Light absorber and method for manufacturing same
By combining carbon nanotubes with epoxy resin, a carbon nanotube network structure is formed and connected to carbon particles through spraying process, the problem of unstable performance of light absorbers in harsh environments is solved, and efficient and stable light absorption is achieved Effects, suitable for aerospace and other fields.
Patent Information
- Application Number
- CN202411132135.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing light absorbers exhibit unstable performance in harsh environments and are difficult to maintain consistent performance under conditions such as mechanical stress, extreme temperatures, ultraviolet radiation and water impact, which limits their application in aerospace, military and other fields.
Carbon nanotubes are combined with epoxy resin to form a carbon nanotube network structure, and connected to carbon particles through spraying process to enhance the durability and stability of the light absorber, and form a light absorber on the substrate.
Achieves a wide spectral range absorption efficiency of more than 99.9% in harsh environments, significantly improves the durability and stability of the light absorber, ensures consistent performance under conditions such as mechanical wear, extreme temperatures, ultraviolet radiation and water shock, and Low cost and suitable for mass production.
Smart Images

Figure CN119087562A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a light absorber and a preparation method thereof, and in particular to a light absorber based on carbon nanotubes and a preparation method thereof. Background Art
[0002] Light absorbers have a wide range of applications in areas including energy harvesting, stray light shielding, and stealth technology. In the design and fabrication of perfect light absorbers, there is often a trade-off between enhancing the density of micro-nanostructures for light absorption and improving the durability and stability of materials. This dichotomy may limit the wider application of these light absorbers, especially under harsh environmental conditions. Currently, there is an urgent need to design perfect light absorbers that can withstand extreme environments, including mechanical stress, extreme temperatures, strong ultraviolet radiation, and other severe challenges. These light absorbers are critical for applications that require consistent performance in harsh environments, such as in aerospace, military operations, and special industries. Summary of the invention
[0003] In view of this, it is indeed necessary to provide a light absorber and a preparation method thereof having excellent light absorption performance, excellent durability and stability in harsh environments.
[0004] A light absorber comprises a plurality of carbon nanotubes, a plurality of carbon particles and an epoxy resin, wherein the plurality of carbon nanotubes form a carbon nanotube network structure, the epoxy resin is coated on the surface of the plurality of carbon nanotubes, and the plurality of carbon particles are connected through the carbon nanotube network structure coated with the epoxy resin.
[0005] A method for preparing a light absorber comprises the following steps: providing a light absorber prefabricated liquid, wherein the light absorber prefabricated liquid comprises a solvent, a plurality of carbon nanotubes, a plurality of carbon particles and an epoxy resin, wherein the plurality of carbon nanotubes form a carbon nanotube network structure, and the plurality of carbon nanotubes and the carbon particles are suspended in the solvent in a colloidal state; and spraying the light absorber prefabricated liquid on a substrate to form the light absorber.
[0006] Compared with the prior art, the light absorber provided by the present invention exhibits excellent absorption efficiency in harsh environmental conditions, exceeding 99.9% over a wide spectrum range. The method and structure of combining carbon nanotubes with epoxy resin as connectors between carbon particles significantly enhances the durability and stability of the light absorber, ensuring consistent performance even under mechanical wear, extreme temperatures, ultraviolet radiation, water shock and long-term outdoor conditions. Moreover, the preparation method of the light absorber adopts a spraying process, which is low in cost and can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1This is a top view SEM image of the light absorber spray layer provided in an embodiment of the present invention, with a scale of 500 μm.
[0008] Figure 2 This is a SEM image of a cross section of a light absorber spray coating provided in an embodiment of the present invention, with a scale of 20 μm.
[0009] Figure 3 This is a SEM image of the side surface of the light absorber spray layer provided in the embodiment of the present invention, with a scale of 500 μm.
[0010] Figure 4 This is an enlarged SEM image of the light absorber spray layer provided in an embodiment of the present invention from a top view, with a scale of 50 μm.
[0011] Figure 5 This is an enlarged SEM image of a top view of the light absorber spray layer provided in an embodiment of the present invention, with a scale of 10 μm.
[0012] Figure 6 SEM image of the sprayed carbon nanotube-carbon black composite without epoxy resin, the scale bar is 20 μm.
[0013] Figure 7 This is a TEM image of carbon nanotubes and epoxy resin dispersed in an ethanol solution provided by an embodiment of the present invention, with a scale of 100 nm.
[0014] Figure 8 A schematic flow chart of a method for preparing a light absorber provided in an embodiment of the present invention.
[0015] Fig. 9 It is the reflection spectrum of the light absorber provided by the present invention within the visible light wavelength range.
[0016] Fig.10 It is the reflection spectrum of the light absorber provided by the present invention in the near-infrared wavelength range.
[0017] Fig.11 It is the reflection spectrum of the light absorber provided by the present invention in the mid-infrared wavelength range.
[0018] Fig.12 The functional relationship between the mirror reflectivity and the incident angle of the light absorber provided by the present invention is measured using non-polarized light with a wavelength of 550nm.
[0019] Fig.13 The light absorber provided by the present invention has a hemispherical reflection spectrum within the visible light wavelength range measured by an integrating sphere.
[0020] Fig.14The hemispherical reflection spectrum of the light absorber provided by the present invention is measured by an integrating sphere within the near-infrared wavelength range.
[0021] Fig.15 This is the reflection spectrum of the light absorber provided by the present invention measured when the incident angle is 15°.
[0022] Fig.16 This is the reflection spectrum of the light absorber provided by the present invention measured when the incident angle is 30°.
[0023] Fig.17 This is the reflection spectrum of the light absorber provided by the present invention measured when the incident angle is 45°.
[0024] Fig.18 This is the reflection spectrum of the light absorber provided by the present invention measured when the incident angle is 60°.
[0025] Fig.19 This is a schematic diagram of the bonding mechanism between carbon black particles and carbon nanotubes added with epoxy resin in the light absorber spray layer provided by the present invention.
[0026] Fig. 20 Schematic diagram of the comparison before and after the scratched area of the light absorber spray layer is adhered with tape in an embodiment of the present invention.
[0027] Fig.21 This is a photo of the wear track of the carbon nanotube-CB particle layer without epoxy resin added after 500 wear cycles in the embodiment of the present invention.
[0028] Fig. 22 This is a microscope image of the wear track of the carbon nanotube-CB particle layer without epoxy resin added in the embodiment of the present invention after 500 wear cycles.
[0029] Fig.23 This is a photograph of the wear track of the light absorber spray layer provided in an embodiment of the present invention after 500 wear cycles.
[0030] Fig.24 A microscope image of the wear track of the light absorber spray coating provided in an embodiment of the present invention after 500 wear cycles.
[0031] Fig.25 It is a schematic diagram of using sandpaper to perform a linear wear test on the light absorber spray layer provided by an embodiment of the present invention.
[0032] Fig.26 Schematic diagram of preparing a spray coating on cloth as a light absorber.
[0033] Fig. 27This is a schematic diagram of testing the mirror reflectivity of the light absorber spray layer of this embodiment under harsh environment with a wavelength of 550nm.
[0034] Main component symbols
[0035] none
[0036] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0037] The light absorber and the method for preparing the light absorber provided by the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0038] An embodiment of the present invention provides a light absorber, which includes a plurality of carbon nanotubes, a plurality of carbon particles and an epoxy resin. The plurality of carbon nanotubes form a carbon nanotube network structure, the epoxy resin is coated on the surface of the plurality of carbon nanotubes, and the plurality of carbon particles are connected by the epoxy resin and the carbon nanotube network structure. That is, the plurality of carbon particles are connected by the carbon nanotube network structure coated with epoxy resin, the carbon particles are wrapped by the carbon nanotubes and the epoxy resin, and there are gaps between the carbon nanotube-carbon particle aggregates. Adding epoxy resin to the light absorber significantly enhances the connection between the carbon nanotubes and the carbon particles, and the addition of epoxy resin significantly strengthens the interface bonding between the carbon nanotubes and the carbon particles. The carbon nanotubes may be single-walled carbon nanotubes, double-walled carbon nanotubes or multi-walled carbon nanotubes. The carbon particles may be carbon particles with a diameter ranging from 100 nm to 100 um, and the epoxy resin may be various alcohol-soluble epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, novolac epoxy resin, and multifunctional glycidyl ether epoxy resin.
[0039] Furthermore, the light absorber may also include a substrate for supporting the light absorber. The type, shape, thickness, etc. of the substrate are not limited. The substrate may be quartz, polymer, metal, ceramic, or cloth, etc. The surface of the substrate may be a plane, a curved surface, or an irregular surface. In this embodiment, the substrate is quartz.
[0040] Furthermore, the light absorber may also include a curing agent, which is selected according to the corresponding epoxy resin and may be aliphatic amine, aromatic amine, polyamide, etc.
[0041] In this embodiment, the light absorber includes a plurality of carbon nanotubes, a plurality of carbon particles, an epoxy resin and a curing agent. The carbon nanotubes are multi-walled carbon nanotubes with an average diameter of 20 nanometers. The carbon particles are carbon black (CB) particles, the epoxy resin is E51, and the curing agent is diethylenetriamine.
[0042] like Figure 1 As shown, the morphology of the light absorber spray coating of this embodiment is very similar to the light absorber spray coating without epoxy resin, the carbon black particles are evenly dispersed on the surface of the light absorber, and the carbon nanotube-carbon black composite material widely covers the light absorber spray coating. This observation shows that by adding appropriate epoxy resin and curing agent, a carbon nanotube-CB particle composite coating can be manufactured by a spray coating process. This method maintains the full carbon nanomaterial system and its surface morphology, lays the foundation for superior absorption characteristics, and ensures the stability and durability of the light absorber spray coating.
[0043] like Figure 2 As shown, a cross-sectional view of the light absorber spray coating reveals that the CB particles are encapsulated by carbon nanotubes and epoxy resin. The light absorber composite is closely arranged to establish a layered structure, a configuration that is like bricks bonded with mortar, in which the CB particles are connected by a carbon nanotube network integrated with the resin. Such a network gives the light absorber spray coating strong mechanical properties and stability. Figure 3 The side view SEM image of the light absorber spray coating presented in the figure depicts an undulating and uniform topography with gaps between carbon nanotube-CB aggregates. These gaps are tens of nanometers, which is very advantageous for light absorption in the visible to infrared spectrum. In addition, from the perspective of light absorber design, the integration of CB particles enhances the scattering and absorption capabilities of the light absorber surface. Figure 4 As shown, the surface morphology of the light absorber spray coating is characterized by stacked carbon nanotube-CB particle composites with gaps between them. The integration of these particles, especially in all-carbon nanomaterials, effectively increases the gap density in the local area. This increase in gap density effectively reduces the equivalent refractive index of the light absorber surface, thereby promoting the reduction of reflection. In addition, the addition of epoxy resin to the carbon nanotube-CB particle composite produces unique properties not observed in the resin-free layer, such as Figure 5 The presence of epoxy resin gives the carbon nanotube-CB particles a smoother surface texture, indicating that the carbon nanotubes and CB particles are completely wrapped by the resin. This feature is shown in Figure 6 This is further demonstrated by the images of the resin-free spray coating presented in .
[0044] Carbon nanotubes exhibit high efficiency as absorbers and connectors connecting carbon particles within light absorber coatings, creating multi-scale, all-carbon-based nanomaterials.
[0045] It can be understood that the light absorber can be composed of a plurality of carbon nanotubes (CNTs), a plurality of carbon particles and epoxy resin.
[0046] In addition, an embodiment of the present invention provides a method for preparing a light absorber, which comprises the following steps:
[0047] S1, providing a light absorber prefabricated liquid, the light absorber prefabricated liquid comprising a solvent, a plurality of carbon nanotubes, a plurality of carbon particles and epoxy resin, the plurality of carbon nanotubes forming a network structure, the carbon nanotubes and the carbon particles are suspended in the solvent in a colloidal state.
[0048] In the light absorber preform solution, carbon nanotubes and carbon particles showed the ability to remain stable for a long time, sometimes even for months, without forming aggregates.
[0049] S2, spraying the light absorber prefabricated liquid onto a substrate to form a light absorber.
[0050] In step S1, the method for preparing the light absorber prefabricated liquid comprises the following steps:
[0051] S11, providing a plurality of carbon nanotubes;
[0052] S12, dispersing the plurality of carbon nanotubes in a solvent and performing flocculation treatment to obtain a carbon nanotube suspension;
[0053] S13, adding epoxy resin and carbon particles into the carbon nanotube suspension, performing ultrasonic dispersion, and forming a light absorber prefabricated liquid.
[0054] In step S11, the preparation method of carbon nanotubes is not limited, for example, arc discharge method, laser evaporation method, or chemical vapor deposition method, etc. In this embodiment, the carbon nanotubes are prepared by chemical vapor deposition method, which includes the following steps:
[0055] S111, growing a carbon nanotube array on a growth substrate; and
[0056] S112, using a blade or other tool to scrape the carbon nanotube array off the growth substrate to obtain a plurality of carbon nanotubes.
[0057] In step S111, the lengths of the plurality of carbon nanotubes in the carbon nanotube array are not limited. Preferably, the length of the carbon nanotubes is greater than 100 μm (micrometer). The plurality of carbon nanotubes are substantially parallel to each other and substantially perpendicular to the surface of the growth substrate. The carbon nanotube array provided in this embodiment is one of a single-walled carbon nanotube array, a double-walled carbon nanotube array, and a multi-walled carbon nanotube array.
[0058] In this embodiment, the preparation method of the carbon nanotube array adopts chemical vapor deposition, and its specific steps include: (a) providing a flat growth substrate, which can be a P-type or N-type silicon substrate, or a silicon substrate with an oxide layer formed thereon. In this embodiment, an 8-inch silicon substrate is preferably used; (b) a catalyst layer is uniformly formed on the surface of the growth substrate, and the catalyst layer material can be iron (Fe), cobalt (Co), nickel (Ni) or any combination of alloys thereof; (c) the growth substrate with the catalyst layer formed thereon is annealed in air at 700°C to 900°C for about 30 minutes to 90 minutes; (d) the treated growth substrate is placed in a reaction furnace, heated to 500°C to 740°C under a protective gas environment, and then a carbon source gas is introduced to react for about 5 minutes to 30 minutes to grow a carbon nanotube array, the height of which is greater than 100 microns. The carbon nanotube array is a pure carbon nanotube array formed by a plurality of carbon nanotubes that grow parallel to each other and perpendicular to the growth substrate. Since the generated carbon nanotubes are relatively long, some of the carbon nanotubes may be entangled with each other. By controlling the growth conditions, the carbon nanotube array contains substantially no impurities, such as amorphous carbon or residual catalyst metal particles, etc. In this embodiment, the carbon source gas can be acetylene or other chemically active hydrocarbons, and the protective gas can be nitrogen, ammonia or an inert gas.
[0059] In step S12, the plurality of carbon nanotubes are dispersed in a solvent, and the flocculation treatment can be carried out by ultrasonic dispersion treatment or high-intensity stirring to obtain a carbon nanotube suspension. Preferably, the plurality of carbon nanotubes are dispersed in an ethanol solvent and ultrasonic dispersion is used for 10 to 30 minutes. Since the carbon nanotubes have a large specific surface area and there is a large van der Waals force between the carbon nanotubes entangled with each other, the flocculation treatment does not completely disperse the carbon nanotubes in the carbon nanotube raw material in the solvent. The carbon nanotubes are attracted and entangled with each other through van der Waals forces to form a network structure, which can also be called a flocculent structure. In this embodiment, the carbon nanotubes are dispersed in an ethanol solution, and the carbon nanotubes are interconnected to form a network structure. It is crucial to maintain the colloidal suspension state of the carbon nanotubes in the ethanol solvent. A higher concentration of carbon nanotubes may increase the viscosity of the solution, thereby possibly damaging the subsequent spraying process, while a lower concentration of carbon nanotubes may reduce the efficiency of the preparation of the light absorber. Preferably, 0.1-0.8 grams of carbon nanotubes are dispersed in every 200 milliliters of ethanol.
[0060] In step S12, preferably, a dispersant may be added during the process of dispersing the plurality of carbon nanotubes into a solvent, and then an ultrasonic cell disruptor is used to perform tip ultrasonic dispersion of the carbon nanotubes to form a carbon nanotube suspension.
[0061] In step S13, after epoxy resin is added to the carbon nanotube suspension and fully mixed, the epoxy resin is evenly distributed among the carbon nanotubes, such as Figure 7As shown. Obviously, the carbon nanotubes are surrounded by epoxy resin, and the epoxy resin accumulates at the joints of the carbon nanotubes to form a uniform composite material of carbon nanotubes and epoxy resin, which is critical to the structural integrity and performance of the light absorber. Epoxy resin is added to the carbon nanotube suspension as a binder, and the dispersion of carbon nanotubes in epoxy resin is critical to enhancing the stability and durability of the light absorber. The use of appropriate dispersion technology can ensure that the epoxy resin is evenly distributed throughout the carbon nanotube suspension, thereby maximizing the interaction between the carbon nanotubes and the epoxy resin, thereby improving the performance of the light absorber. In this embodiment, the epoxy resin uses E51, which can be dissolved in various organic solvents including ethanol, and the concentration of E51 is 0.1-0.4 grams per 200 milliliters.
[0062] Since the amount of resin added to the carbon nanotube suspension is relatively small, the basic properties of the carbon nanotube suspension are not substantially changed, which ensures that the subsequently sprayed light absorber is still mainly composed of carbon nanomaterials, thereby retaining the light capture and absorption properties of the light absorber.
[0063] Add carbon particles to the carbon nanotube suspension so that the mass ratio of carbon nanotubes to carbon particles is 4:5 to 4:70. The content of the solvent can be adjusted according to actual conditions to ensure that the light absorber prefabricated liquid can be sprayed. Preferably, the solvent is 200 mL, the carbon nanotubes are 0.4 g, and the carbon particles are 0.5 g to 7 g. The carbon nanotubes are well dispersed in the ethanol solution, and most of the carbon nanotubes are separated as individuals.
[0064] Preferably, a curing agent may be added to the carbon nanotube suspension. The curing agent is selected according to the corresponding epoxy resin and may be aliphatic amine, aromatic amine, polyamide, and the like.
[0065] In step S2, the spraying method is not limited, and a spray gun can be used for spraying. The diameter of the spray gun is 1 mm, the carrier gas is nitrogen with a pressure of 0.3Mpa, the effective spray range is about 150 mm, and the solution consumption is 100 ml per minute. The spraying process is carried out in a closed exhaust hood. The sample is taken out when the surface is completely dry a few minutes after spraying. No subsequent heating process is required, and finally a spray layer as a light absorber is formed. The spray layer is characterized by its ultra-light property and a density as low as 3.6×10 -6 g / mm2, a property that is particularly advantageous in space or military operations.
[0066] See also Figure 8 This embodiment provides a method for preparing a light absorber, which specifically includes the following steps:
[0067] First, a carbon nanotube array with a height of 285 microns was grown on an 8-inch silicon wafer and then scraped off the silicon wafer.
[0068] Next, 0.4 g of the carbon nanotubes were placed in 200 ml of ethanol solvent, PVP was added, and the concentration of PVP was 0.1 g of PVP per 200 ml of ethanol solvent, and ultrasonic cell disruptor was used to perform ultrasonic flocculation treatment to obtain a carbon nanotube suspension. In this embodiment, each carbon nanotube is multi-walled and has an average diameter of 20 nanometers.
[0069] Then, epoxy resin E51 was added to the carbon nanotube suspension, 0.2 g of E51 was added per 200 ml of ethanol solvent, followed by an additional 30 minutes of ultrasonic dispersion to enhance the bonding between the carbon nanotubes and epoxy resin E51. After that, 7 g of carbon black particles were added to the carbon nanotube suspension, and diethylenetriamine was added as a curing agent to obtain a stable light absorber preform.
[0070] Finally, the light absorber prefabricated liquid is sprayed on a substrate to form a light absorber, and the spraying is performed using a spray gun.
[0071] To quantitatively evaluate the performance of the epoxy-containing spray coating as an absorber, we acquired reflectance spectra in the wavelength range from 400 nm to 20 μm. Considering the lack of periodic or geometric surface features on the sprayed carbon nanotube surface, the reflectance behavior is expected to be independent of the polarization state of the incident light. The reflectance spectra of the prepared light absorber spray coating at normal incidence are shown in detail. Figures 9 to 11 Considering that the measurement equipment and comparison criteria of reflectance spectra in different studies may vary, especially in the case of low-reflectance measurements, carbon nanotube arrays were chosen as the reference for reflectance measurements over the entire wavelength range in the current work as the most efficient light absorber.
[0072] like Fig. 9As shown, the carbon nanotube spray coating without carbon black particles and integrated with epoxy resin exhibited a nearly uniform reflectivity of approximately 0.19% in the visible wavelength region. This represents a moderate reduction compared to the reflectivity of 0.32% for the pure carbon nanotube layer prepared previously. The reduction in reflectivity is attributed to the introduction of epoxy resin, which increases the surface roughness and thus reduces the specular reflection. As a benchmark, the 285-micron-tall carbon nanotube array measured by the equipment used in this study exhibited a reflectivity of 0.05%. By systematically increasing the amount of carbon black particles added per 200 ml of carbon nanotube solution - from 3 grams to 7 grams - a gradual decrease in the reflectivity of the light absorber spray coating was observed. Notably, the minimum reflectivity of 0.063% was achieved after adding 7 grams of carbon black particles, a value very close to the reflectivity level of the absorber model of the carbon nanotube array. In addition, since both carbon nanotubes and CB particles are composed of all-carbon nanomaterials, integrating epoxy resin into the mixture does not negatively affect the light absorption capacity. Therefore, the reflective properties of the light absorber sprayed coating show remarkable consistency in the visible spectrum.
[0073] In the infrared wavelength range, such as Fig.10 and Fig.11 As shown, the reflectance spectra show a similar decreasing trend with the increase of the number of CB particles. The introduction of epoxy resin does not change this trend, corresponding to the near-infrared (NIR) and mid-infrared (MIR) wavelength ranges. For wavelengths above 1 micron, the carbon nanotube arrays show a minimum reflectivity of 0.02%, establishing a reference benchmark. With the gradual increase of the carbon black content in the carbon nanotube suspension, the reflectivity of the spray coating containing 7 grams of CB particles and epoxy resin reaches about 0.05% in the near-infrared range. This performance is comparable to that of the carbon nanotube-CB composite without epoxy resin, indicating that the presence of epoxy resin does not significantly affect the absorption characteristics of the light absorber in this wavelength range.
[0074] With increasing CB particle concentration, the reflectivity of the CNT-7g CB particle composite spray coating with epoxy resin reached about 0.05% in the near-infrared range. This performance is comparable to that of the CNT-CB particle composite without epoxy resin. In addition, in the mid-infrared (MIR) range, the CNT arrays showed an unusually low reflectivity of 0.005%, demonstrating the uniformity of its absorption capacity. The CNT-7g CB particle spray coating with the addition of epoxy resin reached a reflectivity of 0.01%. The trend of the reflectivity change remained consistent in the visible, near-infrared and mid-infrared wavelength ranges. These observations strongly suggest that the addition of epoxy resin does not have a negative impact on the absorption efficiency of the CNT-CB particle composite light absorber. Even with the addition of epoxy resin, the light absorption performance of the CNT-CB light absorber remains consistently strong in the visible, near-infrared and mid-infrared wavelength ranges. This performance is comparable to that of vertically aligned carbon nanotube (VA carbon nanotube) arrays.
[0075] In practical applications, achieving omnidirectional absorption is a key characteristic of light absorbers, which is a significant challenge for existing technologies. In order to evaluate the stability of the omnidirectional light reflection performance of the epoxy-containing spray coating, such as Figure 15-18 As shown in Figure 1, reflectance spectra were obtained at incident angles of 0° to 60° in the visible wavelength range. The reflectance measurements for all samples were found to be consistent, regardless of the incident angle, demonstrating the excellent omni-directional absorption capability of the epoxy-containing carbon nanotube-CB particle composite spray coating in the visible spectrum. At a wavelength of 550 nanometers, the specular reflectance at different incident angles is shown in Figure 1. Fig.12 As shown, close to the midpoint of the visible spectrum. The addition of epoxy resin plays an important role in maintaining the surface morphology of the carbon nanotube-CB particles, which is essential to ensure the strong absorption performance of the carbon nanomaterials in the spray coating. At an incident angle of 60°, the reflectivity of the spray coating increased slightly from 0.05% at normal incidence to 0.09%, suggesting that the absorptivity of the spray coating may exceed 99.9%. The addition of epoxy resin maintains the scattering centers and gaps between the carbon black particles on the surface of the carbon nanotube spray coating, which is beneficial to light absorption. Carbon nanotubes added with epoxy resin are not only crucial for light absorption, but also important for more effective bonding of carbon black particles.
[0076] In order to evaluate the overall absorption performance of the spray coating in the visible and near-infrared wavelength range, the hemispherical reflectance spectrum was measured using an integrating sphere. The carbon nanotube array is highly efficient in promoting light absorption, and the hemispherical reflectance is always below 0.5%. Previous studies have shown that adding carbon black particles to the carbon nanotube spray coating will form a combination of micrometer-scale fluctuations and nanometer-scale gaps on the surface, resulting in a hemispherical reflectance of 0.75%. It can be demonstrated experimentally that the addition of epoxy resin can maintain the surface morphology of the carbon nanotube-carbon black particle spray coating, retaining the key micrometer-scale and nanometer-scale gaps that contribute to light capture and absorption. Fig.13 , Fig.14 As shown, the hemispherical reflectance of the spray coating with epoxy added reached 0.74% in the visible range and 0.85% in the near-infrared range. These results show that the performance is comparable to that of the spray coating without epoxy added, indicating that it is independent of wavelength.
[0077] like Fig.19 As shown, before encapsulating the CB particles to form the composite, the CNTs were coated with epoxy resin, which strengthened their role as a binder between the CB particles. This treatment made the CNTs more robust, effectively “fixing” the micro- and nanostructures after the curing process. The epoxy-coated CNTs provided a large amount of support for the CB particles, significantly enhancing the mechanical stability and durability of the composite. First, the addition of epoxy resin did not change the morphology of the sprayed coating, thereby maintaining the excellent absorption characteristics of all carbon nanomaterials, as established in previous experiments. Second, the epoxy resin facilitated the cross-linking and physical entanglement between the CNT-CB particles, providing forces beyond the van der Waals forces and greatly enhancing the mechanical properties of the sprayed coating. When the CNTs were impregnated with the resin, they acted as strong connectors between the carbon black particles, a property that is critical for the large-scale preparation of light absorbers. This addition is essential for changing the surface morphology and strengthening the interconnections between the CNT-CB particles. Finally, this preparation process is very suitable for large-scale applications via the spray coating method.
[0078] The perfect light absorber for harsh environments is conceptualized as an ideal material that can efficiently absorb most of the incident light. It is designed to maintain its structural integrity and performance without degradation under the harsh conditions typically encountered in these environments. In order to determine the adhesion performance of the light absorber spray coating, the varnish cross-cut test standardized to ASTM D3359 was used. The initial step is to create a 1×1 square millimeter grid on the light absorber spray coating using a cross-cut tester, ensuring complete penetration to the substrate. Afterwards, a tape (3M brand) is firmly adhered to the scratched area and then quickly removed, and this process is repeated until there is no detectable residue on the tape. This ensures a comprehensive evaluation of the adhesion performance. Subsequently, the peeling behavior within the grid squares is carefully examined, such as Fig. 20As shown. There was no residue on the tape after the final iteration, confirming the strong adhesion of the light absorber spray layer to the substrate. Adhesion testing showed that the light absorber spray layer adhered firmly to the substrate, achieving an adhesion grade of 5B according to the ASTM D3359 standard. This excellent adhesion is mainly attributed to the strong binding ability of the carbon nanotube-CB particles encapsulated within the epoxy resin. This interconnected network not only ensures the strong adhesion of the light absorber spray layer, but also maintains the stability of the micro- and nanostructures. Maintaining this stability is critical for all carbon nanomaterials to effectively capture and absorb radiation, making them ideal absorbers.
[0079] Furthermore, wear analysis tests were performed to evaluate the mechanical durability of the sprayed coatings. The tests started with a ball-on-disk sliding test, performed using a universal micro-tribometer (UMT-5, Bruker) in linear mode. The light absorber containing 7 g of CB particles was sprayed on a steel ball and paired with a bearing ball with a diameter of 4 mm and a hardness of 700 HV. Before the test, the bearing ball was ultrasonically cleaned in an acetone and ethanol bath for 10 minutes to eliminate any residual contaminants. The friction test was performed under a normal load of 0.5 N, at a frequency of 1 Hz over a range of 7 mm, for a total of 500 cycles. The purpose of this method is to examine the tribological behavior of the material. To ensure the reliability of the results, the test was performed three times to ensure repeatability and was carried out at ambient conditions of 23 °C. The steel ball passed through the surface at a frequency of 1 Hz to form a wear track to evaluate the wear resistance, such as Figure 21-24 As shown. Compared with the wear track of the carbon nanotube-CB particle layer without epoxy resin, the wear track of the light absorber spray layer of this embodiment is significantly shallower, indicating that the light absorber spray layer with epoxy resin added has better wear resistance. In contrast, the steel substrate is exposed in the wear track of the carbon nanotube-CB particle layer without epoxy resin added. The addition of epoxy resin leads to a significant reduction in wear marks, reflecting the contribution of epoxy resin to improving the wear resistance of the light absorber spray layer.
[0080] In order to fully evaluate the mechanical durability and wear resistance of the light absorber spray coating, a wear analysis test was performed using sandpaper. The test was performed using 800 grit sandpaper under a load of 100 g. Fig.25 As shown. After 100 wear cycles, the spray coating showed continued stability and strong adhesion without obvious damage or detachment. A significant advantage of the spray coating process is that the light absorber preform liquid can be formed on a substrate with a curved surface, irregular shape or uneven surface. Fig.26 As shown, the light absorber preformed liquid can be effectively sprayed onto the cloth substrate to produce a large-scale flexible absorber with excellent mechanical stability. This feature means that the light absorber spray layer integrated with the resin can withstand the severe test of friction and wear in practical applications.
[0081] The present invention also conducted a thermal shock test to evaluate the ability of the light absorber spray coating to withstand sudden and extreme temperature changes. This evaluation is crucial to determine the thermal stability and structural integrity of the material, especially for applications in industries such as aerospace, electronics and ceramics, which often encounter rapid temperature changes. The test began with the light absorber spray coating being coated on a steel substrate and then exposed on a 150°C hot plate for two hours. Throughout the heating process, the light absorber spray coating showed excellent stability and did not show any signs of detachment or damage. Subsequently, a thermal cycling test was conducted to further evaluate the thermal shock resistance of the light absorber spray coating. This test involves alternating exposure of the sample at 150°C and immersion in liquid nitrogen. After the substrate is uniformly heated to 150°C, the light absorber spray coating is quickly immersed in liquid nitrogen, and after a short interval, the sample is placed back on the 150°C hot plate and the process is repeated. The results of this test show that the light absorber spray coating maintains significant thermal shock resistance during rapid temperature changes. This is mainly due to the thermal stability of the carbon nanomaterial and epoxy resin composite material in the layer. The absence of cracks, deformations, or other damage indicative of temperature-induced stress confirms the suitability of the light absorber spray coating for environments with frequent and sudden temperature fluctuations.
[0082] UV irradiation is used to evaluate the photodegradation resistance of the light absorber spray coating, which is critical to ensure the protection of the spray coating against UV and solar radiation. 2 After exposing the light absorber spray coating to UV radiation for two hours at a light power density of 1.5 Å, the spray coating maintained its durability and reflectivity measurements showed stability. This result is consistent with previous studies that have shown that the light absorption properties of carbon nanomaterials are essentially unaffected in the UV wavelength range. The epoxy resin used in the present invention exhibits remarkable resistance to UV radiation, giving the spray coating excellent UV stability. In addition, from another perspective, when carbon nanotubes and carbon black particles are integrated into epoxy resin, they can act as UV stabilizers and absorbers. This dual role helps protect the epoxy resin from the harmful effects of UV radiation.
[0083] In addition, water impact testing was performed to evaluate the ability of the light absorber spray coating to withstand the forces associated with high-velocity water impact, which is critical for applications that may be exposed to such conditions. The water pressure was set to approximately 2kg / mm 2and applied to the substrate using a nozzle. Throughout the testing process, the light absorber spray coating showed excellent durability, and any residual moisture easily evaporated, allowing the light absorber spray coating to be restored to its original state without any observable damage or delamination. To further enhance the evaluation, the light absorber spray coating was also subjected to a 10-hour water immersion test. After immersion, the light absorber spray coating was dried and tactilely inspected, and no signs of detachment were found. Under these rigorous water exposure conditions, the light absorber spray coating has shown excellent durability and reliability in practical applications.
[0084] Finally, a realistic evaluation of the outdoor stability and durability of the light absorber spray coating when installed on a vehicle was conducted. The light absorber spray coating was attached to the front windshield of the vehicle, which was operated under standard conditions and exposed to various weather elements, including wind, rain and solar radiation. After a 30-day test period, the light absorber spray coating maintained its durability.
[0085] like Fig. 27 As shown, under harsh environment, the mirror reflectivity of the light absorber spray layer of this embodiment is tested with a wavelength of 550nm, and the reflectivity measurement shows that the performance is consistent.
[0086] The light absorber provided by the present invention exhibits excellent absorption efficiency in harsh environmental conditions, exceeding 99.9% over a wide spectrum range. The carbon nanotubes are combined with epoxy resin as connectors between carbon particles. This method and structure significantly enhances the durability and stability of the light absorber, ensuring consistent performance even under mechanical wear, extreme temperatures, ultraviolet radiation, water shock and long-term outdoor conditions. Moreover, the spraying process is adopted, which is low in cost and can be mass-produced.
[0087] In addition, those skilled in the art may also make other changes within the spirit of the present invention. Of course, these changes made according to the spirit of the present invention should be included in the scope of protection required by the present invention.
Claims
1. A light absorber, comprising a plurality of carbon nanotubes, a plurality of carbon particles and an epoxy resin, wherein the plurality of carbon nanotubes form a carbon nanotube network structure, the epoxy resin is coated on the surface of the plurality of carbon nanotubes, and the plurality of carbon particles are connected through the carbon nanotube network structure coated with the epoxy resin.
2. The light absorber according to claim 1, It is characterized in that There are gaps between the carbon nanotube-carbon particle aggregates.
3. The light absorber according to claim 1, It is characterized in that The light absorber further includes a curing agent.
4. The light absorber according to claim 1, It is characterized in that The light absorber further includes a substrate, the plurality of carbon nanotubes, the plurality of carbon particles and the epoxy resin are located on the surface of the substrate, and the surface of the substrate is a plane, a curved surface, or the substrate has an irregular surface.
5. The light absorber according to claim 1, It is characterized in that The light absorber consists of a plurality of carbon nanotubes, a plurality of carbon particles and epoxy resin.
6. The light absorber according to claim 1, It is characterized in that A mass ratio of the plurality of carbon nanotubes to the plurality of carbon particles is 4:5 to 4:
70.
7. A method for preparing a light absorber, wherein The following steps are involved: Providing a light absorber prefabricated liquid, the light absorber prefabricated liquid comprising a solvent, a plurality of carbon nanotubes, a plurality of carbon particles and an epoxy resin, wherein the plurality of carbon nanotubes form a carbon nanotube network structure, and the plurality of carbon nanotubes and carbon particles are suspended in the solvent in a colloidal state; The light absorber prefabricated liquid is sprayed on a substrate to form a light absorber.
8. The method for preparing a light absorber according to claim 7, It is characterized in that The method for preparing the light absorber prefabricated liquid comprises the following steps: providing a plurality of carbon nanotubes; dispersing the plurality of carbon nanotubes in a solvent and performing flocculation treatment to obtain a carbon nanotube suspension; Adding epoxy resin and carbon particles into the carbon nanotube suspension and performing ultrasonic dispersion to form a light absorber prefabricated liquid.
9. The method for preparing a light absorber according to claim 7, It is characterized in that The mass ratio of the carbon nanotubes to the carbon particles is 4:5 to 4:
70.
10. The method for preparing a light absorber according to claim 7, It is characterized in that The concentration of the epoxy resin is 0.1-0.4 g of epoxy resin per 200 ml of solvent.
Citation Information
Patent Citations
Reinforced interphase and bonded structures thereof
CA2817987A1
Light absorber and method for manufacturing same
CN114624798A