Reference block for adjustable guide vane diffusion welding ultrasonic detection and application of reference block
By opening a flat bottom hole on the contrast test block of the adjustable guide blade and combining the water-immersed ultrasonic C scanning detection technology, the problem of insufficient sensitivity and accuracy of diffusion welding defect detection is solved, and the diffusion welding bonding surface of the adjustable guide blade is realized The efficient inspection ensures the reliability and accuracy of the inspection.
Patent Information
- Application Number
- CN202411300367.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
During diffusion welding, due to possible contamination on the welding surface or improper control of process parameters, defects in welding areas may appear in the welding area, and it is difficult for the prior art to effectively detect these defects, especially in adjustable guide vanes. Under complex structures and cavity structures, the detection sensitivity and accuracy are insufficient.
A comparison test block for adjustable guide blade diffusion welding ultrasonic detection was designed. By opening multiple flat bottom holes on the blade body, flat bottom holes are set on the detection platform when the bonding surface increases in the chord direction, water-immersed ultrasonic C is used. Scan detection technology forms a C-scan detection diagram, and intuitively judges the size and position of defects by comparing the detection results of the test block and actual parts to ensure the accuracy and reliability of the inspection.
Through the use of comparative test blocks, the sensitivity and accuracy of ultrasonic detection of diffusion welding can be effectively improved, ensuring accurate identification and quantitative evaluation of defects in diffusion welding of adjustable guide blades, avoiding the problem of incomplete detection coverage, and improving detection reliability.
Smart Images

Figure CN119086733A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nondestructive testing and discloses a comparison test block for ultrasonic testing of adjustable guide vane diffusion welding and application thereof. Background Art
[0002] Diffusion welding is to contact the surfaces of the workpieces to be welded under certain pressure and temperature conditions, and to make them tightly bonded through microscopic plastic deformation. The metal atoms at the interface diffuse with each other after a certain period of time to form an integral joint. Diffusion welding can achieve one-time large-area welding, small component deformation, high dimensional accuracy, and obtain joints with physical, chemical and mechanical properties equivalent to those of the parent material. Therefore, it plays a great role in precision welding, micro-connection, special material connection and other fields. At present, diffusion welding technology has been widely used in the forming of key components such as aircraft engine support plates and adjustable guide vanes.
[0003] If there is contamination on the diffusion welding surface or the process parameters such as temperature and pressure are not properly controlled, defects such as unwelded and weak bonding may occur in some areas of the diffusion welding joint surface. In order to ensure the quality of diffusion welding and ensure the safety of product use, it is particularly important to conduct reliable quality inspection and evaluation of diffusion welding welds.
[0004] A certain aircraft engine uses split diffusion welding to connect the two halves of the blade basin and blade back milling grooves into titanium alloy hollow adjustable guide vanes. The blade basin and blade back of the adjustable guide vane are first machined into blade profiles and grooves are milled in the core, and then diffusion welded together to form a cavity. The structural diagram is shown in the figure. Figure 1 As shown. Therefore, when ultrasonic testing is performed on the adjustable guide vane after diffusion welding, the adjustable guide vane has a complex structure cavity inside, and the ribs diffusely connected between the cavities are very narrow, with a width of only 2.5 mm. The diffusion welding joint surface has a curvature change, is not parallel to the incident surface of the sound beam, and has a continuously changing angle. The depth of the diffusion welding joint surface from the surface of the part also changes continuously. It is necessary to make a specific ultrasonic comparison test block and detection method to determine its detection sensitivity and detection plan. Summary of the invention
[0005] The purpose of the present invention is to provide a comparison test block for ultrasonic testing of adjustable guide vane diffusion welding and its application, which can obtain a comparison test block for ultrasonic testing of adjustable guide vanes with artificial defects. The comparison test block is used as a benchmark to determine the sensitivity and detection process of ultrasonic testing of adjustable guide vane diffusion welding. By comparing the test results of actual parts and the comparison test block, the size and position of the defects can be intuitively judged, thereby ensuring the accuracy and reliability of the detection.
[0006] In order to achieve the above technical effects, the technical solution adopted by the present invention is:
[0007] A comparative test block for ultrasonic testing of diffusion welding of adjustable guide vanes, comprising:
[0008] The blade body is a split structure, and the blade body is mainly composed of a blade basin petal body and a blade back petal body; the joint surface between the blade basin petal body and the blade back petal body is welded and formed by diffusion welding;
[0009] There are multiple flat-bottom holes, each of which has an opening located on the combining surface, and the bottom of the flat-bottom hole extends into the first petal body or the second petal body.
[0010] Furthermore, a cavity structure is also provided in the blade body, and the cavity structure is formed by a first groove and a second groove; the first groove extends from the joint surface to the blade basin body, and the second groove extends from the joint surface to the blade back body.
[0011] Furthermore, the center line of each flat-bottom hole is located on the normal line of the curved surface at the corresponding position of the bonding surface where the flat-bottom hole is located, and the diameter of each flat-bottom hole is 0.4-0.8 mm, the depth is 0.5-1 mm, and the position accuracy of the flat-bottom hole is Φ0.4 mm.
[0012] Furthermore, starting from the root position of the blade body, a flat-bottom hole is set at the center of the area where the blade diffusion welding joint surface increases in twist along the chord direction by one degree and the thickness from the joint surface to the upper surface of the detection part on the detection platform increases in the longitudinal direction by 1 to 5 mm.
[0013] In order to achieve the above technical effects, the present invention also provides a method for using the comparative test block to perform ultrasonic testing of adjustable guide vane diffusion welding, comprising:
[0014] A comparison test block of the same model as the adjustable guide vane to be tested is placed on the testing platform of the water immersion ultrasonic testing system; the adjustable guide vane to be tested is obtained by welding a vane basin body and a vane back body by diffusion welding;
[0015] The position of the immersion probe of the immersion ultrasonic testing system is adjusted so that the immersion probe is located directly above the comparison test block; the immersion depth of the probe is adjusted so that the focus of the immersion probe falls at the depth of the flat-bottom hole and the secondary interface echo is after the primary bottom echo;
[0016] Performing water immersion ultrasonic C-scan detection on the comparison test block to form a C-scan detection diagram, and fine-tuning the scanning parameters according to the display of the flat-bottom holes on the C-scan detection diagram, so that each flat-bottom hole on the comparison test block can be displayed on the C-scan detection diagram;
[0017] Placing the adjustable guide vane to be tested on the testing platform;
[0018] The water immersion ultrasonic C-scan test is performed on the adjustable guide vane to be tested using the finely adjusted scanning parameters to obtain a C-scan test image of the diffusion welding bonding surface of the adjustable guide vane to be tested.
[0019] Furthermore, when the comparison test block or the adjustable guide vane to be tested is placed on the testing platform, the corresponding blade basin petal body or blade back petal body is placed flat on the testing platform.
[0020] Furthermore, the center line of each flat-bottom hole is located on the normal line of the curved surface at the corresponding position of the bonding surface where the flat-bottom hole is located, and the diameter of each flat-bottom hole is 0.4-0.8 mm, the depth is 0.5-1 mm, and the position accuracy of the flat-bottom hole is Φ0.4 mm.
[0021] Furthermore, starting from the root position of the blade body, a flat-bottom hole is set at the center of the area where the blade diffusion welding joint surface increases in twist along the chord direction by one degree and the thickness from the joint surface to the upper surface of the detection part on the detection platform increases in the longitudinal direction by 1 to 5 mm.
[0022] Compared with the prior art, the present invention has the following beneficial effects: the present invention provides a comparison test block for ultrasonic welding detection of adjustable guide vanes with artificial defects by opening a flat-bottomed hole on the vane basin or the vane back of the blade body. The comparison test block is used as a reference to determine the sensitivity and detection process of ultrasonic detection of adjustable guide vane diffusion welding. The comparison test block and the actual parts of the adjustable guide vanes can also be detected at the same time. By comparing the detection results of the actual parts and the comparison test block, the size and position of the defect can be intuitively judged, thereby ensuring the accuracy and reliability of the detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Schematic diagram of the two petal structures of the comparison test block for the adjustable guide vane diffusion welding ultrasonic testing in the embodiment;
[0024] Figure 2 It is a schematic diagram of the structure of the comparative test block after welding of the adjustable guide vane diffusion welding ultrasonic test in the embodiment;
[0025] Figure 3 Schematic diagram of the reflection of the sound beam pulse during the ultrasonic testing of the adjustable guide vane diffusion welding by water immersion method in the embodiment;
[0026] Figure 4 A schematic diagram of waveforms generated during ultrasonic testing of adjustable guide vane diffusion welding by water immersion in an embodiment;
[0027] Figure 5 This is a C-scan test diagram of a comparison test block of a certain type of adjustable guide vane in the embodiment;
[0028] Figure 6 A C-scan detection diagram of one of the adjustable guide vanes of a certain type of adjustable guide vane in the embodiment;
[0029] Figure 7 A C-scan detection diagram of another adjustable guide vane of a certain type of adjustable guide vane in the embodiment;
[0030] Among them, 1. leaf basin petal body; 2. leaf back petal body; 3. joint surface; 4. flat bottom hole; 5. first groove; 6. second groove; 7. detection platform; 8. immersion probe. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with the embodiments and drawings. However, it should not be understood that the scope of the above subject matter of the present invention is limited to the following embodiments, and all technologies realized based on the content of the present invention belong to the scope of the present invention.
[0032] Example
[0033] See also Figure 1-Figure 4 , a comparison test block for ultrasonic testing of adjustable guide vane diffusion welding, comprising:
[0034] The blade body is a split structure, and the blade body is mainly composed of a blade basin petal body 1 and a blade back petal body 2; the joint surface 3 of the blade basin petal body 1 and the blade back petal body 2 is welded and formed by diffusion welding;
[0035] The flat-bottom hole 4 is multiple in number, each of the flat-bottom holes 4 has an opening located on the combining surface 3 , and the bottom of the flat-bottom hole 4 extends into the first petal body or the second petal body.
[0036] In this embodiment, a flat-bottomed hole 4 is provided on the blade basin petal body 1 or the blade back petal body 2 of the blade body to obtain a comparison test block for ultrasonic welding detection of an adjustable guide vane with artificial defects. The comparison test block is used as a reference to determine the sensitivity and detection process of ultrasonic detection of diffusion welding of adjustable guide vanes. The comparison test block and the actual parts of the adjustable guide vanes can also be tested at the same time. By comparing the test results of the actual parts and the comparison test block, the size and position of the defect can be intuitively judged, thereby ensuring the accuracy and reliability of the detection.
[0037] The comparison test block in this embodiment can be used to detect double-leaf solid blades or hollow blades. If the test sample is a hollow blade (such as an adjustable guide vane with a cavity), a corresponding cavity structure should be set in the blade body of the corresponding comparison test block, and the cavity structure is surrounded by a first groove 5 and a second groove 6; the first groove 5 extends from the joint surface 3 to the blade basin body 1, and the second groove 6 extends from the joint surface 3 to the blade back body 2. When making a comparison test block with a cavity structure, firstly, the blade profile is machined from the two half-blanks of the blade basin body 1 and the blade back body 2, and grooves (the first groove 5 or the second groove 6) are milled in the core, and a flat-bottom hole 4 is machined at a typical position of the blade basin body 1 or the blade back body 2, and then they are diffusion welded and assembled to form a comparison test block with a cavity structure.
[0038] To ensure the detection sensitivity and detection coverage, in this embodiment, starting from the root position of the blade body, a flat-bottom hole 4 is set at the center of the area where the blade diffusion welding joint surface 3 increases in chordal twist by one degree and the thickness of the upper surface of the detection part on the detection platform 7 from the joint surface 3 increases by 1 to 5 mm in the longitudinal direction. The location selection of the flat-bottom hole 4 comprehensively considers the influence of the curvature change of the joint surface 3 and the thickness of the joint surface 3 to the upper surface of the part on the high-frequency ultrasonic detection, and better covers the joint surface 3, ensuring that the simulation of the diffusion welding defects on the joint surface 3 is more comprehensive, and the detection sensitivity adjustment coverage is also wider, so that the defects on the joint surface 3 can be effectively detected and clearly displayed, avoiding the problem of incomplete detection coverage.
[0039] Based on the same inventive concept, this embodiment also provides a method for ultrasonic testing of adjustable guide vane diffusion welding using the comparative test block, and the specific testing process is as follows:
[0040] Step 1: Place a comparison test block of the same model as the adjustable guide vane to be tested on the testing platform 7 of the high-frequency water immersion ultrasonic testing system; the adjustable guide vane to be tested is obtained by welding the vane basin body 1 and the vane back body 2 by diffusion welding;
[0041] In this embodiment, the diameter of the flat-bottom hole 4 on the comparison test block is determined according to the part acceptance requirements, and should at least include the diameter of the flat-bottom hole 4 involved in the acceptance requirements, and the diameter tolerance is 0.01mm. If it is a comparison test block corresponding to an adjustable guide vane with a cavity structure, the flat-bottom hole 4 should cover the ribs and non-rib areas of the adjustable guide vane. At the same time, in order to ensure the detection sensitivity and detection coverage, starting from the root position of the blade body, a flat-bottom hole 4 is set at the center position of the area where the blade diffusion welding joint surface 3 increases along the chord direction for every degree of twist increase, and the thickness of the upper surface of the detection part from the joint surface 3 to the detection platform 7 increases by 1 to 5mm in the longitudinal direction; in order to make the flat-bottom hole 4 as close to the diffusion welding joint surface 3 as possible, the diameter of each of the flat-bottom holes 4 is 0.4 to 0.8mm, and the depth is 0.5 to 1mm; in order to better simulate the defects of the diffusion welding joint surface 3, the center line of each of the flat-bottom holes 4 is located on the normal of the surface corresponding to the position of the joint surface 3 where the flat-bottom hole 4 is located, and the position accuracy of the flat-bottom hole 4 is Φ0.4mm.
[0042] In addition, the placement of the comparison test block or the adjustable guide vane to be tested on the testing platform 7 can be that the vane base body 1 is placed on the testing platform 7, or that the vane back body 2 is in contact with the surface of the testing platform 7. However, no matter which placement method is used, it must be ensured that the comparison test block and the adjustable guide vane to be tested have the same structure in contact with the surface of the testing platform 7 to ensure data comparability.
[0043] Step 2: adjust the position of the immersion probe 8 of the immersion ultrasonic testing system so that the immersion probe 8 is located directly above the comparison test block; adjust the immersion depth of the probe so that the focus of the immersion probe 8 falls at the depth position of the flat-bottom hole 4, and the secondary interface echo is after the primary bottom echo;
[0044] In this embodiment, the ultrasonic detection of the adjustable guide vane diffusion weld joint adopts the pulse reflection method water immersion ultrasonic C-scan detection technology, and its detection principle is to use a focused water immersion probe 8 and a pulse reflection ultrasonic C-scan imaging automatic detection system to make the focus of the water immersion probe 8 as much as possible on the diffusion welding joint surface 3, and complete the defect imaging detection of the weld area by scanning. The weld area is determined by image processing software, and the defects are judged and quantitatively evaluated according to the C-scan display of the weld area and combined with the A-scan waveform.
[0045] like Figure 3 This is a schematic diagram of the longitudinal wave detection of the adjustable guide vane by water immersion method direct acoustic beam pulse reflection method. The waveform generated is as follows Figure 4 As shown in the figure, after the pulse (T) is transmitted, the first thing that appears is the sound wave reflected back from the interface between the water and the test piece after the ultrasonic wave passes through the water layer, that is, the primary interface echo (S1). Subsequently, if there is a defect, a defect echo (F) and a primary bottom surface echo (B1) will appear; if there is no defect, only the bottom surface echo (B1) and the secondary interface echo (S2) will appear. During the inspection, in order to facilitate defect identification, the water distance is adjusted so that the secondary interface echo (S2) of the probe is after the primary bottom surface echo (B1), and the initial wave is adjusted outside the display screen, and only the part after the interface echo is observed, and a "gate" is used to monitor whether there is a defect echo between S1 and B1, and all echo parameters are displayed in real time, such as burial depth, echo height (amplitude), equivalent size, etc.
[0046] Step 3: Perform water immersion ultrasonic C-scan detection on the comparison test block to form a C-scan detection image, and fine-tune the scanning parameters according to the display of the flat-bottom holes 4 on the C-scan detection image, so that each flat-bottom hole 4 on the comparison test block can be displayed on the C-scan detection image;
[0047] In this embodiment, for adjustable guide vanes with large thickness variations, a double-sided detection partition focusing method can be used to ensure that the sound beam covers the entire diffusion welding joint surface 3 and the detection sensitivity is sufficient. Figure 5 This is a C-scan test image of a certain type of adjustable guide vane comparison test block tested by a high-frequency water immersion ultrasonic testing equipment. The white dots in the image are the displayed images of the preset artificial defect flat-bottom hole 4.
[0048] Step 4: Place the adjustable guide vane to be tested on the testing platform 7, and ensure that the comparison test block and the adjustable guide vane to be tested are placed in the same position;
[0049] Step 5: Performing a water immersion ultrasonic C-scan test on the adjustable guide vane to be tested using the finely adjusted scanning parameters to obtain a C-scan test image of the diffusion welding bonding surface 3 of the adjustable guide vane to be tested;
[0050] In this embodiment, the same process and parameters are used to perform C-scan inspection on the adjustable guide vanes of the same specifications. When evaluating the defect image found on the C-scan inspection image, the flat-bottom hole 4 display in the same or close area of the ultrasonic comparison test block is selected as a reference benchmark to determine whether the defect display in the corresponding area of the adjustable guide vane to be tested exceeds the acceptance standard. Figure 6 This is an ultrasonic C-scan inspection image of an adjustable guide vane of the same specification in step 3. The diffusion welding joint surface 3 of the adjustable guide vane has a flaky diffusion welding defect. Figure 7 This is an ultrasonic C-scan inspection image of another adjustable guide vane of the same specification. The adjustable guide vane has a point-shaped diffusion welding defect on the diffusion welding joint surface 3.
[0051] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A comparative test block for ultrasonic testing of diffusion welding of adjustable guide vanes, characterized in that: include: The blade body is a split-type structure, and the blade body is mainly composed of a blade base petal body (1) and a blade back petal body (2); the joint surface (3) between the blade base petal body (1) and the blade back petal body (2) is formed by diffusion welding; A flat-bottom hole (4), wherein there are a plurality of the flat-bottom holes (4), the opening of each of the flat-bottom holes (4) is located on the combining surface (3), and the bottom of the flat-bottom hole (4) extends into the first petal body or the second petal body.
2. The comparison test block according to claim 1, characterized in that: A cavity structure is also provided in the blade body, and the cavity structure is formed by a first groove (5) and a second groove (6); the first groove (5) extends from the joint surface (3) to the inside of the blade base petal body (1), and the second groove (6) extends from the joint surface (3) to the inside of the blade back petal body (2).
3. The comparison test block according to claim 1, characterized in that: The center line of each flat-bottom hole (4) is located on the normal line of the curved surface at the corresponding position of the joint surface (3) where the flat-bottom hole (4) is located, and the diameter of each flat-bottom hole (4) is 0.4-0.8 mm, the depth is 0.5-1 mm, and the position accuracy of the flat-bottom hole (4) is Φ0.4 mm.
4. The comparison test block according to claim 1, characterized in that: Starting from the root position of the blade body, a flat bottom hole (4) is provided at the center of an area where the blade diffusion welding joint surface (3) increases in chordal twist by one degree and the thickness of the upper surface of the detection part on the detection platform (7) increases in the longitudinal direction by 1 to 5 mm.
5. The method for ultrasonic testing of adjustable guide vane diffusion welding using the comparison test block according to claim 1 is characterized in that: include: A comparison test block of the same model as the adjustable guide vane to be tested is placed on a testing platform (7) of a water immersion ultrasonic testing system; the adjustable guide vane to be tested is obtained by welding a vane basin body (1) and a vane back body (2) by diffusion welding; The position of the immersion probe (8) of the immersion ultrasonic detection system is adjusted so that the immersion probe (8) is located directly above the comparison test block; the immersion depth of the probe is adjusted so that the focus of the immersion probe (8) falls at the depth position of the flat bottom hole (4) and the secondary interface echo is after the primary bottom echo; Performing water immersion ultrasonic C-scan testing on the comparison test block to form a C-scan test image, and fine-tuning the scanning parameters according to the display of the flat-bottom holes (4) on the C-scan test image, so that each flat-bottom hole (4) on the comparison test block can be displayed on the C-scan test image; Placing the adjustable guide vane to be tested on the testing platform (7); The finely adjusted scanning parameters are used to perform water immersion ultrasonic C-scan testing on the adjustable guide vane to be tested, thereby obtaining a C-scan test image of the diffusion welding bonding surface (3) of the adjustable guide vane to be tested.
6. The method according to claim 5, characterized in that When the comparison test block or the adjustable guide vane to be tested is placed on the testing platform (7), the corresponding blade basin petal body (1) or blade back petal body (2) is placed flat on the testing platform (7).
7. The method according to claim 5, characterized in that The center line of each flat-bottom hole (4) is located on the normal line of the curved surface at the corresponding position of the joint surface (3) where the flat-bottom hole (4) is located, and the diameter of each flat-bottom hole (4) is 0.4-0.8 mm, the depth is 0.5-1 mm, and the position accuracy of the flat-bottom hole (4) is Φ0.4 mm.
8. The method according to claim 5, characterized in that Starting from the root position of the blade body, a flat bottom hole (4) is provided at the center of an area where the blade diffusion welding joint surface (3) increases in chordal twist by one degree and the thickness of the upper surface of the detection part on the detection platform (7) increases in the longitudinal direction by 1 to 5 mm.
Citation Information
Cited By
Numerical control machining method for hollow double-journal blade profile