Preparation method of heterogeneous bonding device with controllable bonding interface thickness, heterogeneous bonding device and electro-optical modulator

By bonding the photoelectric thin film material chip to the wafer oxide layer, the die-wafer form from chip to wafer is formed, which solves the problem of incompatibility of photonic system modulators and CMOS processes, and realizes the industrial application of large-scale photoelectric integrated chips and high-performance signal transmission.

CN119087583APending Publication Date: 2024-12-06INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410990828.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing photonic system modulators are incompatible with the CMOS process, making it difficult to achieve large-scale mass production photonic integrated circuits, and the traditional die-die bonding method is difficult to achieve true photoelectron monolithic integration.

Method used

Using the preparation method of hetero-bonding devices with controllable bonding interface thickness, the die-wafer form of chip to wafer is formed by bonding the photoelectric thin film material chip to the wafer oxide layer, and the industry of large-scale photoelectric integrated chips is realized. application. The method includes growing buried oxygen layer, waveguide layer and metal electrode on the wafer, and controlling the thickness and structure of the bonding interface through plasma enhanced chemical vapor deposition and low-pressure chemical vapor deposition, thereby avoiding photoelectric thin film materials etching and alignment error problems.

Benefits of technology

It realizes a high-performance optoelectronic monolithic integrated system that is compatible with the CMOS process, with large bandwidth, low light insertion loss and high extinction ratio, which is suitable for large-scale production and realizes single-wave 200G signal transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119087583A_ABST
    Figure CN119087583A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a heterogeneous bonding device with controllable bonding interface thickness, the heterogeneous bonding device and an electro-optical modulator, and relates to the technical field of photoelectricity. The preparation method of the heterogeneous bonding device comprises the following steps: providing a photoelectric film material chip; providing a wafer, wherein the wafer comprises a wafer oxide layer; and bonding the photoelectric thin film material chip with the wafer oxide layer. The electro-optical modulator comprises the heterogeneous bonding device. According to the heterogeneous bonding device, a chip-to-wafer form is adopted, so that a real optoelectronic monolithic integration system can be realized, and the industrial application of a real large-scale optoelectronic integrated chip can be realized. The heterogeneous bonding device is used for manufacturing the electro-optical modulator at the 3dB bandwidth gt; 110GHz, half-wave voltage lt; therefore, signal transmission of 200G of single wave is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of optoelectronic technology, and in particular to a method for preparing a heterogeneous bonding device with controllable bonding interface thickness, a heterogeneous bonding device and an electro-optic modulator. Background Art

[0002] In the future, photonic systems require modulators to have driving voltages compatible with CMOS technology (CMOS refers to complementary metal oxide semiconductor, which is the most mainstream and mature set of chip processes), large bandwidth, low optical insertion loss, high extinction ratio, excellent signal quality and compatibility with large-scale manufacturing. However, modulators in the existing technology are incompatible with CMOS technology, and all use chip-to-chip (die-die) bonding, which makes it difficult to achieve large-scale mass production of photonic integrated circuits. Summary of the invention

[0003] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.

[0004] To this end, a first aspect of the present invention provides a method for preparing a heterogeneous bonding device with controllable bonding interface thickness, comprising:

[0005] Provide optoelectronic thin film material chips;

[0006] Providing a wafer; wherein the wafer comprises a wafer oxide layer;

[0007] The photoelectric thin film material chip is bonded to the wafer oxide layer.

[0008] In a feasible implementation manner, the wafer preparation method includes:

[0009] growing a first buried oxide layer on the first substrate;

[0010] Etching the first buried oxide layer to form a first etching groove;

[0011] growing a waveguide layer at the first etched groove;

[0012] growing a second buried oxide layer on the first buried oxide layer and the waveguide layer;

[0013] Etching the second buried oxide layer and the first buried oxide layer to form a second etching groove, wherein the second etching groove is spaced apart from the first etching groove;

[0014] Making a metal electrode at the second etching groove;

[0015] A third buried oxide layer is grown on the second buried oxide layer and the metal electrode; wherein the third buried oxide layer is the wafer oxide layer.

[0016] In a feasible implementation manner, the wafer preparation method includes:

[0017] growing a first buried oxide layer on the first substrate;

[0018] Etching the first buried oxide layer to form a first etching groove;

[0019] growing a waveguide layer at the first etched groove;

[0020] growing a second buried oxide layer on the first buried oxide layer and the waveguide layer;

[0021] Etching the second buried oxide layer and the first buried oxide layer to form a second etching groove, wherein the second etching groove is spaced apart from the first etching groove;

[0022] Making a metal electrode at the second etching groove;

[0023] growing a third buried oxide layer on the second buried oxide layer and the metal electrode;

[0024] bonding a second substrate on the third buried oxide layer;

[0025] The first substrate is removed to expose the first buried oxide layer; wherein the first buried oxide layer is the wafer oxide layer.

[0026] In a feasible implementation manner, the method for growing the first buried oxide layer on the first substrate is plasma enhanced chemical vapor deposition, and the thickness of the first buried oxide layer is 150nm to 400nm;

[0027] The method for growing the second buried oxide layer on the first buried oxide layer and the waveguide layer is plasma enhanced chemical vapor deposition, and the thickness of the second buried oxide layer is 400nm to 900nm;

[0028] The method for growing the third buried oxide layer on the second buried oxide layer and the metal electrode is plasma enhanced chemical vapor deposition, and the thickness of the third buried oxide layer is 2000nm-5000nm.

[0029] In a feasible implementation manner, the method for growing the waveguide layer at the first etched groove is low pressure chemical vapor deposition, and the thickness of the waveguide layer is 100 nm to 300 nm.

[0030] In a feasible implementation manner, the method for manufacturing the metal electrode at the second etching groove is a magnetron sputtering method or an evaporation method, and the thickness of the metal electrode is 500nm to 1500nm.

[0031] In a feasible implementation manner, bonding the optoelectronic thin film material chip to the wafer oxide layer includes:

[0032] Cleaning the photoelectric thin film material chip, wherein the photoelectric thin film material chip comprises a photoelectric thin film material layer, a photoelectric thin film material chip buried oxide layer and a photoelectric thin film material chip substrate;

[0033] activating the photoelectric thin film material layer and the wafer oxide layer;

[0034] The photoelectric thin film material layer is brought into contact with the wafer oxide layer at room temperature for bonding, and pressure annealing is applied after bonding;

[0035] Applying a protective layer, removing the photoelectric thin film material chip substrate, and then removing the protective layer;

[0036] Growing a heterogeneous bonding device oxide layer so that the heterogeneous bonding device oxide layer covers the optoelectronic thin film material chip buried oxide layer and the wafer oxide layer;

[0037] The thickness of the oxide layer of the heterogeneous bonding device is maintained to a desired thickness.

[0038] In a feasible implementation manner, the thickness of the oxide layer of the heterogeneous bonding device is retained to be 1 μm to 3 μm.

[0039] A second aspect of the present invention provides a heterogeneous bonding device, which is prepared by using the above-mentioned method for preparing a heterogeneous bonding device with controllable bonding interface thickness.

[0040] A third aspect of the present invention provides an electro-optic modulator, comprising the above-mentioned heterojunction bonding device.

[0041] Compared with the prior art, the present invention has at least the following beneficial effects:

[0042] The present invention provides a method for preparing a heterogeneous bonding device with controllable bonding interface thickness. Different from the traditional die-die bonding type heterogeneous bonding device, it adopts the form of chip to wafer (die-wafer), which is conducive to realizing a truly optoelectronic monolithic integrated system and realizing the industrial application of truly large-scale optoelectronic integrated chips. The heterogeneous bonding device is used to make an electro-optic modulator, and a single-wave 200G signal transmission is achieved when the 3dB bandwidth is >110GHz and the half-wave voltage is <3V. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0044] Figure 1 One of the flow charts for preparing a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0045] Figure 2 A second flow chart of preparing a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0046] Figure 3 A third flow chart of the preparation of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0047] Figure 4 A fourth flow chart of a preparation process of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0048] Figure 5 A fifth flow chart of the preparation of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0049] Figure 6 Figure 6 of the preparation flow chart of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0050] Figure 7 A seventh flow chart of a preparation process of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0051] Figure 8 FIG8 is a flow chart of preparing a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0052] Fig. 9 A ninth flow chart of a preparation process of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application;

[0053] Fig.10 The tenth flowchart of the preparation of a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0054] Fig.11 One of the preparation flow charts for bonding a photoelectric thin film material to a wafer oxide layer in a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0055] Fig.12The second preparation flow chart of bonding between optoelectronic thin film material and wafer oxide layer in a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0056] Fig.13 The third preparation flow chart of bonding between optoelectronic thin film material and wafer oxide layer in a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0057] Fig.14 A fourth preparation flow chart of bonding between a photoelectric thin film material and a wafer oxide layer in a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0058] Fig.15 The fifth preparation flow chart of bonding between optoelectronic thin film material and wafer oxide layer in a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application.

[0059] Fig.16 The sixth preparation flow chart of bonding of optoelectronic thin film material and wafer oxide layer in a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present application is as follows: Fig.16 It is also a schematic diagram of a heterogeneous bonding device with controllable bonding interface thickness prepared in Example 1 of the present application.

[0060] Fig.17 Schematic diagram of the overall structure of the optoelectronic thin film material chip and the oxide layer of the wafer bonded together according to an embodiment of the present application.

[0061] Fig.18 The heterogeneous bonding device with controllable bonding interface thickness of Example 1 is used to make a curve of electro-optic response variation with frequency of an electro-optic modulator.

[0062] The corresponding relationship between the reference numerals and the component names is as follows:

[0063] 1. First substrate; 2. First buried oxide layer; 3. First etching groove; 4. Waveguide layer; 5. Second buried oxide layer; 6. Second etching groove; 7. Metal electrode; 8. Third buried oxide layer; 9. Second substrate; 10. Photoelectric thin film material layer; 11. Photoelectric thin film material chip buried oxide layer; 12. Photoelectric thin film material chip substrate; 13. Protective layer; 14. Heterogeneous bonding device oxide layer. DETAILED DESCRIPTION

[0064] In order to better understand the above-mentioned technical scheme, the technical scheme of the embodiments of the present application is described in detail below through the accompanying drawings and specific embodiments. It should be understood that the embodiments of the present application and the specific features in the embodiments are detailed descriptions of the technical scheme of the embodiments of the present application, rather than limitations on the technical scheme of the present application. In the absence of conflict, the embodiments of the present application and the technical features in the embodiments may be combined with each other.

[0065] According to a first aspect of an embodiment of the present invention, there is provided a method for preparing a heterogeneous bonding device with controllable bonding interface thickness, comprising:

[0066] Provide optoelectronic thin film material chips;

[0067] Providing a wafer; wherein the wafer comprises a wafer oxide layer;

[0068] The photoelectric thin film material chip is bonded to the wafer oxide layer.

[0069] The method for preparing a heterogeneous bonding device with controllable bonding interface thickness provided in an embodiment of the present invention is different from the traditional die-die bonding type heterogeneous bonding device. It adopts the form of chip to wafer (die-wafer), which is conducive to realizing a truly silicon-based optoelectronic monolithic integrated system and realizing the industrial application of truly large-scale optoelectronic integrated chips.

[0070] It can be understood that the wafer is bonded to the optoelectronic thin film material chip, and the structure of the wafer includes the wafer substrate, the wafer buried oxide layer, the wafer waveguide layer, the wafer oxide layer and the wafer metal electrode, and the wafer oxide layer is bonded to the optoelectronic thin film material chip to realize the chip-to-wafer bonding form. Among them, the optoelectronic thin film material includes lithium niobate film, lithium tantalate film, etc.; the wafer can be a silicon nitride wafer, a silicon wafer, etc., that is, the waveguide layer of the wafer can be a silicon nitride waveguide, a silicon waveguide, etc., the substrate of the wafer can be a silicon substrate, a sapphire substrate, a glass substrate, etc., the buried oxide layer of the wafer is a silicon dioxide layer, and the oxide layer of the wafer is a silicon dioxide layer; the structure of the optoelectronic thin film material chip includes the substrate of the optoelectronic thin film material chip, the buried oxide layer of the optoelectronic thin film material chip and the optoelectronic thin film material layer, wherein the substrate of the optoelectronic thin film material chip can be a silicon substrate, a sapphire substrate, a glass substrate, etc., and the buried oxide layer of the optoelectronic thin film material chip is a silicon dioxide layer.

[0071] Specifically, the use of wafer-level processes can greatly improve process stability, increase output and reduce costs. At the same time, more and more applications have put forward higher requirements on process platforms, such as artificial intelligence optical computing, and computing power requires high-performance devices and larger networks. As the hybrid electro-optical modulator design continues to be improved and verified, the capabilities of existing silicon foundry processes can also be applied to combine more and more complex and multifunctional components with TFLN. In this platform, the crystalline properties of the silicon layer can be used to add dopants to make diodes and detectors, etc. Taken together, these designs and manufacturing processes will benefit many applications in classical and quantum photonics.

[0072] In a feasible implementation manner, the wafer preparation method includes:

[0073] (1) growing a first buried oxide layer 2 on a first substrate 1;

[0074] (2) etching the first buried oxide layer 2 to form a first etching groove 3;

[0075] (3) growing a waveguide layer 4 at the first etched groove 3;

[0076] (4) growing a second buried oxide layer 5 on the first buried oxide layer 2 and the waveguide layer 4;

[0077] (5) etching the second buried oxide layer 5 and the first buried oxide layer 2 to form a second etching groove 6, wherein the second etching groove 6 is spaced apart from the first etching groove 3;

[0078] (6) forming a metal electrode 7 at the second etched groove 6, wherein the metal electrode 7 is spaced apart from the waveguide layer 4;

[0079] (7) Growing a third buried oxide layer 8 on the second buried oxide layer 5 and the metal electrode 7; wherein the third buried oxide layer 8 is the wafer oxide layer.

[0080] It is understandable that in this embodiment, the waveguide and electrodes are first made on a wafer compatible with the CMOS process, and the bonding of the optoelectronic thin film material chip is used as a back-end step, which reduces the steps in which the optoelectronic thin film material chip is incompatible with the CMOS process. The allowable alignment error of the bonded optoelectronic thin film material chip can be up to 100μm, and if the electrode is made after bonding, the alignment error of the electrode needs to be as small as possible. Less than 1μm, at the same time, in order to protect the optoelectronic thin film material layer and make the electro-optical overlap integral large enough, we need to control the thickness of the oxide layer on the optoelectronic thin film material layer to 50-100nm, which increases the challenge of the process. At the same time, the bonding method in this embodiment does not need to etch the optoelectronic thin film material, avoiding the problem of difficulty in etching the optoelectronic thin film material, reducing production costs, and is suitable for large-scale production.

[0081] As a preference, see Figures 1 to 10 As shown, the wafer preparation method comprises:

[0082] (1) growing a first buried oxide layer 2 on a first substrate 1;

[0083] (2) etching the first buried oxide layer 2 to form a first etching groove 3;

[0084] (3) growing a waveguide layer 4 at the first etched groove 3;

[0085] (4) growing a second buried oxide layer 5 on the first buried oxide layer 2 and the waveguide layer 4;

[0086] (5) etching the second buried oxide layer 5 and the first buried oxide layer 2 to form a second etching groove 6, wherein the second etching groove 6 is spaced apart from the first etching groove 3;

[0087] (6) forming a metal electrode 7 at the second etching groove 6;

[0088] (7) growing a third buried oxide layer 8 on the second buried oxide layer 5 and the metal electrode 7;

[0089] (8) bonding a second substrate 9 on the third buried oxide layer 8;

[0090] (9) Removing the first substrate 1 to expose the first buried oxide layer 2; wherein the first buried oxide layer 2 is the wafer oxide layer.

[0091] Specifically, the third buried oxide layer 8 is selected as the buried oxide layer for bonding. Since there are metal electrodes 7 and waveguide layer 4 with different structures under the third buried oxide layer 8, it is difficult to accurately control the thickness of the third buried oxide layer 8. Therefore, we preferably use the bottom of the first buried oxide layer 2 as the bonding interface, without the need for chemical mechanical planarization (CMP) on the bonding interface, thereby improving the bonding quality and yield rate.

[0092] In a feasible implementation manner, the method for growing the first buried oxide layer 2 on the first substrate 1 is plasma enhanced chemical vapor deposition, and the thickness of the first buried oxide layer 2 is 150nm to 400nm;

[0093] The method for growing the second buried oxide layer 5 on the first buried oxide layer 2 and the waveguide layer 4 is plasma enhanced chemical vapor deposition, and the thickness of the second buried oxide layer 5 is 400nm to 900nm;

[0094] The method for growing the third buried oxide layer 8 on the second buried oxide layer 5 and the metal electrode 7 is plasma enhanced chemical vapor deposition, and the thickness of the third buried oxide layer 8 is 2000nm-5000nm.

[0095] Specifically, the thickness of the first buried oxide layer 2 needs to be greater than the thickness of the waveguide layer 4. If it is too large, the half-wave voltage after bonding will increase, the light transmission loss will increase, and the extinction ratio will decrease. If it is too small, the waveguide layer 4 of the required thickness cannot be grown. If the thickness of the second buried oxide layer 5 is too large, the thickness of the subsequently grown metal electrode 7 cannot be well controlled. If it is too small, the metal electrode 7 of the required thickness cannot be grown. If the thickness of the third buried oxide layer 8 is too small, the microwave transmission loss will increase and the 3dB bandwidth will be reduced. If it is too large, the microwave and light refractive indexes will not match, reducing the 3dB bandwidth.

[0096] In a feasible implementation manner, the method for growing the waveguide layer 4 at the first etched groove 3 is low-pressure chemical vapor deposition, and the thickness of the waveguide layer 4 is 100 nm to 300 nm.

[0097] Specifically, the thickness of the waveguide is in the range of 100 nm to 300 nm, which can form a better optical mode field. If it is too large or too small, it will increase the light transmission loss and reduce the extinction ratio.

[0098] In a feasible implementation manner, the method for manufacturing the metal electrode 7 at the second etching groove 6 is a magnetron sputtering method or an evaporation method, and the thickness of the metal electrode 7 is 500 nm to 1500 nm.

[0099] Specifically, the thickness of the metal electrode 7 is between 500 nm and 1500 nm, which can achieve good microwave transmission. If the thickness is too small, the microwave loss caused by the skin effect will increase. If the thickness is too large, it will cause impedance mismatch and reduce the 3dB bandwidth.

[0100] In a feasible implementation manner, bonding the optoelectronic thin film material chip to the wafer oxide layer includes:

[0101] Cleaning the photoelectric thin film material chip, wherein the photoelectric thin film material chip comprises a photoelectric thin film material layer 10, a photoelectric thin film material chip buried oxide layer 11 and a photoelectric thin film material chip substrate 12;

[0102] Activating the photoelectric thin film material layer 10 and the wafer oxide layer;

[0103] The photoelectric thin film material layer 10 is brought into contact with the wafer oxide layer at room temperature for bonding, and pressure annealing is applied after bonding;

[0104] Apply a protective layer 13, remove the photoelectric thin film material chip substrate 12, and then remove the protective layer 13;

[0105] Growing a heterogeneous bonding device oxide layer 14 so that the heterogeneous bonding device oxide layer 14 covers the optoelectronic thin film material chip buried oxide layer 11 and the wafer oxide layer;

[0106] The thickness of the heterogeneous bonding device oxide layer 14 is maintained to a desired thickness.

[0107] Specifically, the bonding method of the optoelectronic thin film material chip and the wafer oxide layer of this embodiment has good bonding strength and does not require harsh process conditions such as low pressure or high pressure. The applied pressure is 9-10N cm -2 The annealing temperature can be controlled at 100-350°C to complete the bonding and prevent the influence of excessively high temperature on the device performance.

[0108] In a feasible implementation manner, the thickness of the heterogeneous bonding device oxide layer 14 is retained to be 1 μm to 3 μm.

[0109] Specifically, the thickness of the heterogeneous bonding device oxide layer 14 is kept at 1 μm to 3 μm, which can achieve microwave and light refractive index matching. If it is too large or too small, the 3dB bandwidth will be reduced due to the mismatch between the microwave and light refractive index.

[0110] According to a second aspect of the embodiments of the present invention, a heterogeneous bonding device is provided, which is prepared by using the above-mentioned method for preparing a heterogeneous bonding device with controllable bonding interface thickness.

[0111] According to a third aspect of the embodiments of the present invention, an electro-optic modulator is provided, comprising the above-mentioned heterojunction bonding device.

[0112] The electro-optic modulator of the embodiment of the present invention includes the above-mentioned heterogeneous bonding device, with a 3dB bandwidth > 110GHz and a half-wave voltage < 3V, thus achieving single-wave 200G signal transmission.

[0113] In summary, the electro-optical modulator provided by the embodiment of the present invention has the following advantages:

[0114] (1) Different from the thin film waveguide device formed by the traditional etching method, the present invention adopts the form of die-wafer, which does not need to etch the photoelectric thin film material, avoids the problem of tilted sidewalls and large light loss, gives full play to the excellent characteristics of the photoelectric thin film material, and realizes the cross-generational improvement of device performance. At the same time, the electrode and passive optical waveguide structure are made on a wafer platform compatible with CMOS process (silicon nitride wafer or silicon wafer can be selected), and the process is more mature.

[0115] (2) Use the bottom of the buried oxide layer (i.e., the exposed first buried oxide layer 2, which is also the oxide layer of the wafer) as the bonding surface instead of the top oxide layer after CMP. Because the polishing rate of CMP depends on the potential pattern density, it forms undesirable thickness fluctuations. Using the bottom of the buried oxide layer can avoid these problems. At the same time, when bonding the second substrate 5, we can use more suitable materials according to needs to achieve higher performance devices.

[0116] (3) It is more suitable for on-chip multifunctional integration. The bonded modulator design can also be introduced into the production of other active and passive devices. Different from the die-die bonding, the bonding of optoelectronic thin film materials only occurs in the designated area, and the device structure in other areas is not affected by the bonding. In addition to the integration with other optoelectronic devices, it is also suitable for multi-material integration. The introduction of certain materials with better optical properties is conducive to the integration with other optoelectronic devices such as detectors, lasers, filters, etc., to realize the real silicon-based optoelectronic monolithic integrated system and realize the industrial application of large-scale optoelectronic integrated chips.

[0117] Example 1 A method for preparing a heterogeneous bonding device with controllable bonding interface thickness

[0118] A method for preparing a heterogeneous bonding device with controllable bonding interface thickness comprises the following steps: firstly manufacturing an optical waveguide and a metal electrode on a silicon nitride wafer, and then bonding the silicon nitride wafer to a photoelectric thin film material chip.

[0119] See also Figures 1 to 10 , making optical waveguides and metal electrodes on silicon nitride wafers, including:

[0120] (1) growing a first buried oxide layer 2 with a thickness of 200 nm on a first substrate 1 by plasma enhanced chemical vapor deposition (PECVD), wherein the first substrate 1 is a silicon substrate and the first buried oxide layer 2 is silicon dioxide;

[0121] (2) etching a groove on the first buried oxide layer 2 to form a first etched groove 3;

[0122] (3) using low pressure chemical vapor deposition (LPCVD) to grow a 150 nm thick waveguide layer 4 at the first etched groove 3, wherein the waveguide layer 4 is silicon nitride;

[0123] (4) using plasma enhanced chemical vapor deposition (PECVD) to grow a 900 nm thick second buried oxide layer 5 on the first buried oxide layer 2 and the waveguide layer 4; wherein the second buried oxide layer 5 is silicon dioxide;

[0124] (5) etching the second buried oxide layer 5 and the first buried oxide layer 2 to form a second etching groove 6, wherein the second etching groove 6 is spaced apart from the first etching groove 3;

[0125] (6) using a magnetron sputtering method, a metal electrode 7 with a thickness of 1000 nm is formed at the second etching groove 6, wherein the metal electrode 7 is made of metal gold;

[0126] (7) using plasma enhanced chemical vapor deposition (PECVD) to grow a 4700 nm thick third buried oxide layer 8 on the second buried oxide layer 5 and the metal electrode 7, wherein the third buried oxide layer 8 is silicon dioxide;

[0127] (8) bonding a second substrate 9 on the third buried oxide layer 8, wherein the second substrate 9 is a silicon substrate;

[0128] (9) removing the first substrate 1;

[0129] (10) After removing the first substrate 1, the exposed first buried oxide layer 2 (the first buried oxide layer 2 is the oxide layer of the silicon nitride wafer at this time) is wet-etched for bonding with the optoelectronic thin film material chip.

[0130] See also Figures 11 to 17, and then bonding the silicon nitride wafer to the optoelectronic thin film material chip, the optoelectronic thin film material chip in this embodiment is a lithium niobate thin film chip, specifically comprising:

[0131] (1) Cutting the photoelectric thin film material wafer into small pieces to form individual photoelectric thin film material chips, cleaning to remove dust particles and contaminants, the photoelectric thin film material chip comprising a photoelectric thin film material layer 10, a photoelectric thin film material chip buried oxide layer 11 (silicon dioxide layer) and a photoelectric thin film material chip substrate 12 (silicon substrate); using RF plasma activation; such as 150W and 1.103mbar, the surface activation bonding layer photoelectric thin film material and the first buried oxide layer 2, for 180 seconds;

[0132] (2) Soak in deionized water (DI), blow dry, and allow the surfaces to contact and bond at room temperature. -2 Under the applied pressure, the bonded sample is annealed by setting a certain temperature, such as 100 to 300°C;

[0133] (3) All other areas of the bonded sample except the substrate are coated with a protective layer 13 of a certain thickness;

[0134] (4) removing the optoelectronic thin film material chip substrate 12 by dry or wet etching;

[0135] (5) removing the protective layer 13;

[0136] (6) growing a heterogeneous bonding device oxide layer 14, wherein the heterogeneous bonding device oxide layer 14 is a silicon dioxide layer;

[0137] (7) HF wet etching and CMP of the heterogeneous bonding device oxide layer 14 are performed, and finally a 1 μm thick heterogeneous bonding device oxide layer 14 is retained.

[0138] See also Fig.16 and Fig.17 The heterogeneous bonding device of Example 1 with controllable bonding interface thickness is shown in FIG. The heterogeneous bonding device of Example 1 is used to prepare an electro-optic modulator, and the performance of the electro-optic modulator is evaluated. Fig.18 The heterojunction bonding device of Example 1 is used to prepare an electro-optic modulator, with a 3dB bandwidth > 110GHz and a half-wave voltage < 3V, achieving single-wave 200G signal transmission.

[0139] In the present invention, the terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance; the term "plurality" refers to two or more, unless otherwise clearly defined. The terms "installed", "connected", "connected", "fixed", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; "connected" can be a direct connection or an indirect connection through an intermediate medium. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0140] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by terms such as “upper”, “lower”, “left”, “right”, “front” and “back” are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or unit referred to must have a specific direction, be constructed and operated in a specific orientation, and therefore, cannot be understood as a limitation on the present invention.

[0141] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0142] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a heterogeneous bonding device with controllable bonding interface thickness, characterized in that: include: Provide optoelectronic thin film material chips; Providing a wafer; wherein the wafer comprises a wafer oxide layer; The photoelectric thin film material chip is bonded to the wafer oxide layer.

2. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 1, characterized in that: The wafer preparation method comprises: Growing a first buried oxide layer (2) on a first substrate (1); Etching the first buried oxide layer (2) to form a first etching groove (3); Growing a waveguide layer (4) at the first etched groove (3); Growing a second buried oxide layer (5) on the first buried oxide layer (2) and the waveguide layer (4); Etching the second buried oxide layer (5) and the first buried oxide layer (2) to form a second etching groove (6), wherein the second etching groove (6) is spaced apart from the first etching groove (3); Making a metal electrode (7) at the second etching groove (6); A third buried oxide layer (8) is grown on the second buried oxide layer (5) and the metal electrode (7); wherein the third buried oxide layer (8) is the wafer oxide layer.

3. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 1, characterized in that: The wafer preparation method comprises: Growing a first buried oxide layer (2) on a first substrate (1); Etching the first buried oxide layer (2) to form a first etching groove (3); Growing a waveguide layer (4) at the first etched groove (3); Growing a second buried oxide layer (5) on the first buried oxide layer (2) and the waveguide layer (4); Etching the second buried oxide layer (5) and the first buried oxide layer (2) to form a second etching groove (6), wherein the second etching groove (6) is spaced apart from the first etching groove (3); Making a metal electrode (7) at the second etching groove (6); Growing a third buried oxide layer (8) on the second buried oxide layer (5) and the metal electrode (7); bonding a second substrate (9) on the third buried oxide layer (8); The first substrate (1) is removed to expose the first buried oxide layer (2); wherein the first buried oxide layer (2) is the wafer oxide layer.

4. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 2 or 3, characterized in that: The method for growing the first buried oxide layer (2) on the first substrate (1) is plasma enhanced chemical vapor deposition, and the thickness of the first buried oxide layer (2) is 150nm to 400nm; The method for growing the second buried oxide layer (5) on the first buried oxide layer (2) and the waveguide layer (4) is plasma enhanced chemical vapor deposition, and the thickness of the second buried oxide layer (5) is 400nm to 900nm; The method for growing the third buried oxide layer (8) on the second buried oxide layer (5) and the metal electrode (7) is plasma enhanced chemical vapor deposition, and the thickness of the third buried oxide layer (8) is 2000nm to 5000nm.

5. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 2 or 3, characterized in that: The method for growing the waveguide layer (4) at the first etching groove (3) is low-pressure chemical vapor deposition, and the thickness of the waveguide layer (4) is 100nm to 300nm.

6. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 2 or 3, characterized in that: The method for making the metal electrode (7) at the second etching groove (6) is a magnetron sputtering method or an evaporation method, and the thickness of the metal electrode (7) is 500nm to 1500nm.

7. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 1, characterized in that: The step of bonding the photoelectric thin film material chip to the wafer oxide layer comprises: Cleaning the photoelectric thin film material chip, wherein the photoelectric thin film material chip comprises a photoelectric thin film material layer (10), a photoelectric thin film material chip buried oxide layer (11) and a photoelectric thin film material chip substrate (12); activating the photoelectric thin film material layer (10) and the wafer oxide layer; The photovoltaic thin film material layer (10) is brought into contact with the wafer oxide layer at room temperature for bonding, and pressure annealing is applied after bonding; Applying a protective layer (13), removing the photoelectric thin film material chip substrate (12), and then removing the protective layer (13); Growing a heterogeneous bonding device oxide layer (14) so ​​that the heterogeneous bonding device oxide layer (14) covers the optoelectronic thin film material chip buried oxide layer (11) and the wafer oxide layer; The thickness of the oxide layer (14) of the heterogeneous bonding device is maintained to a desired thickness.

8. The method for preparing a heterogeneous bonding device with controllable bonding interface thickness according to claim 7, characterized in that: The thickness of the heterogeneous bonding device oxide layer (14) is retained to be 1 μm to 3 μm.

9. A heterogeneous bonding device, characterized in that: The device is prepared by the method for preparing a heterogeneous bonding device with controllable bonding interface thickness as described in any one of claims 1 to 8.

10. An electro-optic modulator, characterized in that: Includes the heterogeneous bonding device as described in claim 9.

Citation Information

Cited By

  • Waveguide wafer, composite modulator and preparation method thereof

    CN119882282A