed shape, and is dark gray to black. Based on the morphological characteristics, it is speculated that the inclusions in the sample are refractory or α-Al 2 O 3 , unable to make an accurate judgment.

[0132] Specifically, Fig. 9 As shown, when making a preliminary judgment, Fig. 9 There is an obvious inclusion area in (a). Fig. 9 There is an obvious inclusion area in (b) and the inclusion morphology in (①) is similar and difficult to distinguish. Based on experience, it is speculated that it is refractory or α-Al 2 O 3 However, after LIBS sampling and analysis of this scheme, it was found that Fig. 9 In (a), position ① is a refractory inclusion; Fig. 9 (b) ① is α-Al 2 O 3 Inclusion.

[0133] Table 9 Comparison of the types and contents of inclusions in the examples and comparative examples

[0134] Example Alloy grade Inclusion Type Analysis time (h) Example 1 2xxx <![CDATA[Spinel, magnesium oxide, aluminum oxide, TiB 2 > 1 Comparative Example 1 2xxx Oxide inclusions, refiner particle inclusions 2.5 Example 2 3xxx <![CDATA[Spinel, magnesium oxide, aluminum oxide, TiB 2 , refractory]]> 1.1 Comparative Example 2 3xxx Oxide inclusions, refiner particle inclusions, refractory materials 2.8 Example 3 5xxx <![CDATA[Spinel, magnesium oxide, aluminum oxide, TiB 2 > 1.3 Comparative Example 3 5xxx Oxide inclusions, refiner particle inclusions, refractory materials 3.5 Example 4 7xxx Magnesium oxide, aluminum oxide, Ti-containing particles, refractory materials 0.8 Comparative Example 4 7xxx Oxide inclusions, refiner particle inclusions, refractory materials 2

[0135] It can be seen from the above that the method of the present invention can avoid the error of directly judging the type of inclusions based on the morphology of inclusions, and can quickly and accurately judge the type and content of inclusions in aluminum alloy melt.

[0136] In addition, Comparative Examples 5 to 12 show that during the detection process, parameters other than those in this solution are used to detect the types and contents of inclusions in the aluminum alloy melt. The differences in parameters from Example 1 (the off-line slag sample is a certain 2xxx aluminum alloy, and the filtration volume M is 1.43 kg) are shown in Table 10, and the detection results of the total grid area ratio and content of each type of inclusion are shown in Table 11. The deviations of the detection results and analysis time in Comparative Examples 5 to 12 from those in Example 1 are shown in Table 12.

[0137] Table 10 Parameter differences in comparative examples 5 to 12

[0138]

[0139] Table 11 Test results of Comparative Examples 5 to 12

[0140]

[0141] Table 12 Deviation of test results and analysis time in comparative examples 5 to 12 from those in Example 1

[0142]

[0143]

[0144] Experimental data show that in Comparative Example 5, due to the low magnification of the microscope, it is impossible to accurately identify the inclusions in the sample and perform content statistics; in Comparative Example 6, compared with Example 1, the types of inclusions in the melt are increased and the analysis time is long, indicating that too large a magnification will cause the numerical value of the grid area percentage of some smaller slags to be too high, the analysis accuracy is reduced, and rapid detection cannot be achieved; the analysis time of Comparative Example 7 is increased, which is because the side length of the unit grid becomes smaller, and the difficulty of statistically analyzing the slag content of the sample under the small grid field of view increases; in Comparative Example 8, the content of various types of inclusions in the melt increases, and the grid with too large a side length will cause the numerical value of the unit grid percentage of slag to be falsely high during the statistical process, and the error of the detection result is large; 9 After narrowing the detection area, the content of each type of inclusions decreased, the detection time was shortened, but the detection results were not representative; Comparative Example 10 After increasing the detection area, the content of each type of inclusions in the melt did not change significantly, but the analysis time increased significantly, and rapid detection could not be achieved; Comparative Example 11 The content of each type of inclusions did not change significantly, but the analysis time increased significantly, and a single movement distance of the Y axis that was too small would cause some of the visual fields to repeat, thereby reducing the analysis efficiency; Comparative Example 12 The number of inclusions in the melt decreased and the content decreased, and a single movement distance of the Y axis that was too large would cause the visual field to move discontinuously, and some types and contents of inclusions could not be effectively counted, resulting in a low accuracy of the detection results and a lack of representativeness. It can be seen that the method for determining the types and contents of inclusions in the aluminum alloy melt provided by the present invention can achieve rapid detection while ensuring the accuracy of the detection results.

[0145] In summary, this scheme can effectively determine the types and contents of inclusions in aluminum alloys by using a microscope with LIBS function. The operation process is simple, the measurement speed is fast, and the measurement accuracy is relatively high. It plays a high guiding role in the melt quality control during the aluminum alloy casting process.

[0146] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A method for quickly determining the type and content of inclusions in aluminum alloy melts. Features: The steps include: Step S1, test sample preparation: cutting and processing the offline slag test aluminum alloy sample to prepare an aluminum alloy sample suitable for inlay; Step S2, sample processing: grinding, polishing and cleaning the mounted samples; Step S3, sample loading: placing the sample on a microscope stage with LIBS function and adjusting the microscope detection conditions; Step S4, preliminarily confirm inclusions: turn on the microscope mesh ruler, set the unit grid side length L, move the field of view along the Y-axis direction, observe and count the grid area proportion Pi of each inclusion within the specified detection range; Step S5, detecting and confirming the type of inclusions: using microscope LIBS to detect the composition of each inclusion, and judging the type of inclusions based on the composition results; Step S6, calculating the inclusion content: calculating the content N of each type of inclusion in the sample according to the grid area proportion Pi.

2. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 1, Features: In step S3, the X and Y coordinate axes of the microscope stage position are restored to the coordinate origin, the Z axis distance is set to 5 mm, the light source is coaxial incident, and the sample is observed under bright field.

3. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 1, Features: In step S4, the unit grid side length L is set in the range of 50 to 500 μm, the detection range is specified as the 0.5 to 1 mm area on the left and right sides of the junction of the filter layer and the aluminum substrate, and the field of view of a single movement along the Y-axis direction is 0.2 to 1 mm.

4. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 1, Features: In step S4, a microscope mesh ruler is used to count the grid area proportion Pi of each inclusion within a specified detection range under a 100-500 times field of view, and the value range of Pi is 0.1-1.

5. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 1, Features: In step S5, the magnification is selected to be 300 to 1000 times when the inclusion components are detected by laser induced breakdown plasma emission spectroscopy.

6. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 5, Features: In step S5, 4 to 25 single inclusion component analysis detection points are performed.

7. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 6, Features: In step S6, the calculation formula of the inclusion content in the aluminum alloy melt is as follows: N = [(∑Pi)L 2 ] / M, where i=1, 2, ... n, and M is the filtered weight of the aluminum liquid.

8. A method for rapidly determining the type and content of inclusions in aluminum alloy melt according to claim 1, Features: In step S1, the aluminum alloy slag sample is sliced ​​into thin sheet alloy samples with a size of 15-20 mm*10-15 mm and a thickness of 10-15 mm. The size of the alloy sample to be tested after the thin sheet is embedded is φ25-φ40 mm and the thickness is 20-25 mm.

9. A method for rapidly determining the type and content of inclusions in an aluminum alloy melt according to claim 1, Features: In step S2, the grinding process is to use 800-2000 mesh diamond sandpaper and SiC sandpaper for 5-10 minutes, the polishing process is to use 0.05-5 μm diamond suspension for 10-15 minutes, and the cleaning process is to use water for 0.5-1 minute.

10. A method for rapidly determining the type and content of inclusions in aluminum alloy melt according to claim 1, Features: In step S2, the sample after grinding, polishing and cleaning has a mirror surface and no solvent residue.