Perovskite solar cell based on self-assembled monomolecular layer and preparation method thereof
By using self-assembled single-molecular layer and thermal evaporation-solution method in perovskite solar cells, the problems of unstable hole transport layer material and uneven film formation of perovskite film are solved, and the problem of The preparation of high-efficiency perovskite solar cells reduces manufacturing costs and improves device performance.
Patent Information
- Application Number
- CN202411400195.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-06
AI Technical Summary
The hole transport layer materials in existing perovskite solar cells are unstable and the perovskite film is uneven, resulting in low device performance and high manufacturing cost.
The perovskite absorption layer was prepared by self-assembled single molecule layer as the hole transport layer, combined with the thermal evaporation-solution method, and the ultra-thin self-assembled single molecule layer was anchored on the ITO conductive glass, and uniform pertituitum was obtained by annealing treatment. Ore film.
It improves the stability and performance of perovskite solar cells, reduces device manufacturing costs, and enhances the compatibility of perovskite films and substrates.
Smart Images

Figure CN119095451A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solar cells, and in particular relates to a perovskite solar cell based on a self-assembled monomolecular layer and a preparation method thereof. Background Art
[0002] Perovskite solar cells have attracted widespread attention due to their high efficiency, low cost and simple preparation process. Perovskite is a material with an ABX3 crystal structure, where A is an organic cation, B is a metal cation and X is a halogen anion. This structure gives perovskite materials excellent photoelectric properties, such as high light absorption coefficient, long carrier diffusion length and low carrier recombination rate. The efficiency of perovskite solar cells has increased rapidly in the past decade, from the initial 3.8% to the current 26.7%. The perovskite device structure mainly includes conductive glass, hole transport layer, perovskite absorption layer, electron transport layer and metal electrode. The main function of the hole transport layer is to extract and transport holes, and it has a great influence on the crystallization and film formation of the perovskite absorption layer in the preparation of inverse perovskite cells. Therefore, preparing a high-performance hole transport layer is an important method to improve battery performance.
[0003] In perovskite solar cells, common hole transport layers include conductive polymer films, metal oxides, and polymer materials. However, conductive polymers (such as PEDOT:PSS) have high production costs and are prone to aging due to their hygroscopic and acidic properties. They also have poor thermal stability at the interface with perovskite. Metal oxides (such as NiO x ) has multiple oxidation states and is prone to undergo redox reactions with perovskite materials, leading to the decomposition of perovskite. The large surface contact angle of polymer materials (such as PTAA) leads to major problems in the preparation of uniform perovskite films by solution method, thus limiting the preparation of inverse perovskite solar cells. Summary of the invention
[0004] In order to solve the instability of the widely used hole transport layer materials and the problem of uniform film formation of perovskite thin films on the hole transport layer, and reduce the device manufacturing cost, the present invention provides a perovskite solar cell based on a self-assembled monolayer and a preparation method thereof. The hole transport layer of the inverted perovskite solar cell is obtained by spin coating the self-assembled monolayer, and the perovskite absorption layer is prepared by a thermal evaporation-solution method, so as to further optimize the device performance.
[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: A method for preparing a perovskite solar cell based on a self-assembled monolayer, which uses a series of ultra-thin self-assembled monolayers anchored on indium-doped tin oxide ITO transparent conductive glass, then prepares the perovskite absorption layer by a thermal evaporation-solution method, and then prepares the electron transport layer and the metal electrode, ultimately realizing the preparation of an inverted perovskite solar cell.
[0006] The method for preparing a perovskite solar cell based on a self-assembled monolayer described in the present invention specifically comprises the following steps: (1) Clean the ITO conductive glass. Wipe the ITO conductive glass with a dust-free cloth moistened with ethanol, then ultrasonicate it in acetone and ethanol respectively, then rinse it with deionized water, blow dry it with nitrogen, and treat it with UV for later use; (2) Preparation of a hole transport layer, dissolving a self-assembled monolayer material in an organic solvent, depositing it on the above-mentioned ITO conductive glass by spin coating, and obtaining a hole transport layer by annealing; (3) Preparation of perovskite absorption layer: obtaining an inorganic salt skeleton on the hole transport layer through a thermal evaporation process, then covering the inorganic salt skeleton with an organic salt, and finally obtaining a perovskite film through annealing treatment; (4) Preparation of electron transport layer: preparing fullerene and its derivatives and hole blocking layer on the perovskite absorption layer to obtain a uniform electron transport layer; (5) Preparation of metal electrodes: depositing metal electrodes on the electron transport layer by thermal evaporation process.
[0007] Furthermore, in the step (2), the self-assembled monolayer material is one or more of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), [2-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphonic acid (Me-2PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), [4-(9H-carbazole-9-yl)butyl]phosphonic acid (4PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), and [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid (MeO-4PACz), and the concentration thereof is 0.3-2.5 mg / mL. The organic solvent is ethanol or isopropanol.
[0008] Furthermore, in the step (2), the spin coating speed is 3000-6000 rpm, and the spin coating time is 30-50 s.
[0009] Furthermore, in the step (2), the annealing temperature is 100-150°C and the time is 5-30 min.
[0010] Furthermore, in step (3), the inorganic salt skeleton is PbI 2 、PbCl 2 、PbBr 2 The organic salt is one or more of MACl, MABr, MAI, FACl, FABr and FAI.
[0011] Furthermore, the annealing treatment in step (3) is a two-step annealing, wherein the first annealing temperature is 130-170°C and the time is 0-20 min; the second annealing temperature is 80-130°C and the time is 0-20 min.
[0012] Furthermore, in step (4), the electron transport layer is prepared by a solution method or a thermal evaporation method, and its thickness is 5-50 nm.
[0013] Furthermore, in the step (5), the metal electrode is one of Au, Ag, and Cu, and has a thickness of 60-150 nm.
[0014] The perovskite solar cell uses the self-assembled monolayer obtained by the preparation method of the present invention as a hole transport layer.
[0015] Beneficial effects of the present invention: The present invention provides a method for preparing a perovskite solar cell based on a self-assembled monolayer, which uses a series of ultra-thin self-assembled monolayers anchored on indium-doped tin oxide ITO transparent conductive glass, and then prepares a perovskite absorption layer by a thermal evaporation-solution method, and then prepares an electron transport layer and a metal electrode, and finally obtains a high-efficiency inverse perovskite solar cell. Compared with the commonly used hole transport layer, the self-assembled monolayer has better stability and low production cost. In addition, the present invention prepares the perovskite absorption layer by a thermal evaporation-solution method, which improves the compatibility of the perovskite film and the substrate surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A schematic diagram of the structure of a perovskite solar cell based on a self-assembled monolayer according to the present invention; Figure 2 JV curves of the perovskite solar cells obtained in Examples 1-4 and Comparative Example 1. DETAILED DESCRIPTION
[0017] The purpose of the present invention is to provide a perovskite solar cell based on a self-assembled monolayer and a preparation method thereof. An ultra-thin self-assembled monolayer is anchored on an ITO transparent conductive glass, and a perovskite absorption layer is prepared by a thermal evaporation-solution method, thereby solving the instability of the widely used hole transport layer material and the uniform film formation of the perovskite film on the hole transport layer, and reducing the device manufacturing cost.
[0018] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. Example 1
[0019] A method for preparing a perovskite solar cell based on a self-assembled monolayer specifically comprises the following steps: (1) Clean the ITO conductive glass. Wipe the ITO conductive glass with a dust-free cloth moistened with ethanol, then ultrasonicate it in acetone and ethanol respectively, then rinse it with deionized water, blow dry it with nitrogen, and treat it with UV for later use; (2) Preparation of a hole transport layer, dissolving a self-assembled monolayer material in an organic solvent, depositing it on the above-mentioned ITO conductive glass by spin coating, and obtaining a hole transport layer by annealing; (3) Preparation of perovskite absorption layer: obtaining an inorganic salt skeleton on the hole transport layer through a thermal evaporation process, then covering the inorganic salt skeleton with an organic salt, and finally obtaining a perovskite film through annealing treatment; (4) Preparation of electron transport layer: preparing fullerene and its derivatives and hole blocking layer on the perovskite absorption layer to obtain a uniform electron transport layer; (5) Preparation of metal electrodes: depositing metal electrodes on the electron transport layer by thermal evaporation process.
[0020] Furthermore, in the step (2), the self-assembled monolayer material is [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and its concentration is 1.0 mg / mL. The organic solvent is ethanol.
[0021] Furthermore, in the step (2), the spin coating speed is 6000 rpm and the spin coating time is 30 s.
[0022] Furthermore, in the step (2), the annealing temperature is 150°C and the time is 15 min.
[0023] Furthermore, in step (3), the inorganic salt skeleton is PbI 2 The organic salts are MABr and FAI.
[0024] Furthermore, the annealing treatment in step (3) is a two-step annealing, wherein the first annealing temperature is 150°C and the time is 10 min; and the second annealing temperature is 100°C and the time is 10 min.
[0025] Furthermore, in step (4), the electron transport layer is prepared by a solution method and has a thickness of 20 nm.
[0026] Furthermore, in the step (5), the metal electrode is Cu, and its thickness is 120 nm. Example 2
[0027] A method for preparing a perovskite solar cell based on a self-assembled monolayer specifically comprises the following steps: (1) Clean the ITO conductive glass. Wipe the ITO conductive glass with a dust-free cloth moistened with ethanol, then ultrasonicate it in acetone and ethanol respectively, then rinse it with deionized water, blow dry it with nitrogen, and treat it with UV for later use; (2) Preparation of a hole transport layer, dissolving a self-assembled monolayer material in an organic solvent, depositing the self-assembled monolayer material on the above-mentioned ITO conductive glass by spin coating, and obtaining the hole transport layer by annealing; (3) Preparation of perovskite absorption layer: obtaining an inorganic salt skeleton on the hole transport layer through a thermal evaporation process, then covering the inorganic salt skeleton with an organic salt, and finally obtaining a perovskite film through annealing treatment; (4) Preparation of electron transport layer: preparing fullerene and its derivatives and hole blocking layer on the perovskite absorption layer to obtain a uniform electron transport layer; (5) Preparation of metal electrodes: depositing metal electrodes on the electron transport layer by thermal evaporation process.
[0028] Furthermore, in the step (2), the self-assembled monolayer material is [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and its concentration is 1.5 mg / mL. The organic solvent is ethanol.
[0029] Furthermore, in the step (2), the spin coating speed is 6000 rpm and the spin coating time is 30 s.
[0030] Furthermore, in the step (2), the annealing temperature is 150°C and the time is 15 min.
[0031] Furthermore, in step (3), the inorganic salt skeleton is PbI 2 The organic salts are MABr and FAI.
[0032] Furthermore, the annealing treatment in step (3) is a two-step annealing, wherein the first annealing temperature is 150°C and the time is 10 min; the second annealing temperature is 100°C and the time is 10 min.
[0033] Furthermore, in step (4), the electron transport layer is prepared by a solution method and has a thickness of 20 nm.
[0034] Furthermore, in the step (5), the metal electrode is Cu, and its thickness is 120 nm. Example 3
[0035] A method for preparing a perovskite solar cell based on a self-assembled monolayer specifically comprises the following steps: (1) Clean the ITO conductive glass. Wipe the ITO conductive glass with a dust-free cloth moistened with ethanol, then ultrasonicate it in acetone and ethanol respectively, then rinse it with deionized water, blow dry it with nitrogen, and treat it with UV for later use; (2) Preparation of a hole transport layer, dissolving a self-assembled monolayer material in an organic solvent, depositing the self-assembled monolayer material on the above-mentioned ITO conductive glass by spin coating, and obtaining the hole transport layer by annealing; (3) Preparation of perovskite absorption layer: obtaining an inorganic salt skeleton on the hole transport layer through a thermal evaporation process, then covering the inorganic salt skeleton with an organic salt, and finally obtaining a perovskite film through annealing treatment; (4) Preparation of electron transport layer: preparing fullerene and its derivatives and hole blocking layer on the perovskite absorption layer to obtain a uniform electron transport layer; (5) Preparation of metal electrodes: depositing metal electrodes on the electron transport layer by thermal evaporation process.
[0036] Furthermore, in the step (2), the self-assembled monolayer material is [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and its concentration is 2.0 mg / mL. The organic solvent is ethanol.
[0037] Furthermore, in the step (2), the spin coating speed is 6000 rpm and the spin coating time is 30 s.
[0038] Furthermore, in the step (2), the annealing temperature is 150°C and the time is 15 min.
[0039] Furthermore, in step (3), the inorganic salt skeleton is PbI 2 The organic salts are MABr and FAI.
[0040] Furthermore, the annealing treatment in step (3) is a two-step annealing, wherein the first annealing temperature is 150°C and the time is 10 min; the second annealing temperature is 100°C and the time is 10 min.
[0041] Furthermore, in step (4), the electron transport layer is prepared by a solution method and has a thickness of 20 nm.
[0042] Furthermore, in the step (5), the metal electrode is Cu, and its thickness is 120 nm. Example 4
[0043] A method for preparing a perovskite solar cell based on a self-assembled monolayer specifically comprises the following steps: (1) Clean the ITO conductive glass. Wipe the ITO conductive glass with a dust-free cloth moistened with ethanol, then ultrasonicate it in acetone and ethanol respectively, then rinse it with deionized water, blow dry it with nitrogen, and treat it with UV for later use; (2) Preparation of a hole transport layer, dissolving a self-assembled monolayer material in an organic solvent, depositing the self-assembled monolayer material on the above-mentioned ITO conductive glass by spin coating, and obtaining the hole transport layer by annealing; (3) Preparation of perovskite absorption layer: obtaining an inorganic salt skeleton on the hole transport layer through a thermal evaporation process, then covering the inorganic salt skeleton with an organic salt, and finally obtaining a perovskite film through annealing treatment; (4) Preparation of electron transport layer: preparing fullerene and its derivatives and hole blocking layer on the perovskite absorption layer to obtain a uniform electron transport layer; (5) Preparation of metal electrodes: depositing metal electrodes on the electron transport layer by thermal evaporation process.
[0044] Furthermore, in the step (2), the self-assembled monolayer material is [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), and its concentration is 2.5 mg / mL. The organic solvent is ethanol.
[0045] Furthermore, in the step (2), the spin coating speed is 6000 rpm and the spin coating time is 30 s.
[0046] Furthermore, in the step (2), the annealing temperature is 150°C and the time is 15 min.
[0047] Furthermore, in step (3), the inorganic salt skeleton is PbI 2 The organic salts are MABr and FAI.
[0048] Furthermore, the annealing treatment in step (3) is a two-step annealing, wherein the first annealing temperature is 150°C and the time is 10 min; the second annealing temperature is 100°C and the time is 10 min.
[0049] Furthermore, in step (4), the electron transport layer is prepared by a solution method and has a thickness of 20 nm.
[0050] Furthermore, in the step (5), the metal electrode is Cu, and its thickness is 120 nm.
[0051] The perovskite solar cell uses the self-assembled monolayer obtained by the preparation method of the present invention as a hole transport layer.
[0052] Comparative Example 1 The preparation method of the perovskite solar cell in Comparative Example 1 is similar to that in Example 1, except for the preparation of the hole transport layer. The preparation method of the hole transport layer is as follows: 20 mg / mL NiO x The aqueous solution was dispersed by ultrasound for 2-5 min and filtered through a 0.22 μm pore size polytetrafluoroethylene water filter membrane. x After the aqueous solution is prepared, annealing treatment is performed to obtain a hole transport layer.
[0053] The perovskite solar cells obtained in Examples 1-4 and Comparative Example 1 were subjected to JV tests, and their JV curves are shown in FIG. Figure 2 As shown. We found that in perovskite solar cells with self-assembled monolayers as hole transport layers, the concentration of the self-assembled monolayer has a great influence on the short-circuit current density of the battery. When the concentration is too high, it is not conducive to the extraction of carriers. When the concentration is 2.0 mg / mL, the obtained battery efficiency is similar to that of NiO x The method simplifies the battery preparation process and reduces the device manufacturing cost.
[0054] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a perovskite solar cell based on a self-assembled monolayer, characterized in that: The specific steps include: (1) Clean the ITO conductive glass. Wipe the ITO conductive glass with a dust-free cloth moistened with ethanol, then ultrasonicate it in acetone and ethanol respectively, then rinse it with deionized water, blow dry it with nitrogen, and treat it with UV for later use; (2) Preparation of a hole transport layer, dissolving a self-assembled monolayer material in an organic solvent, depositing it on the above-mentioned ITO conductive glass by spin coating, and obtaining a hole transport layer by annealing; (3) Preparation of perovskite absorption layer: obtaining an inorganic salt skeleton on the hole transport layer through a thermal evaporation process, then covering the inorganic salt skeleton with an organic salt, and finally obtaining a perovskite film through annealing treatment; (4) Preparation of electron transport layer: preparing fullerene and its derivatives and hole blocking layer on the perovskite absorption layer to obtain a uniform electron transport layer; (5) Preparation of metal electrodes: depositing metal electrodes on the electron transport layer by thermal evaporation process.
2. The preparation method according to claim 1, characterized in that In the step (2), the self-assembled monolayer material is one or more of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), [2-(3,6-dimethyl-9H-carbazole-9-yl)ethyl]phosphonic acid (Me-2PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), [4-(9H-carbazole-9-yl)butyl]phosphonic acid (4PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), and [4-(3,6-dimethoxy-9H-carbazole-9-yl)butyl]phosphonic acid (MeO-4PACz), and the concentration thereof is 0.3-2.5 mg / mL. The organic solvent is ethanol or isopropanol.
3. The preparation method according to claim 1, characterized in that In the step (2), the spin coating speed is 3000-6000 rpm, and the spin coating time is 30-50 s.
4. The preparation method according to claim 1, characterized in that In the step (2), the annealing temperature is 100-150°C and the time is 5-30 min.
5. The preparation method according to claim 1, characterized in that: In the step (3), the inorganic salt skeleton is one of PbI2, PbCl2, and PbBr2. The organic salt is one or more of MACl, MABr, MAI, FACl, FABr, and FAI.
6. The preparation method according to claim 1, characterized in that The annealing treatment in step (3) is a two-step annealing process, wherein the first annealing temperature is 130-170°C and the time is 0-20 min; the second annealing temperature is 80-130°C and the time is 0-20 min.
7. The preparation method according to claim 1, characterized in that The electron transport layer in step (4) is prepared by a solution method or a thermal evaporation method, and its thickness is 5-50 nm.
8. The preparation method according to claim 1, characterized in that In the step (5), the metal electrode is one of Au, Ag and Cu, and its thickness is 60-150 nm.
9. A perovskite solar cell based on a self-assembled monolayer, characterized in that: A battery obtained by the preparation method according to any one of claims 1 to 8.
Citation Information
Cited By
Perovskite interface treating agent, perovskite solar cell and application thereof
CN122520632A
Perovskite thin film manufacturing method and apparatus, and perovskite solar cell module
WO2026170610A1