Electrolyte additive for all-vanadium redox flow battery

By using modified crown ether and functionalized graphene composite materials in all vanadium flow batteries, the problems of high internal resistance of the battery and low vanadium ion transmission efficiency are solved, and higher electrolysis rate and cycle stability are achieved, which improves the The battery's energy and Coulomb efficiency are suitable for commercial applications.

CN119092768APending Publication Date: 2024-12-06山西国润储能科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185812.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

All vanadium flow batteries are limited by high internal resistance and low vanadium ion transmission efficiency under high current density, and insufficient stability of the electrolyte, which affects the cycle stability and life of the battery.

Method used

Modified crown ether and functionalized graphene composite materials are used as electrolyte additives to enhance the solubility and migration rate of vanadium ions through hydrophobic side chains and functional groups (amino and carboxylic groups), and graphene is modified by silane coupling agent. Improve conductivity and interface compatibility.

Benefits of technology

It significantly reduces the internal resistance of the battery, improves charging and discharging efficiency and cycle stability, extends battery life, improves energy efficiency and Coulomb efficiency, and is suitable for commercial and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013465650000171
    Figure BDA0005013465650000171
  • Figure BDA0005013465650000181
    Figure BDA0005013465650000181
Patent Text Reader

Abstract

The present invention relates to the technical field of electrochemical energy storage, and discloses an all-vanadium redox flow battery electrolyte additive, which comprises the following components by weight: 80-90% of modified crown ether, the modified crown ether comprises basic 18-crown-6 ether, and a hydrophobic side chain and a functional group are introduced; 10-20% of a graphene composite material, wherein graphene is subjected to surface modification through a silane coupling agent; the hydrophobic side chain is selected from an alkyl chain, and the functional group is selected from amino and carboxyl; the alkyl bromide is selected from C10-C18 alkyl chains so as to introduce hydrophobic side chains; the graphene composite material comprises a mixture of unmodified graphene and modified graphene. According to the all-vanadium redox flow battery electrolyte additive disclosed by the invention, higher electrolytic efficiency, lower internal resistance, more stable charge-discharge cycle and longer battery service life are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochemical energy storage, in particular to an electrolyte additive for an all-vanadium liquid flow battery. Background Art

[0002] Vanadium redox flow battery (VRFB) technology has been widely recognized as one of the most promising solutions for large-scale energy storage systems due to its unique advantages, such as high reversibility, long cycle life, and scalable energy storage capacity. However, despite its great potential, the commercial application and performance efficiency of vanadium redox flow batteries are still limited by several key technical challenges.

[0003] First, a major problem faced by all-vanadium batteries during operation is the high internal resistance of the electrolyte, which directly affects the power density and energy efficiency of the battery. The main source of internal resistance is the insufficient migration rate of vanadium ions in the electrolyte, which largely limits the performance of the battery at high current density. In addition, the insufficient stability of vanadium ions in the electrolyte may also lead to the loss of active materials, further affecting the cycle stability and economic benefits of the battery.

[0004] Secondly, existing electrolyte formulations often lack the necessary electrolyte-electrode interface stability, which may lead to corrosion or degradation of electrode materials during long-term battery operation, thereby reducing the overall life and performance of the battery. In addition, the viscosity and fluidity of the electrolyte are also one of the key factors limiting battery design and optimization, especially under low temperature or high flow rate operating conditions. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides an electrolyte additive for an all-vanadium liquid flow battery to solve the problems of all-vanadium liquid flow batteries being limited by high internal resistance and low vanadium ion transmission efficiency at high current density. By optimizing the electrolyte formula, the electrolysis rate of the battery is increased and the internal resistance is reduced, thereby improving the battery's charge and discharge efficiency and cycle stability.

[0006] To achieve the above objectives, the present invention is implemented by the following technical solution: an all-vanadium liquid flow battery electrolyte additive, the additive comprising the following components in weight percentage:

[0007] 80-90% of modified crown ether, wherein the modified crown ether includes basic 18-crown-6 ether and introduces hydrophobic side chains and functional groups;

[0008] By introducing hydrophobic side chains into the molecular structure of 18-crown-6 ether, this design enables the crown ether molecules to more effectively "encapsulate" vanadium ions in water-based electrolytes, reduce the free movement of vanadium ions in the electrolyte, thereby reducing the internal resistance of the electrolyte and accelerating the migration speed of vanadium ions between electrodes.

[0009] Functional groups (such as amino and carboxyl groups) are introduced into the crown ether structure. These groups can enhance the interaction between the crown ether and the vanadium ion, and further improve the solubility and stability of the vanadium ion by forming a stable coordination complex. This design helps to improve the electrochemical performance of the electrolyte, especially the charge and discharge cycle stability at high current density.

[0010] 10-20% of graphene composite material, wherein the graphene is surface-modified by a silane coupling agent;

[0011] Selecting silane coupling agent to functionalize the graphene surface not only improves the dispersion and stability of graphene, but also enhances the interfacial compatibility of graphene with electrolyte and electrode materials. This surface modification significantly improves the conductivity and electrochemical activity of graphene, and has a positive impact on the overall conductivity of the electrolyte and the power density of the battery.

[0012] Functionalized graphene acts as a conductive channel in the electrolyte, reducing the barrier to charge transfer in the electrolyte and improving the overall response speed and charge and discharge efficiency of the battery. At the same time, the high conductivity and chemical stability of graphene also help improve the durability of the battery in long-term operation.

[0013] Through the above technical scheme, the modified crown ether and the functionalized graphene composite material are used in combination. The present invention not only improves the electrolysis efficiency of the all-vanadium liquid flow battery, but also significantly improves the cycle stability and energy efficiency of the battery.

[0014] Preferably, the hydrophobic side chains are selected from alkyl chains;

[0015] The introduction of alkyl chains improves the overall hydrophobicity of crown ethers, helps to form a more stable environment in water-based electrolytes, reduces the disordered movement of vanadium ions, and thus reduces internal resistance.

[0016] Longer alkyl chains can effectively "encapsulate" vanadium ions. This encapsulation effect helps to maintain the stability of vanadium ions in the electrolyte, reduce the free state of vanadium ions in the electrolyte, and improve their transmission efficiency.

[0017] The alkyl chain has good chemical stability and compatibility, and is not easy to undergo chemical reactions or decomposition under battery operating conditions, which is beneficial to maintaining the long-term stability of the electrolyte.

[0018] Preferably, the functional group is selected from amino and carboxyl groups;

[0019] Amino and carboxyl groups can form stable coordination bonds with vanadium ions, and this coordination effect significantly improves the solubility and migration rate of vanadium ions in the electrolyte. Amino groups have strong electron donor properties, while carboxyl groups can act as electron acceptors. Together, they can effectively balance the charge distribution in the electrolyte.

[0020] The introduction of these groups not only improves the electrochemical stability of the electrolyte, but also helps to form a more uniform distribution of vanadium ions in the electrolyte, thereby improving the performance of the battery during charging and discharging.

[0021] The introduction of amino and carboxyl groups helps to adjust the pH value of the electrolyte, optimize the acid-base environment of the electrolyte, and further improve the charge and discharge efficiency and cycle life of the battery.

[0022] Preferably, the preparation of the modified crown ether comprises the following steps:

[0023] Step 1: Initial Response

[0024] The 18-crown-6 ether is reacted with an alkyl bromide under the catalysis of an alkali metal (such as sodium or potassium). The alkyl bromide can be a long-chain alkyl bromide such as hexadecane bromide, which serves to introduce a hydrophobic side chain into the structure of the 18-crown-6 ether.

[0025] The reaction is carried out in an inert atmosphere (such as nitrogen or argon) to prevent moisture and oxygen in the air from interfering with the reaction, thereby protecting the purity and activity of the reactants and products.

[0026] The reaction temperature is 80-120°C, and the reaction time is 12-24 hours.

[0027] Step 2: Introduction of functional groups

[0028] A precursor compound containing amino and carboxyl groups, an amino acid of choice such as glycine or β-alanine, is added to the reaction mixture.

[0029] As naturally occurring functional molecules, the amino and carboxyl groups of these amino acids can react with the hydrophobic side chains on the crown ethers to further introduce new functional groups.

[0030] The concentration of the amino acid is controlled within the range of 5-10% w / w relative to 18-crown-6 ether, and such a ratio is sufficient to provide the necessary functional groups without excessively affecting the overall solubility and stability.

[0031] The pH value is adjusted to 7 to 9, and the reaction is continued at 60 to 80° C. for 6 to 12 hours. The appropriate pH value and temperature can promote the effective reaction of amino acids with crown ethers without causing unnecessary decomposition or side reactions.

[0032] Through the above technical scheme, the present invention can prepare a modified crown ether with specific structure and optimized function.

[0033] Preferably, the alkyl bromide is selected from C10-C18 alkyl chains to introduce hydrophobic side chains.

[0034] This range of alkyl chain lengths is sufficient to provide good hydrophobic properties without adding excessive bulk to the molecule. Shorter chains may not be sufficient to improve hydrophobicity, while longer chains may cause solubility issues or unwanted viscosity increases.

[0035] Through the above technical scheme, the electrochemical performance of the electrolyte can be significantly improved by selecting 18-crown-6 ether modified by the alkyl chain length, especially in application scenarios of high current density and long-term operation.

[0036] Preferably, the graphene composite material comprises a mixture of unmodified graphene and modified graphene.

[0037] Although pure modified graphene has excellent performance, it is expensive, while unmodified graphene is cheap but easy to agglomerate. By mixing the two, the material cost can be controlled while maintaining performance, achieving the optimal balance between economic benefits and performance.

[0038] Mixing unmodified graphene and modified graphene can take advantage of the advantages of both and improve the overall electrochemical performance of the electrolyte. Unmodified graphene provides high conductivity, while modified graphene enhances interface stability and dispersibility. Together, the electrolyte has better electrochemical stability and lower internal resistance.

[0039] Through the above technical solution, the application of a composite material composed of unmodified graphene and modified graphene in the electrolyte additive of all-vanadium liquid flow battery not only improves the electrochemical properties of the electrolyte, but also optimizes the cost-effectiveness.

[0040] Preferably, the preparation of the graphene composite material comprises the following steps:

[0041] Step 1: Dispersion of graphene

[0042] Select a suitable organic solvent (such as N,N-dimethylformamide or acetone) to disperse graphene in it. The concentration of graphene is set at 0.5% to 2% w / v. This concentration range ensures sufficient dispersibility without being too diluted, thereby facilitating subsequent processing and application.

[0043] The purpose of this step is to fully disperse the graphene sheets and reduce agglomeration to improve their performance and reaction efficiency in the electrolyte.

[0044] Step 2: Functionalization of graphene

[0045] 1% to 5% (relative to the weight of graphene) of silane coupling agent is added to the graphene dispersion. The silane coupling agent reacts with the functional groups on the surface of graphene to form chemical bonds, thereby improving the surface properties of graphene and increasing its stability and compatibility in the electrolyte.

[0046] The functionalization treatment is carried out at room temperature with a stirring time of 24 to 48 hours to ensure that the silane coupling agent fully reacts with the graphene surface to form a uniform functionalized layer.

[0047] Step 3: Mixing functionalized graphene with unmodified graphene

[0048] Functionalized graphene is mixed with unmodified graphene in a weight ratio of 1:1 to 4. This ratio balances cost and performance, with unmodified graphene providing high conductivity and functionalized graphene providing the necessary chemical stability and interfacial activity.

[0049] The mixed graphene is heated and stirred at 50 to 70°C for 4 to 8 hours. This step is to ensure that the two graphenes are fully mixed, improve the uniformity and dispersion of the final product, and ensure performance in the electrolyte.

[0050] The present invention also provides a method for preparing an all-vanadium liquid flow battery electrolyte additive, comprising the following steps:

[0051] Step S1: Addition and premixing of phase transfer catalyst

[0052] Phase transfer catalysts, such as tetrabutylammonium bromide or other similar compounds, are added to the graphene composites. These catalysts act as a catalyst in the chemical reaction, helping the chemical reaction and physical mixing between the graphene composites and the modified crown ethers, thereby enhancing the performance of the final additive.

[0053] The concentration of the catalyst ranges from 0.2% to 3% of the total mass of the additive, which is sufficient to achieve effective catalysis without affecting the stability of the electrolyte.

[0054] The premixing is completed within 30 to 60 minutes, which is sufficient to evenly disperse the phase transfer catalyst in the graphene composite material.

[0055] Step S2: Mixing process

[0056] The treated graphene composite material is mixed with the modified 18-crown-6 ether in an appropriate proportion and mixed at 25 to 70°C for 1 to 2 hours. This temperature and time range ensures that the materials can be fully integrated without thermal decomposition.

[0057] Step S3: Ultrasonic treatment and low temperature vacuum drying

[0058] Ultrasonic treatment was applied to further optimize the homogeneity and dispersion of the mixture, which is critical in improving the electrochemical performance of the final product. The treatment time was set to 30 to 60 minutes, which is sufficient to achieve micro-homogenization of the mixture.

[0059] Vacuum drying is performed at a temperature not exceeding 50°C to remove unreacted solvents and moisture from the mixture. This step not only ensures the dryness and purity of the additive, but also avoids any thermal degradation that may be caused by high temperature, ensuring the chemical stability and quality of the additive.

[0060] Through the above technical solution, not only the performance of graphene and modified crown ether is optimized, but also the efficiency and practicality of electrolyte additives are ensured. The additives prepared by this method can significantly improve the electrolysis efficiency of all-vanadium redox flow batteries, reduce battery internal resistance, and enhance cycle stability, thus providing a solid material foundation for the long-term stable operation of batteries.

[0061] The present invention also provides an all-vanadium liquid flow battery electrolyte, wherein the electrolyte comprises the all-vanadium liquid flow battery electrolyte additive.

[0062] The present invention provides an electrolyte additive for an all-vanadium liquid flow battery. It has the following beneficial effects:

[0063] 1. The modified crown ether used in the present invention effectively increases the solubility and migration rate of vanadium ions in the electrolyte through its hydrophobic side chain and functional groups (amino and carboxyl groups). This improvement directly increases the electrolysis rate, allowing the battery to achieve a faster reaction speed during the charge and discharge process, thereby improving the overall battery efficiency. In this way, the battery can maintain a higher power output at a high current density to meet the needs of fast charge and discharge.

[0064] 2. The graphene composite material introduced in the present invention significantly reduces the internal resistance of the electrolyte through its excellent electrical conductivity. Unmodified graphene provides a good electrical conductivity channel, while functionalized graphene enhances its compatibility with the electrolyte through its surface modification, further optimizing the conductive environment of the electrolyte. This dual effect enables the battery to achieve lower energy loss during operation and improves energy utilization efficiency, especially under continuous long-term operation and high-load conditions.

[0065] 3. The present invention significantly enhances the chemical stability and physical uniformity of the electrolyte through the synergistic effect of the modified crown ether and graphene composite material, thereby reducing material degradation and electrochemical side reactions during the charge and discharge cycle. This improvement in stability directly affects the cycle life of the battery, allowing the battery to maintain a low performance decay rate during long-term use. As a result, the maintenance cost of the battery is reduced, making it more suitable for commercial and industrial-scale applications, especially in situations where reliable energy storage solutions are required.

[0066] 4. The all-vanadium liquid flow battery electrolyte additive of the present invention achieves a comprehensive improvement in battery performance, including higher electrolysis efficiency, lower internal resistance, more stable charge and discharge cycles, and longer battery life. These advantages make the all-vanadium liquid flow battery technology of the present invention more competitive in the energy storage market, meeting the dual requirements of high efficiency and high reliability of modern energy systems. DETAILED DESCRIPTION

[0067] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0068] Embodiment 1:

[0069] Step 1: Preparation of modified crown ethers

[0070] 1. In a 500 mL three-necked flask, add 50 g of 18-crown-6 ether.

[0071] 2. Add 10 g of hexadecane bromide (C 16 H 33 Br) as a hydrophobic side chain introduction.

[0072] 3. Under nitrogen protection, add 0.5 g of sodium metal as a catalyst.

[0073] 4. Heat the reaction mixture to 100°C and stir the reaction at 80-120°C for 16 hours.

[0074] 5. After the reaction was completed, 5 g of β-alanine was added to the reaction mixture in a concentration range of 5% w / w of 18-crown-6 ether.

[0075] 6. Adjust the pH of the reaction mixture to 8 and continue the reaction at 70°C for 8 hours.

[0076] 7. After the reaction is completed, cool to room temperature to obtain modified crown ether.

[0077] Step 2: Preparation of graphene composites

[0078] 1. Disperse 2 g of graphene in 200 mL of N,N-dimethylformamide, with a graphene concentration of 1% w / v.

[0079] 2. Add 0.1 g of silane coupling agent (equivalent to 5% of the weight of graphene) to the graphene dispersion and stir at room temperature for 24 hours.

[0080] 3. The functionalized graphene and unmodified graphene were mixed in a weight ratio of 3:1, and then heated and stirred at 60 °C for 6 hours.

[0081] 4. Obtain a uniformly dispersed graphene composite material.

[0082] Step 3: Preparation of additives

[0083] 1. Add 1 g of tetrabutylammonium bromide (equivalent to 2% of the total mass of the additive) to the graphene composite material and premix for 40 minutes.

[0084] 2. Add the treated graphene composite material to 90 g of modified 18-crown-6 ether and mix at 25°C for 1 hour.

[0085] 3. Treat the mixture with ultrasound (frequency 30 kHz) for 45 minutes.

[0086] 4. The mixture was dried at 50°C and -0.1 MPa for 3 hours using low temperature vacuum drying technology to obtain an electrolyte additive.

[0087] Embodiment 2:

[0088] Step 1: Preparation of modified crown ethers

[0089] 1. In a 500 mL three-necked flask, add 40 g of 18-crown-6 ether.

[0090] 2. Add 6 g of bromodecane (C 10 H 21 Br).

[0091] 3. Under nitrogen protection, add 0.3 g of potassium metal as a catalyst.

[0092] 4. Heat the reaction mixture to 90°C and stir the reaction at 80-120°C for 20 hours.

[0093] 5. After the reaction was completed, 4 g of glycine was added to the reaction mixture in a concentration range of 10% w / w of 18-crown-6 ether.

[0094] 6. Adjust the pH of the reaction mixture to 7.5 and continue the reaction at 65°C for 10 hours.

[0095] 7. After the reaction is completed, cool to room temperature to obtain modified crown ether.

[0096] Step 2: Preparation of graphene composites

[0097] 1. Disperse 1 g of graphene in 100 mL of N,N-dimethylformamide, with a graphene concentration of 1% w / v.

[0098] 2. Add 0.05 g of silane coupling agent (equivalent to 5% of the weight of graphene) to the graphene dispersion and stir at room temperature for 36 hours.

[0099] 3. The functionalized graphene and unmodified graphene were mixed in a weight ratio of 2:1, and then heated and stirred at 50 °C for 5 hours.

[0100] 4. Obtain a uniformly dispersed graphene composite material.

[0101] Step 3: Preparation of additives

[0102] 1. Add 0.6 g of tetrabutylammonium bromide (equivalent to 1.5% of the total mass of the additive) to the graphene composite material and premix for 50 minutes.

[0103] 2. The treated graphene composite material was added to 80 g of modified 18-crown-6 ether and mixed at 30 °C for 1.5 hours.

[0104] 3. Treat the mixture with ultrasound (frequency 25 kHz) for 40 minutes.

[0105] 4. The mixture was dried at 40°C and -0.09 MPa for 4 hours using low temperature vacuum drying technology to obtain an electrolyte additive.

[0106] Embodiment 3:

[0107] Step 1: Preparation of modified crown ethers

[0108] 1. In a 500 mL three-necked flask, add 45 g of 18-crown-6 ether.

[0109] 2. Add 8 g of dodecane bromide (C 12 H 25 Br).

[0110] 3. Under nitrogen protection, add 0.4 g of sodium metal as a catalyst.

[0111] 4. Heat the reaction mixture to 110°C and stir the reaction at 80-120°C for 18 hours.

[0112] 5. After the reaction was completed, 4.5 g of β-alanine was added to the reaction mixture in a concentration range of 8% w / w of 18-crown-6 ether.

[0113] 6. Adjust the pH of the reaction mixture to 8 and continue the reaction at 75°C for 9 hours.

[0114] 7. After the reaction is completed, cool to room temperature to obtain modified crown ether.

[0115] Step 2: Preparation of graphene composites

[0116] 1. Disperse 1.5 g of graphene in 150 mL of N,N-dimethylformamide, with a graphene concentration of 1% w / v.

[0117] 2. Add 0.075 g of silane coupling agent (equivalent to 5% of the weight of graphene) to the graphene dispersion and stir at room temperature for 30 hours.

[0118] 3. The functionalized graphene was mixed with unmodified graphene in a weight ratio of 1:1, and then heated and stirred at 55 °C for 6 h.

[0119] 4. Obtain a uniformly dispersed graphene composite material.

[0120] Step 3: Preparation of additives

[0121] 1. Add 0.8 g of tetrabutylammonium bromide (equivalent to 2.2% of the total mass of the additive) to the graphene composite material and premix for 45 minutes.

[0122] 2. The treated graphene composite material was added to 85 g of modified 18-crown-6 ether and mixed at a temperature of 28°C for 1.2 hours.

[0123] 3. Treat the mixture with ultrasound (frequency 35 kHz) for 50 minutes.

[0124] 4. The mixture was dried for 2.5 hours at 45°C and -0.095 MPa by low temperature vacuum drying technology to obtain an electrolyte additive.

[0125] Embodiment 4:

[0126] Step 1: Preparation of modified crown ethers

[0127] 1. In a 500 mL three-necked flask, add 55 g of 18-crown-6 ether.

[0128] 2. Add 12g of tetradecane bromide (C 14 H 29 Br).

[0129] 3. Under nitrogen protection, add 0.6 g of potassium metal as a catalyst.

[0130] 4. Heat the reaction mixture to 95°C and stir the reaction at 80-120°C for 24 hours.

[0131] 5. After the reaction was completed, 6 g of glycine was added to the reaction mixture in a concentration range of 10% w / w of 18-crown-6 ether.

[0132] 6. Adjust the pH of the reaction mixture to 8 and continue the reaction at 70°C for 10 hours.

[0133] 7. After the reaction is completed, cool to room temperature to obtain modified crown ether.

[0134] Step 2: Preparation of graphene composites

[0135] 1. Disperse 2 g of graphene in 200 mL of N,N-dimethylformamide, with a graphene concentration of 1% w / v.

[0136] 2. Add 0.1 g of silane coupling agent (equivalent to 5% of the weight of graphene) to the graphene dispersion and stir at room temperature for 48 hours.

[0137] 3. The functionalized graphene and unmodified graphene were mixed in a weight ratio of 4:1, and then heated and stirred at 65 °C for 7 hours.

[0138] 4. Obtain a uniformly dispersed graphene composite material.

[0139] Step 3: Preparation of additives

[0140] 1. Add 0.4 g of tetrabutylammonium bromide (equivalent to 0.8% of the total mass of the additive) to the graphene composite material and premix for 35 minutes.

[0141] 2. The treated graphene composite material was added to 88 g of modified 18-crown-6 ether and mixed at 30°C for 2 hours.

[0142] 3. Treat the mixture with ultrasound (frequency 40 kHz) for 55 minutes.

[0143] 4. The mixture was dried at 50°C and -0.1 MPa for 3 hours using low temperature vacuum drying technology to obtain an electrolyte additive.

[0144] Embodiment 5:

[0145] Step 1: Preparation of modified crown ethers

[0146] 1. In a 500 mL three-necked flask, add 60 g of 18-crown-6 ether.

[0147] 2. Add 15g of octadecane bromide (C 18 H 37 Br).

[0148] 3. Under nitrogen protection, add 0.7 g of potassium metal as a catalyst.

[0149] 4. Heat the reaction mixture to 110°C and stir the reaction at 80-120°C for 22 hours.

[0150] 5. After the reaction was completed, 7 g of glycine was added to the reaction mixture in a concentration range of 10% w / w of 18-crown-6 ether.

[0151] 6. Adjust the pH of the reaction mixture to 9 and continue the reaction at 75°C for 12 hours.

[0152] 7. After the reaction is completed, cool to room temperature to obtain modified crown ether.

[0153] Step 2: Preparation of graphene composites

[0154] 1. Disperse 3 g of graphene in 300 mL of N,N-dimethylformamide, with a graphene concentration of 1% w / v.

[0155] 2. Add 0.15 g of silane coupling agent (equivalent to 5% of the weight of graphene) to the graphene dispersion and stir at room temperature for 24 hours.

[0156] 3. The functionalized graphene was mixed with unmodified graphene in a weight ratio of 1:1, and then heated and stirred at 70 °C for 4 h.

[0157] 4. Obtain a uniformly dispersed graphene composite material.

[0158] Step 3: Preparation of additives

[0159] 1. Add 2.5 g of tetrabutylammonium bromide (equivalent to 3% of the total mass of the additive) to the graphene composite material and premix for 60 minutes.

[0160] 2. Add the treated graphene composite material to 85 g of modified 18-crown-6 ether and mix at 35 °C for 1.5 hours.

[0161] 3. Treat the mixture with ultrasound (frequency 35 kHz) for 30 minutes.

[0162] 4. The mixture was dried at 50°C and -0.1 MPa for 2 hours using low temperature vacuum drying technology to obtain an electrolyte additive.

[0163] Comparative Examples 1 to 10:

[0164] Comparative Example 1: Different from the present invention, Comparative Example 1 uses unmodified 18-crown-6 ether instead of modified 18-crown-6 ether with introduced hydrophobic side chains and functional groups. The remaining preparation steps are the same as those of the present invention.

[0165] Comparative Example 2: Different from the present invention, Comparative Example 2 uses modified 18-crown-6 ether, but does not introduce functional groups, and only adds hydrophobic side chains. The remaining preparation steps are the same as those of the present invention.

[0166] Comparative Example 3: Different from the present invention, the graphene in Comparative Example 3 is surface-modified using a non-specific functionalizing agent (general polymer) instead of a silane coupling agent. The remaining preparation steps are the same as those of the present invention.

[0167] Comparative Example 4: Different from the present invention, in the preparation of the graphene composite material in Comparative Example 4, no functionalizing agent is used at all. The remaining preparation steps are the same as those of the present invention.

[0168] Comparative Example 5: Different from the present invention, Comparative Example 5 uses modified 18-crown-6 ether and functionalized graphene, but the ratio of functionalized graphene to modified crown ether is different from that of the present invention, where the ratio of graphene is increased to 30% and the ratio of modified crown ether is reduced to 70%. The remaining preparation steps are the same as those of the present invention.

[0169] Comparative Example 6: Different from the present invention, Comparative Example 6 uses only one functional group (only carboxyl group) in the modified crown ether instead of using both amino group and carboxyl group. The remaining preparation steps are the same as those of the present invention.

[0170] Comparative Example 7: Different from the present invention, in Comparative Example 7, unmodified graphene is completely excluded from the graphene composite material, and 100% functionalized graphene is used. The remaining preparation steps are the same as those of the present invention.

[0171] Comparative Example 8: Different from the present invention, Comparative Example 8 uses a completely different type of crown ether (12-crown-4) instead of 18-crown-6 ether. The remaining preparation steps are the same as those of the present invention.

[0172] Comparative Example 9: Different from the present invention, in the preparation of the modified crown ether, no hydrophobic side chain or functional group is used, but the proportion of the solvent stabilizer in the electrolyte is increased to explore the effect of not modifying the crown ether but enhancing the solvent stability. The remaining preparation steps are the same as those of the present invention.

[0173] Comparative Example 10: Different from the present invention, in the preparation of the graphene composite material, a different organic solvent (acetone) is used instead of N,N-dimethylformamide. The remaining preparation steps are the same as those of the present invention.

[0174] Comparative experiment 1: Electrochemical performance test

[0175] Experimental setup:

[0176] Electrolyte preparation:

[0177] 1.6M VOSO4

[0178] 2.5M H2SO4

[0179] Corresponding electrolyte additives (Example or Comparative Example additives)

[0180] Preparation steps of electrolyte:

[0181] 1. Preparation of basic electrolyte:

[0182] Weigh the required amount of VOSO4·xH2O and dissolve it in an appropriate amount of deionized water.

[0183] Gradually add 2.5M H2SO4 to the solution and stir well.

[0184] Adjust the solution volume to a concentration of 1.6 M VOSO4 and 2.5 M H2SO4.

[0185] 2. Addition of additives:

[0186] The electrolyte was divided into 15 portions, each of 500 mL.

[0187] Add the corresponding additives to each electrolyte respectively, ensure the same concentration of additives (add according to the optimal concentration of each additive), and stir to mix evenly.

[0188] Battery Assembly:

[0189] The same electrode materials and cell configuration were used.

[0190] The prepared electrolyte is injected into the assembled all-vanadium liquid flow battery.

[0191] Experimental procedures

[0192] 1. Charging: 300mA / cm 2 The battery is charged with a current density of 1.6 V.

[0193] 2. Discharge: 300mA / cm 2 The battery was discharged at a current density of 0.8 V until the voltage dropped to 0.8 V.

[0194] 3. Cycle test: Repeat the charge and discharge cycle 20 times, and record the charging time, discharge time, open circuit voltage and battery internal resistance of each cycle.

[0195] 4. Data collection: record energy efficiency (energy efficiency = discharge capacity / charge capacity × 100%), coulombic efficiency (coulombic efficiency = discharge current / charge current × 100%), open circuit voltage and battery internal resistance.

[0196] The experimental results are shown in Table 1:

[0197] Table 1 Electrochemical performance test data of electrolyte additives of the present invention and comparative examples

[0198] Additive samples Energy efficiency (%) Coulombic efficiency (%) Open circuit voltage(V) Battery internal resistance (mΩ) Example 1 86.5 95.3 1.5 12.4 Example 2 85.7 94.8 1.52 13.1 Example 3 87.1 95.1 1.51 11.9 Example 4 85.9 95 1.5 12.7 Example 5 86.2 95.2 1.51 12.5 Comparative Example 1 78.3 88.5 1.4 18.6 Comparative Example 2 80.2 90.4 1.42 17.8 Comparative Example 3 81.5 91 1.45 16.5 Comparative Example 4 79.8 89.3 1.41 18.2 Comparative Example 5 83.6 92.5 1.47 15.3 Comparative Example 6 82.1 91.8 1.44 16.7 Comparative Example 7 84 93 1.48 14.9 Comparative Example 8 77.9 88 1.39 19 Comparative Example 9 80.7 90.8 1.43 17.4 Comparative Example 10 81.2 91.2 1.44 16.9

[0199] From the data in Table 1, we can get:

[0200] The embodiments of the present invention are generally superior to the comparative examples in terms of energy efficiency, coulomb efficiency, open circuit voltage and battery internal resistance. Specifically, the energy efficiency and coulomb efficiency of embodiments 1-5 of the present invention are both over 85% and 94%, which are significantly higher than the highest values ​​of 83.6% and 93.0% in the comparative examples. In addition, the open circuit voltage and battery internal resistance of the embodiments of the present invention show more stable and better performance.

[0201] Analysis of material action mechanism

[0202] Effect of modified crown ethers:

[0203] Hydrophobic side chains and functional groups: In the present invention, the interaction between 18-crown-6 ether and vanadium ions is enhanced by introducing hydrophobic side chains and amino and carboxyl groups as functional groups. The hydrophobic side chains help to improve the structural stability of the electrolyte and reduce the disordered movement of vanadium ions in the electrolyte, thereby reducing the internal resistance of the battery. The amino and carboxyl groups form stable coordination complexes with vanadium ions, thereby improving the ion transmission efficiency and the charge and discharge capacity of the battery, which explains the higher energy efficiency and coulomb efficiency of the embodiments of the present invention.

[0204] Performance of Comparative Examples 2 and 6: Comparative Example 2 only introduced hydrophobic side chains without adding functional groups. The results showed that although its performance was better than that of the unmodified Comparative Example 1, it was still lower than that of the embodiment of the present invention. Comparative Example 6 used only one functional group and failed to reach the performance level of the embodiment of the present invention, proving the importance of the synergistic effect of the two functional groups.

[0205] The role of functionalized graphene:

[0206] Application of silane coupling agent: In the present invention, graphene is functionalized using a silane coupling agent, which significantly improves the conductivity of graphene and its compatibility with the electrolyte. The silane coupling agent optimizes the dispersibility and stability of graphene by forming a stable chemical bond on the graphene surface, thereby reducing the charge transfer barrier in the battery. As shown in Comparative Example 3, the performance of graphene treated with a non-specific functionalizing agent is significantly inferior to that of the present invention embodiment using a silane coupling agent.

[0207] Performance of Comparative Examples 4 and 10: Comparative Example 4 without using any functionalizing agent and Comparative Example 10 using different solvents showed no advantages in terms of electrolysis rate and battery internal resistance, emphasizing the importance of specific functionalization treatment for improving electrolyte performance.

[0208] The embodiments of the present invention effectively improve the electrochemical performance of the all-vanadium liquid flow battery by comprehensively utilizing modified crown ethers and functionalized graphene. The modified crown ether optimizes the transport and stability of vanadium ions through the dual effects of its hydrophobicity and functional groups, while the application of functionalized graphene further enhances the conductivity of the electrolyte and the overall electrochemical stability of the battery. These technological innovations significantly improve the energy efficiency and coulombic efficiency of the battery, while reducing the internal resistance of the battery and increasing the electrolysis rate, so that the battery performs well at high current density, which is of great significance for commercial applications and practical operations.

[0209] Comparative experiment 2: Cyclic stability test

[0210] Experimental setup

[0211] Electrolyte preparation:

[0212] As in Experiment 1, a base electrolyte of 1.6 M VOSO4 and 2.5 M H2SO4 was used.

[0213] The corresponding electrolyte additives are added at the optimal concentration.

[0214] Experimental steps:

[0215] 1. Electrolyte preparation: Prepare and add additives according to the method of comparative experiment 1.

[0216] 2. Battery assembly: Use standard all-vanadium liquid flow battery assembly to ensure that each battery has the same configuration.

[0217] 3. Cycle test: at 300mA / cm 2 Perform at least 100 charge and discharge cycles at a current density of 1.5 %. Record performance data every 10 cycles, including open circuit voltage, charge and discharge capacity, battery internal resistance, etc.

[0218] The experimental data are shown in Table 2:

[0219] Table 2 Cyclic stability test data of electrolyte additives of the present invention and comparative examples

[0220]

[0221]

[0222] From the data in Table 2, we can get:

[0223] The examples of the present invention show lower capacity decay rate and internal resistance increase during the electrolyte circulation process, and have significant performance advantages compared with the comparative examples. These data reveal that the additives of the present invention significantly improve the performance stability of all-vanadium redox flow batteries.

[0224] Material action analysis

[0225] Synergistic effect of modified crown ethers:

[0226] The modified crown ether used in the present invention plays a key role in the battery recycling process by combining hydrophobic side chains and amino and carboxyl functional groups. These functional groups not only enhance the interaction with vanadium ions and improve the migration efficiency of ions, but also help buffer the acid-base changes in the electrolyte, thereby maintaining the chemical stability of the electrolyte and preventing excessive decomposition of the electrolyte.

[0227] Impact of graphene composites:

[0228] Graphene functionalized with silane coupling agents plays an important role in the electrolyte. This specific surface modification enhances the interfacial interaction between graphene and the electrolyte, effectively reducing the overpotential on the electrode surface and the internal resistance of the battery during the cycle. In addition, the good conductivity and structural stability of graphene also help to maintain a uniform charge distribution on the electrode surface during battery charging and discharging, reducing local overload and loss of electrode materials.

[0229] Comparative analysis:

[0230] The comparative examples using unmodified crown ethers and graphene without specific functionalization showed higher capacity decay rates and increased internal resistance, indicating that unoptimized additives cannot effectively support the long-term stability of the electrolyte and battery performance, especially in applications at high current densities.

[0231] Especially for Comparative Examples 4 and 8, the performance degradation of the samples without using functionalizing agents or using completely different types of crown ethers (such as 12-crown-4) is more obvious, which further confirms the importance of selecting the right crown ether type and properly functionalizing graphene.

[0232] The present invention achieves all-round optimization of electrolyte performance by introducing specific chemical functional groups and surface modification strategies into modified crown ether and graphene composite materials. This strategy not only improves the electrochemical performance of the battery, but also significantly improves the cycle stability of the battery, enabling the battery to maintain low performance degradation under high load and long-term operation conditions, providing strong technical support for the commercialization and industrial application of all-vanadium redox flow batteries.

[0233] Comparative experiment 3: Starting voltage comparison

[0234] Experimental setup

[0235] Electrolyte preparation:

[0236] Using a basic electrolyte of 1.6M VOSO4 and 2.5M H2SO4, the additives were prepared and added according to the method of Comparative Experiment 1.

[0237] Experimental steps:

[0238] 1. Electrolyte preparation: Prepare the electrolyte containing additives according to the steps described in Comparative Experiment 1.

[0239] 2. Battery assembly: Use standard all-vanadium liquid flow battery assembly.

[0240] 3. Determine the starting voltage: Set up the electrochemical workstation to perform linear sweep voltammetry (LSV) test to determine the starting voltage at 300 mA / cm 2 The minimum voltage required to achieve stable output at the current density. The scan rate was set to 5mV / s, and the voltage was scanned from the open circuit voltage to the voltage at which the electrolyte was fully electrolyzed.

[0241] The experimental results are shown in Table 3:

[0242] Table 3 Comparison of electrolysis rate of electrolyte additives in the embodiments of the present invention and the comparative examples

[0243] Additive samples <![CDATA[Minimum voltage (V) to reach 300 mA / cm 2 > Example 1 0.75 Example 2 0.77 Example 3 0.74 Example 4 0.76 Example 5 0.78 Comparative Example 1 0.85 Comparative Example 2 0.84 Comparative Example 3 0.83 Comparative Example 4 0.86 Comparative Example 5 0.82 Comparative Example 6 0.81 Comparative Example 7 0.8 Comparative Example 8 0.87 Comparative Example 9 0.85 Comparative Example 10 0.84

[0244] From the experimental data in Table 3, we can get:

[0245] The electrolyte formulation of the embodiment of the present invention exhibits a lower starting voltage. Compared with the comparative example, these data highlight the innovation and effectiveness of the present invention in optimizing the electrolyte formulation.

[0246] Analysis of the mechanism of action of substances

[0247] Optimization of electrolysis kinetics of modified crown ethers:

[0248] The present invention significantly improves the solubility and mobility of vanadium ions by introducing hydrophobic side chains and amino and carboxyl functional groups into 18-crown-6 ether. This structural change improves the ion conductivity of the electrolyte and reduces the potential threshold required to reach the target current density. This is particularly evident in Example 3, which has the lowest starting voltage.

[0249] The enhanced vanadium ion transport channels provided by the modified crown ethers make the electrolysis reaction more rapid and efficient at high current density.

[0250] Interfacial conduction properties of graphene composites:

[0251] The addition of functionalized graphene optimizes the conductivity of the electrolyte, and the use of silane coupling agent enhances the compatibility and interface stability of graphene and electrolyte, reducing the interface impedance. This feature is crucial for reducing the starting voltage, allowing the electrolyte to quickly reach the required current output at a lower voltage.

[0252] Comparative analysis:

[0253] The samples using unmodified crown ether and unfunctionalized graphene in the comparative examples (such as comparative examples 1 and 4) showed a higher starting voltage. These results verify the key role of modified crown ether and functionalized graphene in improving the electrochemical performance of the electrolyte.

[0254] In the comparative examples, the samples in which graphene was treated with non-specific functionalizing agents (such as comparative example 3) and the formulations in which the hydrophobic side chains and functional groups were not fully optimized (such as comparative example 6) also failed to exhibit performance matching that of the present invention, further emphasizing the importance of selecting a specific chemical modification strategy in the present invention.

[0255] The formulation of the present invention achieves optimized starting voltage performance under high current density operating conditions through precise chemical design and synergistic effects of substances, which is crucial for improving the operating efficiency of all-vanadium liquid flow batteries and reducing energy losses.

[0256] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. An all-vanadium redox flow battery electrolyte additive, characterized in that: The additive comprises the following components by weight percentage: 80-90% of modified crown ether, wherein the modified crown ether includes basic 18-crown-6 ether and introduces hydrophobic side chains and functional groups; 10-20% of graphene composite material, wherein the graphene is surface-modified by a silane coupling agent.

2. The electrolyte additive for all-vanadium redox flow battery according to claim 1, characterized in that: The hydrophobic side chain is selected from an alkyl chain, and the functional group is selected from an amino group and a carboxyl group.

3. The electrolyte additive for all-vanadium redox flow battery according to claim 1, characterized in that: The preparation of the modified crown ether comprises the following steps: The 18-crown-6 ether is reacted with an alkyl bromide under alkali metal catalysis in an inert atmosphere at 80 to 120° C. for 12 to 24 hours, Adding a precursor compound containing amino and carboxyl groups to the reaction mixture, wherein the precursor compound is an amino acid selected from glycine or β-alanine, and the concentration thereof is in the range of 5 to 10% w / w relative to 18-crown-6 ether; The pH value of the reaction mixture is adjusted to 7-9, and the reaction is continued at 60-80° C. for 6-12 hours to introduce functional groups.

4. The electrolyte additive for all-vanadium redox flow battery according to claim 1, characterized in that: The alkyl bromide is selected from C10-C18 alkyl chains to introduce hydrophobic side chains.

5. The electrolyte additive for all-vanadium redox flow battery according to claim 1, characterized in that: The graphene composite material comprises a mixture of unmodified graphene and modified graphene.

6. The electrolyte additive for all-vanadium redox flow battery according to claim 1, characterized in that: The preparation of the graphene composite material comprises the following steps: Dispersing graphene in a selected organic solvent, wherein the concentration of graphene is 0.5 to 2% w / v; Adding a silane coupling agent to the graphene dispersion in an amount of 1 to 5% of the weight of the graphene, and stirring at room temperature for 24 to 48 hours to achieve functionalization of the graphene; The functionalized graphene and the unmodified graphene are mixed in a weight ratio of 1:1 to 4, and then heated and stirred at 50 to 70° C. for 4 to 8 hours to ensure thorough mixing and uniform dispersion.

7. The electrolyte additive for all-vanadium redox flow battery according to claim 6, characterized in that: The organic solvent is N,N-dimethylformamide.

8. A method for preparing an all-vanadium redox flow battery electrolyte additive, used for preparing the all-vanadium redox flow battery electrolyte additive as claimed in any one of claims 1 to 7, characterized in that: The following steps are involved: Adding 0.2-3% of the total weight of the additive into the graphene composite material is a phase transfer catalyst, and premixing is performed within 30-60 minutes; Adding the treated graphene composite material to the modified 18-crown-6 ether and mixing at a temperature of 25 to 70° C. for 1 to 2 hours to form an additive mixture; After the mixture is ultrasonically treated for 30 to 60 minutes, the mixture is dried by low-temperature vacuum drying at a temperature not exceeding 50° C. to remove unreacted solvent and water, thereby preparing an electrolyte additive.

9. The preparation method according to claim 8, characterized in that: The phase transfer catalyst is tetrabutylammonium bromide.

10. An all-vanadium redox flow battery electrolyte, characterized in that: The electrolyte comprises the all-vanadium redox flow battery electrolyte additive according to any one of claims 1 to 7.