N-p-n middle-middle two-color tellurium-cadmium-mercury infrared photoelectric detector semiconductor device and preparation method thereof

By optimizing material components and structural parameters in n-p n-type dual-color mercury tellurization infrared photodetector, the problem of insufficient performance in the prior art is solved, and the effects of high sensitivity, high response speed, low dark current and low crosstalk are achieved. , meet the high performance needs of multi-color imaging systems.

CN119092590AActive Publication Date: 2024-12-0611TH RES INST OF CHINA ELECTRONICS TECH GROUP CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411184818.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Preparation of high-performance n-p n-type dual-color mercury cadmium telluride infrared photodetectors in the prior art face challenges that are difficult to meet performance requirements such as sensitivity, response speed and dark current. Especially in the application of multi-color imaging systems, existing dual-color detectors are available. There are shortcomings in high sensitivity, high responsiveness and low crosstalk.

Method used

By establishing a simulation model, optimizing material components and structural parameters, determining the components, doping concentration and thickness ranges of the first and second n-type HgCdTe layers, and growing corresponding layer structures on the substrate layer, realizing device design optimization, including The thickness of the first n-type HgCdTe layer is 4 μm to 9 μm, the thickness of the second n-type HgCdTe layer is 2 μm to 5 μm, the thickness of the p-type HgCdTe layer is 2 μm to 5 μm, and the device inclination range is 75 ° to 90 ° to improve the sensitivity of the device. and response speed, reduce dark current and crosstalk.

Benefits of technology

It realizes performance devices with high sensitivity, high response speed, low dark current, and low crosstalk, which meets the high performance requirements of multi-color infrared detectors and significantly improves the device's light response and quantum efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092590A_ABST
    Figure CN119092590A_ABST
Patent Text Reader

Abstract

The invention discloses a middle-middle double-color infrared photoelectric detector semiconductor device and a preparation method thereof, and relates to the semiconductor technology, and the method comprises the steps: S10, building a simulation model, and obtaining the relationship trend between the parameters of each layer of the device and the performance of the device through a performance test experiment; s20, determining a parameter range of each layer of the device based on the relationship trend; s30, growing a substrate layer in sequence; the Cd component of the first n-type layer is 0.33-0.36, the doping concentration of In is 5 * 10 < 14 > / cm < 3 >-5 * 10 < 16 > / cm < 3 >, and the thickness of the first n-type layer is 4-9 microns; in the p-type layer, the Cd component is 0.35-0.38, the Hg vacancy or As doping concentration is 5 * 10 < 16 > / cm < 3 >-5 * 10 < 18 > / cm < 3 >, and the thickness is 2-5 microns; the Cd component of the second n-type layer is 0.29-0.31, the In doping concentration is 5 * 10 < 14 > / cm < 3 >-5 * 10 < 16 > / cm < 3 >, and the thickness is 2-5 microns; and the gradient of the device is 75-90 degrees.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor technology, and in particular to an npn dual-color mercury cadmium telluride infrared photodetector semiconductor device and a preparation method thereof. Background Art

[0002] Due to the advantages of HgCdTe materials such as excellent carrier transport properties, large adjustable response range, and extremely high photoelectric conversion efficiency, mercury cadmium telluride (HgCdTe) infrared detectors are widely used in infrared detection systems and can work in the atmospheric windows of 1μm to 3μm, 3μm to 5μm, and 8μm to 12μm. Although monochromatic detectors can detect effective targets, the detection of radiation characteristics of complex targets needs to be improved. With the development of HgCdTe infrared detection technology, the demand for multicolor imaging systems in various fields such as fiber-optic communications, 3D lidar, astronomical observations, and atmospheric detection has been put on the agenda.

[0003] Multicolor detectors can provide information in more than two bands, and are superior to monochrome detectors in terms of target recognition, signal recognition and anti-interference performance. At present, many international institutions have carried out research on multicolor infrared detectors and put them into practical application. In the existing technology, the two-color HgCdTe detector uses two layers of n-type absorption layer and one layer of p-type barrier layer to form two back-to-back diode structures. In the working mode of the HgCdTe two-color readout circuit of the British SELEX company, the medium and long-wave two-color signals can realize the integration / readout of the monochrome signal, the sequential / integrated readout of the two-color signal, or the two-color signal can be integrated / readout twice alternately. The development of the dual-band focal plane can be traced back to the MW / LW line array two-color detector that started in 1995. The MW / LW line array two-color detector realizes the 25μm pixel 256×256SW / MW focal plane of the npn structure, and the readout circuit adopts the working mode of sequential integration of the two-color signal. Based on the technical accumulation of nearly ten years, Sofradir proposed a new semiplanar process technology route that has been used to this day. After optimizing the new process technology, the 24μm pixel 640×512MW / LW focal plane component shelf product was realized after 2009. The detector of Sofradir Company adopts the technical route of semi-planar structure. By integrating the dual-color signal input level unit circuit in the pixel area of ​​the readout circuit, the dual-color signal synchronous integration and the complete synchronization of the dual-color signal in the time domain are realized. For the dual-color signal synchronous integration requirements, the existing technology uses special potential well capacitor design technology and high-density layout wiring technology to finally realize the dual-color signal synchronous integration and synchronous readout in a limited pixel area. In another technology, based on the 0.35μm 2P4M process, direct injection and TDMI integration structure are used to develop a 640×512 dual-color focal plane readout circuit suitable for a stacked structure. Although the research on multi-color detectors has made some progress, the research task of preparing high-performance mature multi-color detectors is still quite arduous and urgent. Summary of the invention

[0004] The embodiments of the present application provide an npn two-color mercury cadmium telluride infrared photodetector semiconductor device and a preparation method, which are used to optimize the material preparation and device structure parameters, thereby providing a device with better sensitivity, higher response speed, smaller dark current, lower crosstalk and other performances, and meeting the high performance requirements of various fields for npn two-color mercury cadmium telluride photodetectors with high sensitivity, high responsiveness, low dark current, low crosstalk, etc.

[0005] The present application embodiment provides a method for preparing an npn medium dual-color mercury cadmium telluride infrared photodetector semiconductor device, comprising:

[0006] S10, establishing a simulation model of an npn bicolor HgCdTe infrared photodetector semiconductor device, obtaining the relationship trends of the components, doping concentration, thickness of the first n-type HgCdTe layer, the p-type HgCdTe layer, and the second n-type HgCdTe layer and the device dark current, electrode current, quantum efficiency, photoresponse, and crosstalk through performance test experiments; and obtaining the relationship trends of the device tilt and the device dark current, electrode current, quantum efficiency, photoresponse, and crosstalk;

[0007] S20, based on the obtained composition, doping concentration, thickness and device inclination of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer, and the relationship trend of the device dark current, electrode current, quantum efficiency, light response and crosstalk, respectively determine the composition range, doping concentration range and thickness range of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer of the npn bicolor mercury cadmium telluride infrared photodetector device to be prepared, and determine the inclination range of the device to be prepared;

[0008] S30, growing a substrate layer, and sequentially growing a first n-type HgCdTe layer, a p-type HgCdTe layer, and a second n-type HgCdTe layer on the substrate layer; wherein,

[0009] The thickness of the first n-type HgCdTe layer is 4 μm to 9 μm;

[0010] The thickness of the second n-type HgCdTe layer is 2 μm to 5 μm;

[0011] The thickness of the p-type HgCdTe layer is 2 μm to 5 μm;

[0012] The overall inclination of the device ranges from 75° to 90°.

[0013] Optionally, the relationship trends among the components, doping concentration, thickness and device dark current, electrode current, quantum efficiency, photoresponse and crosstalk of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer are respectively obtained through performance testing experiments, and the component range, doping concentration range and thickness range of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer are determined according to the corresponding relationship trends; and the inclination range of the device is determined according to the relationship trends among the inclination of the device and the device dark current, electrode current, quantum efficiency, photoresponse and crosstalk.

[0014] Optionally, the first n-type HgCdTe layer grown is a shorter medium-wavelength n-type HgCdTe layer, whose Cd composition ranges from 0.33 to 0.36, and the In doping concentration ranges from 5×10 14 / cm3 ~5×10 16 / cm 3 .

[0015] Optionally, the Cd composition of the second n-type HgCdTe layer is in the range of 0.29 to 0.31, and the doping In concentration is in the range of 5×10 14 / cm 3 ~5×10 16 / cm 3 .

[0016] Optionally, the p-type HgCdTe layer is a relatively long medium-wavelength n-type HgCdTe layer, the Cd component of which ranges from 0.35 to 0.37, and the Hg vacancy or As doping concentration ranges from 5×10 16 / cm 3 ~5×10 18 / cm 3 , and the Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer.

[0017] The embodiment of the present application also provides an npn dual-color mercury cadmium telluride infrared photodetector semiconductor device, comprising:

[0018] Substrate or composite substrate;

[0019] A first n-type HgCdTe layer is grown on the substrate or the composite substrate, wherein the first n-type HgCdTe layer has a thickness of 4.0 μm to 9.0 μm;

[0020] A p-type HgCdTe layer is grown on the first n-type HgCdTe layer, wherein the p-type HgCdTe layer has a thickness of 2.0 μm to 5.0 μm;

[0021] The second n-type HgCdTe layer is grown on the p-type HgCdTe layer, and the thickness of the second n-type HgCdTe layer is 2.0 μm to 5.0 μm.

[0022] Optionally, the first n-type HgCdTe layer is a 3.0 μm to 4.0 μm medium-wavelength n-type HgCdTe layer with an In doping concentration of 5×10 14 / cm 3 ~5×10 16 / cm 3 , the Cd component is between 0.33 and 0.36.

[0023] Optionally, the p-type HgCdTe layer is doped with Hg vacancies or As at a concentration of 5×10 16 / cm 3 ~5×10 18 / cm 3, the Cd component is between 0.35 and 0.37, and the Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer.

[0024] Optionally, the second n-type HgCdTe layer is a 4.0 μm to 5.0 μm medium-wave n-type HgCdTe layer with an In doping concentration of 5×10 14 / cm 3 ~5×10 16 / cm 3 , the Cd component is between 0.29 and 0.31.

[0025] The embodiment of the present application also provides an npn dual-color mercury cadmium telluride infrared photodetector semiconductor device, which is prepared by the method as described above.

[0026] The embodiments of the present application optimize the material preparation and device structure parameters, thereby providing a device with better sensitivity, higher response speed, smaller dark current, lower crosstalk and other performances, meeting the high performance requirements of various fields for npn-type two-color mercury cadmium telluride photodetectors with high sensitivity, high responsiveness, low dark current, low crosstalk, etc.

[0027] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0029] Figure 1 The basic process diagram of the method for preparing the npn bicolor mercury cadmium telluride infrared photodetector semiconductor device of the embodiment of the present application is shown;

[0030] Figure 2 It is a schematic structural diagram of an npn dual-color mercury cadmium telluride infrared photodetector semiconductor device in an embodiment of the present application;

[0031] Figure 3 This is a diagram showing the device's higher performance at a moderate composition of the npn bicolor mercury cadmium telluride infrared photodetector semiconductor device in an embodiment of the present application;

[0032] Figure 4The performance of the npn dual-color HgCdTe detector varies with the thickness of the 3.0μm to 4.0μm medium-wave n-layer in the application example of this application (a) 4.0μm to 5.0μm medium-wave n-layer quantum efficiency wavelength diagram (b) 3.0μm to 4.0μm medium-wave n-layer quantum efficiency wavelength diagram (c) crosstalk thickness diagram (d) light response wavelength diagram (e) 3.0μm to 4.0μm medium-wave n-layer current wavelength diagram (f) 4.0μm to 5.0μm medium-wave n-layer current wavelength diagram (thickness unit: μm);

[0033] Figure 5 The performance of the npn two-color HgCdTe detector varies with the thickness of the p-layer in the application example of this application (a) 4.0μm ~ 5.0μm medium wave n-layer quantum efficiency wavelength diagram (b) 3.0μm ~ 4.0μm medium wave n-layer quantum efficiency wavelength diagram (c) crosstalk thickness diagram (d) light response wavelength diagram (e) 3.0μm ~ 4.0μm medium wave n-layer current wavelength diagram (f) 4.0μm ~ 5.0μm medium wave n-layer current wavelength diagram (thickness unit: μm);

[0034] Figure 6 The performance of the npn dual-color HgCdTe detector varies with the thickness of the 3.0μm to 4.0μm medium-wave n-layer in the application example of this application (a) 4.0μm to 5.0μm medium-wave n-layer quantum efficiency wavelength diagram (b) 3.0μm to 4.0μm medium-wave n-layer quantum efficiency wavelength diagram (c) crosstalk thickness diagram (d) light response wavelength diagram (e) 3.0μm to 4.0μm medium-wave n-layer current wavelength diagram (f) 4.0μm to 5.0μm medium-wave n-layer current wavelength diagram (thickness unit: μm);

[0035] Figure 7 As an example of the application of this application, the performance of the npn medium-color mercury cadmium telluride detector varies with the pixel inclination: (a) 4.0μm to 5.0μm medium-wave n-layer quantum efficiency wavelength diagram (b) crosstalk thickness diagram (c) light response wavelength diagram (d) current wavelength diagram (thickness unit: μm). DETAILED DESCRIPTION

[0036] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0037] The present application embodiment provides an npn medium dual-color mercury cadmium telluride infrared photodetector semiconductor device and a preparation method, such as Figure 1 As shown, including:

[0038] S10, establishing a simulation model of an npn bicolor HgCdTe infrared photodetector semiconductor device, obtaining the relationship trends of the components, doping concentration, thickness of the first n-type HgCdTe layer, the p-type HgCdTe layer, and the second n-type HgCdTe layer and the device dark current, electrode current, quantum efficiency, photoresponse, and crosstalk through performance test experiments; and obtaining the relationship trends of the device tilt and the device dark current, electrode current, quantum efficiency, photoresponse, and crosstalk;

[0039] S20, based on the obtained composition, doping concentration, thickness and device inclination of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer, and the relationship trend of the device dark current, electrode current, quantum efficiency, light response and crosstalk, respectively determine the composition range, doping concentration range and thickness range of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer of the npn bicolor mercury cadmium telluride infrared photodetector device to be prepared, and determine the inclination range of the device to be prepared;

[0040] S30, growing a substrate layer, and sequentially growing a first n-type HgCdTe layer, a p-type HgCdTe layer, and a second n-type HgCdTe layer on the substrate layer; wherein,

[0041] The thickness of the first n-type HgCdTe layer is 4 μm to 9 μm;

[0042] The thickness of the second n-type HgCdTe layer is 2 μm to 5 μm;

[0043] The thickness of the p-type HgCdTe layer is 2 μm to 5 μm;

[0044] The overall tilt of the device ranges from 75° to 90°. For example, in some examples, Figure 1 As shown, the inclination angle between the side surface of the semiconductor device and the horizontal plane (lower top surface) ranges from 75° to 90°, and the cross-sectional width of the substrate or composite substrate is greater than the cross-sectional width of the second n-type HgCdTe layer 3 .

[0045] Optionally, the relationship trends among the components, doping concentration, thickness and device dark current, electrode current, quantum efficiency, photoresponse and crosstalk of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer are respectively obtained through performance testing experiments, and the component range, doping concentration range and thickness range of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer are determined according to the corresponding relationship trends; and the inclination range of the device is determined according to the relationship trends among the inclination of the device and the device dark current, electrode current, quantum efficiency, photoresponse and crosstalk.

[0046] Optionally, the first n-type HgCdTe layer grown is a 3.0 μm to 4.0 μm medium-wavelength n-type HgCdTe layer, whose Cd composition ranges from 0.33 to 0.36, and the In doping concentration ranges from 5×10 14 / cm 3 ~5×10 16 / cm 3 .

[0047] Optionally, the Cd composition of the second n-type HgCdTe layer is in the range of 0.29 to 0.31, and the doping In concentration is in the range of 5×10 14 / cm 3 ~5×10 16 / cm 3 .

[0048] Optionally, the Cd content of the p-type HgCdTe layer is in the range of 0.35 to 0.37, and the Hg vacancy or As doping concentration is in the range of 5×10 16 / cm 3 ~5×10 18 / cm 3 , and the Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer.

[0049] The present application also provides an npn medium dual-color mercury cadmium telluride infrared photodetector semiconductor device, such as Figure 2 As shown, including:

[0050] Substrate or composite substrate;

[0051] The first n-type HgCdTe layer 1 is grown on the substrate or composite substrate and is a 3.0μm-4.0μm n-type HgCdTe layer with a thickness of 4.0μm-9.0μm and is doped with In. For example, a 3.0μm-4.0μm medium-wave n-type HgCdTe layer is grown on the substrate or composite substrate.

[0052] A p-type HgCdTe layer 2, grown on the first n-type HgCdTe layer 1, with a thickness of 2.0 μm to 5.0 μm, doped with Hg vacancies or As;

[0053] The second n-type HgCdTe layer 3 is grown on the p-type HgCdTe layer 2 and is a 4.0 μm to 5.0 μm n-type HgCdTe layer with a thickness of 2.0 μm to 5.0 μm and doped with In. For example, a relatively long medium-wavelength n-type HgCdTe layer is grown on the p-type HgCdTe layer 2 .

[0054] In some embodiments, Figure 2As shown, the side of the infrared photodetector semiconductor device is inclined at an angle of 75° to 90° with respect to the horizontal plane, and the cross-sectional width of the substrate or composite substrate is greater than the cross-sectional width of the second n-type HgCdTe layer 3 .

[0055] The embodiments of the present application optimize the material preparation and device structure parameters, thereby providing a device with better sensitivity, higher response speed, smaller dark current, lower crosstalk and other performances, meeting the high performance requirements of various fields for npn-type two-color mercury cadmium telluride photodetectors with high sensitivity, high responsiveness, low dark current, low crosstalk, etc.

[0056] In some embodiments, the first n-type HgCdTe layer 1 (3.0 μm-4.0 μm medium-wave n-type HgCdTe layer) is doped with an In concentration of 5×10 14 / cm 3 ~5×10 16 / cm 3 , the Cd component is between 0.33 and 0.36.

[0057] In some embodiments, the p-type HgCdTe layer 2 is doped with Hg vacancies or As at a concentration of 5×10 16 / cm 3 ~5×10 18 / cm 3 , the Cd component is between 0.35 and 0.37. The Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer, and the Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer.

[0058] In some embodiments, the second n-type HgCdTe layer 3 (4.0 μm-5.0 μm medium-wave n-type HgCdTe layer) is doped with an In concentration of 5×10 14 / cm 3 ~5×10 16 / cm 3 , the Cd component is between 0.29 and 0.31.

[0059] Figure 3 The relevant performance diagram of the npn dual-color mercury cadmium telluride infrared photodetector semiconductor device in the embodiment of the present application is shown (wherein, the thickness of the wave layer in 4.0μm-5.0μm is 2μm, the component x=0.3; the thickness of the p layer is 2.2μm, the component x=0.37; the thickness of the wave layer in 3.0μm-4.0μm is 5μm, the component x=0.345, and the crosstalk is 4.3%). Figure 2 It can be seen that under the appropriate composition and doping concentration design of the present application, the detector can have higher quantum efficiency, better photoresponse, better IV value, lower crosstalk, and the dark current and photocurrent levels differ by more than two orders of magnitude.

[0060] Figure 4 This is the corresponding performance diagram of the 4.0μm to 5.0μm medium-wave layer thickness change of the npn medium-wave dual-color cadmium telluride infrared photodetector in the application example; Figure 4 (a) It can be seen that as the thickness of the 4.0μm to 5.0μm medium-wave n-layer increases, the overall quantum efficiency of the 4.0μm to 5.0μm medium-wave n-layer gradually increases. In some specific application examples, a thickness of 2μm to 3.5μm can be selected, which can further solve the problem of the difficulty of etching and other processes caused by the long 4.0μm to 5.0μm medium-wave n-layer on the upper layer of the device structure. Figure 4 (b) It can be seen that with the increase of the thickness of the medium-wave n-layer in the range of 4.0μm to 5.0μm, the quantum efficiency of the medium-wave n-layer in the range of 3.0μm to 4.0μm does not change much. 4(c) With the increase of the thickness of the medium-wave n-layer in the range of 4.0μm to 5.0μm, the crosstalk of the detector gradually increases. Figure 4 (d) shows that the detector has good photoresponse under the designed conditions. Figure 4 (e) and Figure 4 (f) shows that the calculated magnitude of the current in the two bands is consistent with the current range of general detectors. According to the calculation, the thickness design of the 4.0μm to 5.0μm medium-wave n layer proposed in the embodiment of the present application has a difference of more than two orders of magnitude between the dark current and the current magnitude in the two bands.

[0061] Figure 5 This is the performance diagram of the npn medium-wave two-color cadmium telluride infrared photodetector in the application example. It can be seen from Figure 5(a) that with the increase of the p-layer thickness, the quantum efficiency of the 4.0μm to 5.0μm medium-wave n-layer in the shorter wave band gradually becomes lower. Figure 5(b) describes that with the increase of the p-layer thickness, the quantum efficiency of the 3.0μm to 4.0μm medium-wave n-layer does not change much. Figure 5(c) shows that with the increase of the p-layer thickness, the crosstalk of the detector gradually decreases. Figure 5 (d) shows that the detector has good photoresponse under the designed conditions. Figure 5 (e) and Figure 5 (f) shows that the calculated magnitude of the current in the two bands is consistent with the current range of a general detector. According to the calculation, by applying the thickness design of the p-type HgCdTe layer proposed in the embodiment of the present application, the dark current and current magnitude of the two bands differ by more than two orders of magnitude.

[0062] Figure 6 This is the performance diagram of the shorter medium-wave layer thickness change of the npn medium-wave dual-color cadmium telluride infrared photodetector in the application example. Figure 6(a) It can be seen that with the increase of the thickness of the 3.0μm~4.0μm medium-wave n-layer, the overall quantum efficiency of the 4.0μm~5.0μm medium-wave n-layer does not change much, but the quantum efficiency in the 3.0μm~4.0μm band gradually decreases. Figure 6 (b) describes that as the thickness of the medium-wave n-layer in the range of 3.0μm to 4.0μm increases, the quantum efficiency of the medium-wave n-layer in the range of 3.0μm to 4.0μm decreases, and at the same time, the band with higher quantum efficiency shifts toward 4.0μm to 5.0μm.

[0063] In the embodiment of the present application, the thickness of the first n-type HgCdTe layer is designed to be 4.0μm to 9.0μm, which is relatively thick. This solves the problem that the thinner 3.0μm to 4.0μm medium-wave n-layer will have a higher transmittance to shorter wavelength light, and will produce a higher 3.0μm to 4.0μm band quantum efficiency in the 4.0μm to 5.0μm band, thereby increasing the problem of device crosstalk.

[0064] Figure 6 In (c), as the thickness of the medium-wave n-layer increases from 3.0 μm to 4.0 μm, the crosstalk of the detector gradually decreases. Figure 6 (d) shows that the detector has good photoresponse under the designed conditions. Figure 6 (e) and Figure 6 (f) shows that the calculated magnitude of the current in the two bands is consistent with the current range of general detectors. According to the calculation, the thickness design of the 3.0μm to 4.0μm medium-wave n layer in the embodiment of the present application has a difference of more than two orders of magnitude between the dark current and the current magnitude in the two bands.

[0065] Figure 7 This is an example of the performance of the npn medium-wave dual-color cadmium telluride infrared photodetector device with tilt changes. Figure 7 (a) and Figure 7 (b) It can be seen that as the pixel tilt increases, the quantum efficiency of the n-layer in the 4.0μm to 5.0μm medium wave gradually decreases, causing the crosstalk to gradually decrease. Figure 7 (b) It can be seen that changing the pixel tilt can adjust the device crosstalk to a smaller value. Figure 7 (c) shows that the detector has good photoresponse under the designed conditions. Figure 7 (d) shows that the calculated current magnitude of the detector under the design conditions is consistent with the current range of general detectors. According to calculations, the two side inclinations in the embodiment of the present application are designed, and the dark current and current magnitude of the two bands differ by more than two orders of magnitude.

[0066] It can be seen from the relationship diagram that within the device parameter range determined by the embodiment of the present application, the device maintains high quantum efficiency, high high response and low crosstalk, and the dark current and device current differ by more than 2 orders of magnitude. Further, considering the actual low dark current, high sensitivity, high response, low crosstalk and other performances, the device material and device structure can be adjusted according to each relationship trend diagram. The device structure of the embodiment of the present application lays the foundation for the preparation of high-performance npn-type medium-wave two-color mercury cadmium telluride photodetectors.

[0067] The embodiment of the present application also provides an npn dual-color mercury cadmium telluride infrared photodetector semiconductor device, which is prepared by the method as described above.

[0068] It should be noted that in the various embodiments of the present application, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "includes a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.

[0069] The serial numbers of the above-mentioned embodiments of the present application are for description only and do not represent the advantages or disadvantages of the embodiments.

[0070] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.

Claims

1. A method for preparing a npn medium dual-color mercury cadmium telluride infrared photodetector semiconductor device, characterized in that: include: S10, establish a simulation model of the npn bicolor HgCdTe infrared photodetector semiconductor device, and obtain the relationship between the composition, doping concentration, thickness and device dark current, electrode current, quantum efficiency, photoresponse, and crosstalk of the first n-type HgCdTe layer, the p-type HgCdTe layer, and the second n-type HgCdTe layer through performance test experiments; And obtain the relationship trend between the device tilt and the device dark current, electrode current, quantum efficiency, photoresponse, and crosstalk; S20, based on the obtained composition, doping concentration, thickness and device inclination of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer, and the relationship trend of the device dark current, electrode current, quantum efficiency, light response and crosstalk, respectively determine the composition range, doping concentration range and thickness range of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer of the npn bicolor mercury cadmium telluride infrared photodetector device to be prepared, and determine the inclination range of the device to be prepared; S30, growing a substrate layer, and sequentially growing a first n-type HgCdTe layer, a p-type HgCdTe layer, and a second n-type HgCdTe layer on the substrate layer; wherein, The thickness of the first n-type HgCdTe layer is 4 μm to 9 μm; The thickness of the second n-type HgCdTe layer is 2 μm to 5 μm; The thickness of the p-type HgCdTe layer is 2 μm to 5 μm; The overall inclination of the device ranges from 75° to 90°.

2. The method for preparing the npn bicolor mercury cadmium telluride infrared photodetector semiconductor device according to claim 1, characterized in that: The performance test experiment obtains the relationship trends of the components, doping concentration, thickness and device dark current, electrode current, quantum efficiency, photoresponse and crosstalk of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer respectively, and determines the component range, doping concentration range and thickness range of the first n-type HgCdTe layer, the p-type HgCdTe layer and the second n-type HgCdTe layer according to the corresponding relationship trends; and determines the inclination range of the device according to the obtained relationship trends between the inclination of the device and the device dark current, electrode current, quantum efficiency, photoresponse and crosstalk.

3. The method for preparing the npn bicolor mercury cadmium telluride infrared photodetector semiconductor device according to claim 1, characterized in that: The first n-type HgCdTe layer grown is a shorter medium-wavelength n-type HgCdTe layer, whose Cd composition ranges from 0.33 to 0.36 and In doping concentration ranges from 5×10 14 / cm 3 ~5×10 16 / cm 3 .

4. The method for preparing the npn dual-color mercury cadmium telluride infrared photodetector semiconductor device according to claim 1, characterized in that: The Cd composition of the second n-type HgCdTe layer ranges from 0.29 to 0.31, and the doping In concentration ranges from 5×10 14 / cm 3 ~5×10 16 / cm 3 .

5. The method for preparing the npn bicolor mercury cadmium telluride infrared photodetector semiconductor device according to claim 1, characterized in that: The p-type HgCdTe layer is a relatively long medium-wavelength n-type HgCdTe layer, wherein the Cd component ranges from 0.35 to 0.37, and the Hg vacancy or As doping concentration ranges from 5×10 16 / cm 3 ~5×10 18 / cm 3 , and the Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer.

6. An npn dual-color mercury cadmium telluride infrared photodetector semiconductor device, characterized in that: include: Substrate or composite substrate; A first n-type HgCdTe layer is grown on the substrate or the composite substrate, wherein the first n-type HgCdTe layer has a thickness of 4.0 μm to 9.0 μm; A p-type HgCdTe layer is grown on the first n-type HgCdTe layer, wherein the p-type HgCdTe layer has a thickness of 2.0 μm to 5.0 μm; The second n-type HgCdTe layer is grown on the p-type HgCdTe layer, and the thickness of the second n-type HgCdTe layer is 2.0 μm to 5.0 μm.

7. The npn dual-color mercury cadmium telluride infrared photodetector semiconductor device as claimed in claim 6, characterized in that: The first n-type HgCdTe layer is a shorter medium-wavelength n-type HgCdTe layer with an In doping concentration of 5×10 14 / cm 3 ~5×10 16 / cm 3 , the Cd component is between 0.33 and 0.

36.

8. The npn dual-color mercury cadmium telluride infrared photodetector semiconductor device as claimed in claim 6, characterized in that: The p-type HgCdTe layer is doped with Hg vacancies or As at a concentration of 5×10 16 / cm 3 ~5×10 18 / cm 3 , the Cd component is between 0.35 and 0.37, and the Cd component value of the p-type HgCdTe layer is greater than or equal to the Cd component value of the n-type HgCdTe layer.

9. The npn dual-color mercury cadmium telluride infrared photodetector semiconductor device as claimed in claim 6, characterized in that: The second n-type HgCdTe layer is a longer medium-wave n-type HgCdTe layer with an In doping concentration of 5×10 14 / cm 3 ~5×10 16 / cm 3 , the Cd component is between 0.29 and 0.

31.

10. An npn dual-color mercury cadmium telluride infrared photodetector semiconductor device, characterized in that: The semiconductor device is manufactured by the method according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Silicon-based short wave / medium wave laminated layer two-color HgCdTe material and preparation method thereof

    CN106384751A

  • Double-color tellurium-cadmium-mercury infrared photoelectric detector and preparation method thereof

    CN116387393A

  • Electromagnetic wave detector, electromagnetic wave detector array, and method for manufacturing electromagnetic wave detector

    CN117063298A

  • Structure photosensitive to infrared radiation and method for its manufacture

    RU2769232C1

  • Multispectral radiation detectors using strain-compensating superlattices

    US20020125472A1