AR film with excellent durability and preparation process thereof
By adopting a multi-layer structural design in the AR film, including the base layer, the upper coating layer, the base layer, the niobium oxide layer and the silicon-aluminum hybrid layer, the problem of insufficient durability of the existing AR film is solved and a higher degree of Hardness, wear resistance and high temperature resistance while maintaining excellent optical properties.
Patent Information
- Application Number
- CN202411221825.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-02
AI Technical Summary
While ensuring optical performance, the existing AR films have insufficient durability, especially wear resistance and high temperature resistance, resulting in insufficient use performance.
The AR film design adopts a multi-layer structure, including a base layer, an upper coating layer, a base layer, a first niobium oxide layer, a hafnium dioxide layer, a second niobium oxide layer, a silicon-aluminum hybrid layer and a scratch-resistant layer, through Control the thickness and material combination of each layer to improve the hardness, wear resistance and high temperature resistance of the AR film while maintaining excellent optical properties.
It significantly improves the overall durability of the AR film, including hardness, wear resistance and high temperature resistance, while maintaining excellent optical properties, enhancing its durability and stability in practical applications.
Smart Images

Figure CN119087557A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical films, and in particular relates to an AR film with excellent durability and a preparation process thereof. Background Art
[0002] AR film, also known as anti-reflection film, is a high-transmittance optical film that can reduce reflection and allow light to pass more completely. AR film can reduce or eliminate reflected light from optical surfaces such as prisms and plane mirrors, thereby increasing the light transmittance of these components and presenting the light to the user's eyes to the greatest extent. Due to the performance of AR film itself, it is usually applied to display device protection screens such as car displays, TVs, computers, mobile phones, tablets and other electronic products that increase transmittance and reduce reflectivity. AR film can effectively increase the glass transmittance of these electronic products and reduce the glass reflectivity.
[0003] At present, the performance of AR film focuses more on transmittance and reflectivity, while other physical properties such as wear resistance and high temperature resistance will also affect its durability, but there are few corresponding studies. Therefore, how to improve the durability of AR film while ensuring optical performance is a problem that needs to be further solved.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] The purpose of the present invention is to provide an AR film with excellent durability and a preparation process thereof. The AR film has excellent wear resistance and high temperature resistance and has high durability.
[0006] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0007] An AR film with excellent durability comprises a substrate layer, on which an upper coating layer, a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer and an anti-scratch layer are sequentially arranged;
[0008] Wherein, a hafnium dioxide layer is provided between the first niobium oxide layer and the silicon dioxide layer, or a hafnium dioxide layer is provided between the second niobium oxide layer and the silicon-aluminum mixed layer;
[0009] The thickness of the hafnium dioxide layer is 1-20 nm.
[0010] In one or more embodiments of the present invention, the base material is selected from one or more of SiO2, Ti, Si, Al, MgF2, SiO, Sn and Y; and / or,
[0011] The thickness of the base layer is 0.1-10 nm.
[0012] In one or more embodiments of the present invention, the thickness of the first niobium oxide layer is 5-200 nm.
[0013] In one or more embodiments of the present invention, the silicon dioxide layer has a thickness of 10 to 260 nm.
[0014] In one or more embodiments of the present invention, the thickness of the second niobium oxide layer is 5-280 nm.
[0015] In one or more embodiments of the present invention, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2) based on silicon and aluminum atoms; and / or,
[0016] The thickness of the silicon-aluminum mixed layer is 50-310 nm.
[0017] In one or more embodiments of the present invention, the substrate layer is selected from one of a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer; and / or,
[0018] The thickness of the substrate layer is 5.7-250 μm.
[0019] In one or more embodiments of the present invention, a lower coating layer is further provided on the surface of the substrate layer away from the upper coating layer, the upper coating layer has a thickness of 50 to 500 nm, and the lower coating layer has a thickness of 0.2 to 4.1 μm.
[0020] In one or more embodiments of the present invention, the anti-scratch layer has a thickness of 2 to 190 nm.
[0021] Another specific embodiment of the present invention provides a technical solution as follows:
[0022] A process for preparing AR with excellent durability comprises the following steps:
[0023] A lower coating layer and an upper coating layer are coated on both sides of the substrate layer, and a high-temperature protective film is provided on the lower coating layer;
[0024] A primer layer, a first niobium oxide layer, a hafnium dioxide layer, a silicon dioxide layer, a second niobium oxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; or a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a hafnium dioxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer;
[0025] coating an anti-scratch layer on the silicon-aluminum mixed layer;
[0026] A positive protective film is provided on the anti-scratch layer.
[0027] Compared with the prior art, the AR film of the present invention exhibits superior hardness, wear resistance and high temperature resistance, while having excellent optical properties and overall high durability. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 Schematic diagram of the structure of the AR film with excellent durability in Example 1 of the present invention;
[0030] Figure 2 Schematic diagram of the structure of an AR film with excellent durability in Example 5 of the present invention;
[0031] Figure 3 It is a comparison chart of the reflection curves of 1380-780nm of Example 1, Example 5 and Comparative Example of the present invention;
[0032] Figure 4 It is a comparison chart of the reflection curves of Example 1, Example 5 and the comparative example at 1400-700nm of the present invention.
[0033] Description of main reference numerals:
[0034] 1-high temperature protective film, 2-lower coating layer, 3-substrate layer, 4-upper coating layer, 5-base layer, 6-first niobium oxide layer, 7-hafnium dioxide layer, 8-silicon dioxide layer, 9-second niobium oxide layer, 10-silicon aluminum mixed layer, 11-anti-scratch layer, 12-positive protective film. DETAILED DESCRIPTION
[0035] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0036] A specific embodiment of the present invention provides an AR film with excellent durability, comprising a substrate layer, on which an upper coating layer, a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer and an anti-scratch layer are sequentially arranged; wherein a hafnium oxide layer is arranged between the first niobium oxide layer and the silicon dioxide layer or a hafnium oxide layer is arranged between the second niobium oxide layer and the silicon-aluminum mixed layer; the thickness of the hafnium oxide layer is 1 to 20 nm.
[0037] Specifically, the base layer can improve the adhesion of the AR film, the first niobium oxide layer can increase the transmittance of the AR film, the silicon dioxide layer can reduce reflection, the second niobium oxide layer further increases the transmittance, the silicon-aluminum mixed layer further reduces reflection and can also improve the weather resistance of the AR film. The combination of the base layer, the first niobium oxide layer, the silicon dioxide layer, the second niobium oxide layer and the silicon-aluminum mixed layer can ensure that the AR film has better optical properties.
[0038] Hafnium dioxide has excellent scratch resistance and high temperature resistance, and exhibits excellent optical properties in terms of transparency, refractive index and luminescence performance. By setting a hafnium dioxide layer between the first niobium oxide layer and the silicon dioxide layer or between the second niobium oxide layer and the silicon-aluminum mixed layer, the surface hardness, wear resistance and high temperature resistance of the AR film can be effectively improved, while the overall optical properties of the AR film are not affected, and the overall durability is excellent.
[0039] In a specific embodiment, the base layer material is selected from one or more of SiO2, Ti, Si, Al, MgF2, SiO, Sn and Y; the thickness of the base layer is 0.1 to 10 nm.
[0040] Specifically, SiO2 (silicon dioxide), Ti (titanium), Si (silicon), Al (aluminum), MgF2 (magnesium fluoride), SiO (silicon monoxide), Sn (tin) and Y (yttrium) are selected to make the base layer, which can effectively improve the adhesion of the AR film.
[0041] In a specific embodiment, the thickness of the first niobium oxide layer is 5 to 200 nm, the thickness of the silicon dioxide layer is 10 to 260 nm, and the thickness of the second niobium oxide layer is 5 to 280 nm.
[0042] Specifically, the layer thickness will affect the optical properties of the AR film. When the layer thickness is too small, the expected optical properties cannot be obtained. Although increasing the layer thickness helps to improve the optical properties of the AR film, when the layer thickness is too large, the optical properties will gradually deteriorate. Therefore, by controlling the layer thickness, the optical properties of the AR film can be improved.
[0043] In a specific embodiment, the molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2) based on silicon and aluminum atoms; and the thickness of the silicon-aluminum mixed layer is 50-310 nm.
[0044] Specifically, the silicon-aluminum mixed layer is located on the surface of the AR film, and has a more obvious effect on the uniformity of the coating. Selecting a silicon-aluminum mixed target for coating can improve the stability of the coating and make the coating more uniform, thereby ensuring the overall optical stability of the AR film.
[0045] In a specific embodiment, the substrate layer is selected from one of a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer; and the thickness of the substrate layer is 5.7 to 250 μm.
[0046] Specifically, the PET layer is a polyethylene terephthalate layer, the PI layer is a polyimide layer, the SRF layer is a super-reflective polyester film, the TAC layer is a triacetyl cellulose layer, the COP layer is a cycloolefin polymer layer, and the PC layer is a polycarbonate layer. Selecting the above types of substrate layers can make the AR film have a stable structure and optical properties.
[0047] In a specific embodiment, a lower coating layer is further provided on the surface of the substrate layer away from the upper coating layer, the upper coating layer has a thickness of 50 to 500 nm, and the lower coating layer has a thickness of 0.2 to 4.1 μm.
[0048] Specifically, the lower coating layer and the upper coating layer are both formed by coating an acrylic resin coating liquid, which is an existing product. By coating the acrylic resin coating liquid, the hardness, wear resistance and high temperature resistance of the AR film can be improved.
[0049] In one specific embodiment, the anti-scratch layer has a thickness of 2 to 190 nm.
[0050] Specifically, the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid, which is an existing product and its main component is perfluoropolyether polymer. The anti-scratch layer is located on the surface of the AR film and can effectively improve the anti-oil, anti-fingerprint and anti-scratch properties of the AR film.
[0051] Another specific embodiment of the present invention provides a process for preparing an AR film with excellent durability, comprising the following steps:
[0052] A lower coating layer and an upper coating layer are coated on both sides of the substrate layer, and a high-temperature protective film is provided on the lower coating layer;
[0053] A primer layer, a first niobium oxide layer, a hafnium dioxide layer, a silicon dioxide layer, a second niobium oxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; or a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a hafnium dioxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer;
[0054] An anti-scratch layer is coated on the silicon-aluminum mixed layer, and a positive protective film is disposed on the anti-scratch layer.
[0055] Specifically, the high temperature protection film and the positive protection film are both PET films, the high temperature protection film has a thickness of 30 to 188 μm, and the positive protection film has a thickness of 30 to 188 μm. Conventional magnetron sputtering technology is used to plate each coating layer.
[0056] The present invention is further described in detail below in conjunction with specific embodiments.
[0057] Example 1
[0058] like Figure 1 As shown, the AR film with excellent durability includes, from bottom to top, a high-temperature protective film with a thickness of 30μm, a lower coating layer with a thickness of 2μm, a substrate layer with a thickness of 125μm, an upper coating layer with a thickness of 200nm, a primer layer with a thickness of 10nm, a first niobium oxide layer with a thickness of 5nm, a hafnium dioxide layer with a thickness of 1nm, a silicon dioxide layer with a thickness of 10nm, a second niobium oxide layer with a thickness of 5nm, a silicon-aluminum mixed layer with a thickness of 50nm, a scratch-resistant layer with a thickness of 2nm, and a positive protective film with a thickness of 40μm.
[0059] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0060] Example 2
[0061] The AR film with excellent durability includes, from bottom to top, a high-temperature protective film with a thickness of 100μm, a lower coating layer with a thickness of 0.2μm, a substrate layer with a thickness of 38μm, an upper coating layer with a thickness of 50nm, a primer layer with a thickness of 0.1nm, a first niobium oxide layer with a thickness of 90nm, a hafnium dioxide layer with a thickness of 10nm, a silicon dioxide layer with a thickness of 260nm, a second niobium oxide layer with a thickness of 280nm, a silicon-aluminum mixed layer with a thickness of 170nm, a scratch-resistant layer with a thickness of 190nm, and a positive protective film with a thickness of 40μm.
[0062] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is a PET layer, the base material is Y, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 85:15 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0063] Example 3
[0064] The AR film with excellent durability includes, from bottom to top, a high-temperature protective film with a thickness of 188μm, a lower coating layer with a thickness of 4.1μm, a substrate layer with a thickness of 250μm, an upper coating layer with a thickness of 500nm, a primer layer with a thickness of 6nm, a first niobium oxide layer with a thickness of 200nm, a hafnium dioxide layer with a thickness of 20nm, a silicon dioxide layer with a thickness of 130nm, a second niobium oxide layer with a thickness of 120nm, a silicon-aluminum mixed layer with a thickness of 310nm, a scratch-resistant layer with a thickness of 100nm, and a positive protective film with a thickness of 40μm.
[0065] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is TAC layer, the base material is Ti, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0066] Example 4
[0067] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 20nm thick hafnium dioxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0068] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0069] Example 5
[0070] like Figure 2 As shown, the AR film with excellent durability includes, from bottom to top, a high-temperature protective film with a thickness of 30μm, a lower coating layer with a thickness of 2μm, a substrate layer with a thickness of 125μm, an upper coating layer with a thickness of 200nm, a primer layer with a thickness of 10nm, a first niobium oxide layer with a thickness of 5nm, a silicon dioxide layer with a thickness of 10nm, a second niobium oxide layer with a thickness of 5nm, a hafnium dioxide layer with a thickness of 1nm, a silicon-aluminum mixed layer with a thickness of 50nm, a scratch-resistant layer with a thickness of 2nm, and a positive protective film with a thickness of 40μm.
[0071] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0072] Example 6
[0073] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 20nm thick hafnium dioxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0074] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0075] Comparative Example 1
[0076] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0077] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0078] Comparative Example 2
[0079] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 0.3nm thick hafnium dioxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0080] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0081] Comparative Example 3
[0082] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 40nm thick hafnium dioxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0083] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0084] Comparative Example 4
[0085] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 0.3nm thick hafnium dioxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0086] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0087] Comparative Example 5
[0088] The AR film with excellent durability includes, from bottom to top, a 30μm thick high-temperature protective film, a 2μm thick lower coating layer, a 125μm thick substrate layer, a 200nm thick upper coating layer, a 10nm thick primer layer, a 5nm thick first niobium oxide layer, a 10nm thick silicon dioxide layer, a 5nm thick second niobium oxide layer, a 40nm thick hafnium dioxide layer, a 50nm thick silicon-aluminum mixed layer, a 2nm thick anti-scratch layer and a 40μm thick positive protective film.
[0089] Among them, the materials of the high-temperature protective film and the positive protective film are both PET, the lower coating layer and the upper coating layer are both formed by coating acrylic resin coating liquid, the substrate layer is PI layer, the base material is SiO, the silicon-aluminum mixed layer has a silicon-aluminum molar ratio of 98:2 based on silicon-aluminum atoms, and the anti-scratch layer is formed by coating AF anti-fingerprint coating liquid.
[0090] The AR films in the examples and comparative examples were prepared by the above-mentioned preparation method, and their performances were tested.
[0091] (1) The total light transmittance and 400-700 nm spectrophotometer light transmittance of the AR films in Example 1, Example 5 and Comparative Example 1 were tested. The results are shown in Table 1.
[0092] Table 1 Optical transmittance test results
[0093]
[0094] (2) The reflection curves of the AR films in Example 1, Example 5 and Comparative Example 1 at 380-780 nm and 400-700 nm were tested. The results are as follows: Figure 3 and Figure 4 As shown, Figure 3 and Figure 4 In the figure, the old scheme refers to comparative example 1, the existing scheme 1 refers to example 1, and the existing scheme 2 refers to example 5.
[0095] (3) Place the AR film on the glass panel and divide it into three sections, left, middle and right, according to the width of the film surface. Use a pencil hardness tester with a weight of 500g and 750g respectively, and use a 3H hardness pencil and a 4H hardness pencil to test the hardness of the coating surface. Draw 5 lines at each position during the test, and record the number of lines without scratches among the 5 lines. Result judgment: If there are 3 or more (including 3) lines without scratches among the 5 lines, it is judged as OK, and if there are less than 3 lines, it is judged as NG. The results are shown in Table 2.
[0096] Table 2 Pencil hardness test results
[0097]
[0098]
[0099] (4) Steel wool wear test: The AR film was placed on a glass panel and the wear tester was loaded with 1000 g. The number of scratches after 2000, 3000 and 5000 frictions was recorded. A scratch number ≥ 4 was judged as NG and a scratch number ≤ 3 was judged as OK. The results are shown in Table 3.
[0100] Table 3 Steel wool wear test results
[0101]
[0102]
[0103]
[0104] (4) The back of the AR film was bonded with OCA optical adhesive and then bonded to the transparent glass. After bonding, the film was degassed with a degassing machine. After degassing, the surface was wiped clean. The AR film was then boiled in 100°C water for 3h and 5h, placed at double 85 (i.e., high temperature 85°C, high humidity 85%) for 32 days and 36 days, placed at 95°C for 32 days and 36 days, placed at -40°C for 32 days and 36 days, and exposed to sunlight (light intensity 0.55w / (m 2 ·nm), wavelength 340nm, filter Extended UV-Q / B, 3.8h of light + 1h of darkness as one cycle. The temperature of the blackboard during the light exposure was set at 89℃, the temperature of the box was 63℃, and the humidity was 50%; the temperature of the box and blackboard was set at 38℃ and the humidity was 95% during the dark stage) for 32 days and 36 days, and then a hundred grids were cut with a hundred grid knife, and then 3M company 681 type tape was used. After pressing and sticking, the tape was pulled off after standing for more than 30s. No peeling was 5B, slight peeling was 3-4B, barely OK, and NG was judged below 2B. The results are shown in Table 4.
[0105] Table 4 Comparison of various environmental tests
[0106]
[0107]
[0108] As can be seen from Table 1, the total light transmittance of the AR film in Example 1, Example 5 and Comparative Example 1 can reach more than 95%, and the light transmittance of the 400-700nm spectrophotometer can reach more than 93%, which meets the qualified requirements. According to the optical test requirements, the average reflectivity of 380-780nm is less than 1.0%, and the average reflectivity of 400-700nm is less than 0.5%. Figure 2 It can be seen that within 380-780nm, the average reflectivity of Example 1 is 0.70%, the average reflectivity of Example 5 is 0.70%, and the average reflectivity of Comparative Example 1 is 0.76%. Figure 3 It can be seen that within 400-700 nm, the average reflectivity of Example 1 is 0.24%, the average reflectivity of Example 5 is 0.25%, and the average reflectivity of Comparative Example 1 is 0.25%. It can be seen that the AR films in Example 1, Example 5 and Comparative Example 1 all have good optical effects, indicating that the optical performance of the AR film in the present invention meets the requirements.
[0109] It can be seen from Tables 2 and 3 that the AR film in the embodiment of the present invention has better hardness and wear resistance, indicating that the present invention can effectively improve the surface hardness and wear resistance of the AR film while ensuring that the overall optical properties of the AR film are not affected by adding a hafnium dioxide layer in the AR film. It can be seen from Table 4 that the AR film in the present invention also exhibits better high temperature resistance, and the overall durability is greatly improved.
[0110] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0111] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. An AR film with excellent durability, It is characterized in that It comprises a substrate layer, on which an upper coating layer, a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a silicon-aluminum mixed layer and an anti-scratch layer are sequentially arranged; Wherein, a hafnium dioxide layer is provided between the first niobium oxide layer and the silicon dioxide layer, or a hafnium dioxide layer is provided between the second niobium oxide layer and the silicon-aluminum mixed layer; The thickness of the hafnium dioxide layer is 1-20 nm.
2. The AR film having excellent durability according to claim 1, It is characterized in that The base material is selected from SiO 2 、Ti、Si、Al、MgF 2 , SiO, Sn and Y; and / or, The thickness of the base layer is 0.1-10 nm.
3. The AR film having excellent durability according to claim 1, It is characterized in that The first niobium oxide layer has a thickness of 5 to 200 nm.
4. The AR film having excellent durability according to claim 1, It is characterized in that The thickness of the silicon dioxide layer is 10 to 260 nm.
5. The AR film having excellent durability according to claim 1, It is characterized in that The second niobium oxide layer has a thickness of 5 to 280 nm.
6. The AR film having excellent durability according to claim 1, It is characterized in that The molar ratio of silicon to aluminum in the silicon-aluminum mixed layer is (85-98): (15-2) based on silicon and aluminum atoms; and / or The thickness of the silicon-aluminum mixed layer is 50-310 nm.
7. The AR film having excellent durability according to claim 1, It is characterized in that The substrate layer is selected from one of a PET layer, a PI layer, a SRF layer, a TAC layer, a COP layer and a PC layer; and / or, The thickness of the substrate layer is 5.7-250 μm.
8. The AR film having excellent durability according to claim 1, It is characterized in that A lower coating layer is also provided on the surface of the substrate layer away from the upper coating layer. The upper coating layer has a thickness of 50 to 500 nm, and the lower coating layer has a thickness of 0.2 to 4.1 μm.
9. The AR film having excellent durability according to claim 1, It is characterized in that The anti-scratch layer has a thickness of 2 to 190 nm.
10. A process for preparing an AR film with excellent durability as claimed in any one of claims 1 to 9, It is characterized in that The following steps are involved: A lower coating layer and an upper coating layer are coated on both sides of the substrate layer, and a high-temperature protective film is provided on the lower coating layer; A primer layer, a first niobium oxide layer, a hafnium dioxide layer, a silicon dioxide layer, a second niobium oxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; or a primer layer, a first niobium oxide layer, a silicon dioxide layer, a second niobium oxide layer, a hafnium dioxide layer and a silicon-aluminum mixed layer are sequentially plated on the upper coating layer; coating an anti-scratch layer on the silicon-aluminum mixed layer; A positive protective film is provided on the anti-scratch layer.
Citation Information
Patent Citations
Scratch-resistant transparent film and preparation method thereof
CN107422402A
Anti-reflection film, preparation method, anti-reflection optical product and application
CN111999785A
Anti-reflection laminate and application and preparation method thereof
CN114966910A
AR film, element and device
CN117488262A
High-weather-resistance high-reflection film and preparation process thereof
CN118465899A