Polymer composition preparation method and polymer composition

By adding compounds containing tert-butylphenol groups in the preparation process of the polymer composition, the yellowing problem caused by the residue of alkylated dianiline in polybutadiene is solved, and the processing and physical properties of the polymer are improved .

CN119095887APending Publication Date: 2024-12-06LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036855.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-04
Filing Date
2023-02-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The alkylated dianiline compounds and p-styreneized dianiline introduced in the prior art during the preparation of polybutadiene remain in the rubber composition, resulting in yellowing and affecting processing performance.

Method used

By mixing a compound containing a tert-butylphenol group with a branched conjugated diene polymer when preparing the polymer composition, the conjugated diene polymer prepared from a dianiline catalyst is prevented from turning yellow, and Improve its processing performance.

Benefits of technology

The excellent processing properties of the polymer composition are achieved while preventing yellowing, ensuring the physical properties and processability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005104885930000031
    Figure BDA0005104885930000031
  • Figure BDA0005104885930000061
    Figure BDA0005104885930000061
  • Figure BDA0005104885930000161
    Figure BDA0005104885930000161
Patent Text Reader

Abstract

The present invention relates to a method for preparing a polymer composition capable of preventing a yellowing phenomenon of a branched conjugated diene-based polymer having an improved degree of branching, and a polymer composition prepared thereby.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2022-0081775 filed in the Korean Intellectual Property Office on July 4, 2022, the disclosure of which is incorporated herein by reference in its entirety. Technical Field

[0004] The present invention relates to a method for preparing a polymer composition and a polymer composition prepared thereby. Background Art

[0005] Recently, with the increasing attention to energy saving and environmental protection, there is a demand for low fuel consumption of automobiles. As one of the methods for achieving low fuel consumption, a method of increasing the cis bond content of polybutadiene in a rubber composition for forming a tire has been proposed.

[0006] Polybutadiene can be prepared using a Ziegler-Natta catalyst, which can be prepared by activating an organic metal compound such as an organic nickel compound with an alkyl aluminum compound and a fluorine compound, and reacting the prepared catalyst with a 1,3-butadiene monomer to prepare polybutadiene.

[0007] U.S. Patent No. 7081504 (Patent Document 1) and U.S. Patent No. 5451646 (Patent Document 2) disclose a method for preparing polybutadiene having a high cis bond content, wherein, in order to improve processability, when preparing polybutadiene, an alkylated diphenylamine compound and a styrenated diphenylamine compound are introduced to control the molecular weight of the polybutadiene and increase branching.

[0008] However, as shown in Patent Documents 1 and 2, alkylated diphenylamine compounds and para-styrenated diphenylamine compounds introduced when preparing polybutadiene remain in the polybutadiene, and amine compounds such as alkylated diphenylamine compounds and para-styrenated diphenylamine compounds remaining in the polybutadiene cause yellowing of the rubber composition.

[0009] [Prior art literature]

[0010] [Patent Document]

[0011] (Patent Document 1) US 7081504 B2

[0012] (Patent Document 2) US 5451646 A Summary of the invention

[0013] Technical issues

[0014] An object of the present invention is to prevent yellowing of a branched conjugated diene-based polymer having an increased degree of branching.

[0015] That is, in order to solve the problems mentioned in the background of the present invention, the present invention provides a method for preparing a polymer composition, which can prevent the yellowing phenomenon of a conjugated diene polymer prepared by a catalyst containing a diphenylamine compound by mixing a compound containing a tert-butylphenol group with a branched conjugated diene polymer.

[0016] In addition, another object of the present invention is to provide a polymer composition prepared by the above-mentioned method for preparing a polymer composition, thereby having excellent processability by including a branched conjugated diene-based polymer and preventing yellowing.

[0017] Technical Solution

[0018] To this end, the present invention provides a method for preparing a polymer composition and a polymer composition.

[0019] (1) The present invention provides a method for preparing a polymer composition, the method comprising: S10, preparing a branched conjugated diene polymer by polymerizing a conjugated diene monomer in the presence of a catalyst composition comprising an organic metal compound, an organic aluminum compound, a fluorine-based compound and a diphenylamine compound; and S20, mixing the monomer before polymerization in step S10, the polymerization solution during polymerization or the branched conjugated diene polymer after polymerization with a compound containing a tert-butylphenol group.

[0020] (2) In (1) above, the present invention provides a method for preparing a polymer composition, wherein the organic metal compound is an organic nickel compound.

[0021] (3) In the above (1) or (2), the present invention provides a method for preparing a polymer composition, wherein the organic metal compound is selected from one or more of nickel benzoate, nickel acetate, nickel cyclohexaneate, nickel octanoate, nickel neodecanoate, bis(α-furanyldioxime)nickel, nickel palmitate, nickel stearate, nickel acetylacetonate, salicylaldehyde nickel, bis(cyclopentadiene)nickel, bis(salicylicaldehyde)ethylenediimine nickel, cyclopentadienyl-nitrosyl nickel, bis(π-allylnickel), bis(π-cyclooct-1,5-diene)nickel, bis(π-allyltrifluoroacetate) and tetracarbonyl nickel.

[0022] (4) In any one of (1) to (3) above, the present invention provides a method for preparing a polymer composition, wherein the organic aluminum compound is an alkyl aluminum compound represented by the following Formula 1.

[0023] [Formula 1]

[0024] AHr 1 R2R 3

[0025] In the above formula 1, R 1 To R 3 are each independently hydrogen or an alkyl group having 1 to 12 carbon atoms, wherein R 1 To R 3 Not all hydrogen.

[0026] (5) In any one of (1) to (4) above, the present invention provides a method for preparing a polymer composition, wherein the fluorine-based compound is one or more selected from hydrogen fluoride and boron trifluoride.

[0027] (6) In any one of the above (1) to (5), the present invention provides a method for preparing a polymer composition, wherein the diphenylamine compound is a compound represented by the following Formula 2.

[0028] [Formula 2]

[0029]

[0030] In the above formula 2, R 4 and R 5 Each is independently an alkyl group having 2 to 18 carbon atoms which may be substituted with an aryl group having 6 to 30 carbon atoms.

[0031] (7) In any one of (1) to (6) above, the present invention provides a method for preparing a polymer composition, wherein the compound containing a tert-butylphenol group is tert-butylcatechol, butylhydroxytoluene or a mixture thereof.

[0032] (8) In any one of (1) to (7) above, the present invention provides a method for preparing a polymer composition, wherein, in step S20, a compound containing a tert-butylphenol group is mixed in an amount of 0.0001 to 0.005 parts by weight based on 100 parts by weight of a conjugated diene monomer or a branched conjugated diene polymer.

[0033] (9) The present invention provides a polymer composition comprising a metal-catalyzed branched conjugated diene polymer and a compound containing a tert-butylphenol group.

[0034] (10) In the above (9), the present invention provides a polymer composition wherein the content of the compound containing a tert-butylphenol group is 0.0001 to 0.005 parts by weight based on 100 parts by weight of the metal-catalyzed branched conjugated diene polymer.

[0035] Beneficial Effects

[0036] The polymer composition prepared by the method for preparing a polymer composition according to the present invention includes a branched conjugated diene-based polymer, thereby having excellent processing properties and preventing yellowing. DETAILED DESCRIPTION

[0037] Hereinafter, the present invention will be described in more detail to facilitate understanding of the present invention.

[0038] It should be understood that the words or terms used in the specification and claims of the present invention should not be construed as limited to having the meanings defined in commonly used dictionaries. It will be further understood that, based on the principle that the inventor can appropriately define the meanings of words or terms to best illustrate the invention, the words or terms should be understood to have the same meanings as they have in the context of the relevant technology and in the technical concept of the present invention.

[0039] The present invention relates to a method for preparing a polymer composition and a polymer composition prepared therefrom, and includes all the contents described in U.S. Patent No. 7081504 (Patent Document 1) and U.S. Patent No. 5451646 (Patent Document 2) regarding branched conjugated diene polymers. Therefore, even if there are matters not described regarding the preparation of branched conjugated diene polymers in the specification of the present invention, the matters described in U.S. Patent No. 7081504 (Patent Document 1) and U.S. Patent No. 5451646 (Patent Document 2) all correspond to the branched conjugated diene polymers of the present invention, and the matters described in U.S. Patent No. 7081504 (Patent Document 1) and U.S. Patent No. 5451646 (Patent Document 2) can be applied to the preparation of branched conjugated diene polymers of the present invention.

[0040] Hereinafter, in addition to the contents disclosed in U.S. Patent No. 7081504 (Patent Document 1) and U.S. Patent No. 5451646 (Patent Document 2), the technical features of the present invention for solving the problems of U.S. Patent No. 7081504 (Patent Document 1) and U.S. Patent No. 5451646 (Patent Document 2) will be described in detail below.

[0041] Method for preparing polymer composition

[0042] The present invention provides a method for preparing a polymer composition.

[0043] According to one embodiment of the present invention, the method for preparing a polymer composition may include: S10, preparing a branched conjugated diene polymer by polymerizing a conjugated diene monomer in the presence of a catalyst composition comprising an organic metal compound, an organic aluminum compound, a fluorine-based compound and a diphenylamine compound; and S20, mixing the monomer before the polymerization of step S10, the polymerization solution during the polymerization process, or the branched conjugated diene polymer after the polymerization with a compound containing a tert-butylphenol group.

[0044] According to one embodiment of the present invention, step S10 is a step of preparing a branched conjugated diene-based polymer, and may be performed by polymerizing a conjugated diene-based monomer in the presence of a catalyst composition.

[0045] According to one embodiment of the present invention, the catalyst composition may include: an organic metal compound activated with an organic aluminum compound and a fluorine-based compound for polymerizing a conjugated diene monomer; and a diphenylamine compound for inducing branching of a conjugated diene polymer. Here, the branching of a conjugated diene polymer refers to the formation of a side chain by inducing a branch in the main chain formed by the conjugated diene monomer, and the branched conjugated diene polymer is distinguished from a linear conjugated diene polymer and refers to a conjugated diene polymer comprising a side chain.

[0046] According to one embodiment of the present invention, the organometallic compound can be an organonickeric compound. As a specific example, the organometallic compound can be selected from nickel benzoate, nickel acetate, nickel naphthenate, nickel octanoate, nickel neodecanoate, bis(α-furanyldioxime) nickel, nickel palmitate, nickel stearate, nickel acetylacetonate, salicylaldehyde nickel, bis(cyclopentadiene) nickel, bis(salicylicaldehyde)ethylenediimine nickel, cyclopentadienyl-nitrosyl nickel, bis(π-allyl nickel), bis(π-cyclooct-1,5-diene) nickel, bis(π-allyl trifluoroacetic acid nickel) and tetracarbonyl nickel One or more, and as a more specific example, can be nickel octanoate.

[0047] According to one embodiment of the present invention, the organoaluminum compound is used to activate the organometallic compound, and may be an alkylaluminum compound represented by Formula 1 below.

[0048] [Formula 1]

[0049] AHr 1 R 2 R 3

[0050] In the above formula 1, R 1 To R 3 are each independently hydrogen or an alkyl group having 1 to 12 carbon atoms, wherein R 1 To R 3 Not all hydrogen.

[0051] According to one embodiment of the present invention, the organoaluminum compound can be: alkylaluminum, such as trimethylaluminum, triethylaluminum, tri-n-propylaluminum, triisopropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-tert-butylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum, etc.; dialkylaluminum hydride, such as diethylaluminum hydride, di-n-propylaluminum hydride, diisopropylaluminum hydride, di-n-butylaluminum hydride, diisobutylaluminum hydride (DIBAH), di-n-octylaluminum hydride, diphenylaluminum hydride, di-p-tolylaluminum hydride, dibenzylaluminum hydride, phenethylaluminum hydride, phenyl-n-propylaluminum hydride, phenyl-isopropylaluminum hydride , phenyl n-butylaluminum hydride, phenyl isobutylaluminum hydride, phenyl n-octylaluminum hydride, p-tolyl ethylaluminum hydride, p-tolyl n-propylaluminum hydride, p-tolyl isopropylaluminum hydride, p-tolyl n-butylaluminum hydride, p-tolyl isobutylaluminum hydride, p-tolyl n-octylaluminum hydride, benzyl ethylaluminum hydride, benzyl n-propylaluminum hydride, benzyl isopropylaluminum hydride, benzyl n-butylaluminum hydride, benzyl isobutylaluminum hydride, benzyl n-octylaluminum hydride, etc.; hydrocarbon dialuminum hydride, such as ethylaluminum dihydride, n-propylaluminum dihydride, isopropylaluminum dihydride, n-butylaluminum dihydride, isobutylaluminum dihydride, n-octylaluminum dihydride, etc.

[0052] According to one embodiment of the present invention, the fluorine-based compound is used to activate the organometallic compound, and can be one or more selected from hydrogen fluoride and boron trifluoride. If necessary, the fluorine-based compound can be in the form of a complex, and the complex can be formed by an ether compound, an alcohol compound, a ketone compound, an ester compound, a nitrile compound, an amine compound, water, etc. containing atoms or free radicals that can provide electrons to hydrogen fluoride or boron trifluoride or share electrons with it.

[0053] According to one embodiment of the present invention, in the catalyst composition, the molar ratio of the organometallic compound: the organoaluminum compound may be 1:0.3 to 300, the molar ratio of the organometallic compound: the fluorine-based compound may be 1:0.5 to 200, and the molar ratio of the organoaluminum compound: the fluorine-based compound may be 1:0.7 to 7.

[0054] According to one embodiment of the present invention, the diphenylamine-based compound may be a compound represented by Formula 2 below.

[0055] [Formula 2]

[0056]

[0057] In the above formula 2, R 4 and R 5 Each is independently an alkyl group having 2 to 18 carbon atoms which may be substituted with an aryl group having 6 to 30 carbon atoms.

[0058] According to one embodiment of the present invention, R 4 and R 5 may be present in the ortho, meta or para position independently, and may be an alkyl group having 2 or more, 3 or more, or 4 or more carbon atoms which may be substituted or unsubstituted by an aryl group having 6 to 30 carbon atoms, or an alkyl group having 18 or less, 16 or less, 14 or less, or 12 or less carbon atoms which may be substituted or unsubstituted by an aryl group having 6 to 30 carbon atoms. As a specific example, R 4 and R 5 Each of the alkyl groups may be independently present in the para position. In addition, when the alkyl group is substituted with an aryl group having 6 to 30 carbon atoms, the alkyl group may be an alkyl group having 2 carbon atoms, and as a more specific example, the alkyl group having 2 carbon atoms substituted with an aryl group having 6 to 30 carbon atoms may be a styrene derivative. That is, the diphenylamine compound may be a diphenylamine compound alkylated with an alkyl group having 2 to 18 carbon atoms or a para-styrenated diphenylamine compound.

[0059] According to one embodiment of the present invention, the content of the diphenylamine-based compound may be 0.25 parts by weight to 1.5 parts by weight, or 0.5 parts by weight to 0.75 parts by weight, based on 100 parts by weight of the conjugated diene-based monomer.

[0060] According to one embodiment of the present invention, step S10 may be performed by polymerizing the conjugated diene-based monomer in a hydrocarbon solvent in the presence of the catalyst composition.

[0061] According to one embodiment of the present invention, the hydrocarbon solvent may be one or more selected from n-pentane, n-hexane, n-heptane, isooctane, cyclohexane, toluene, benzene and xylene.

[0062] According to one embodiment of the present invention, the conjugated diene monomer may be one or more selected from 1,3-butadiene, isoprene, 1,3-pentadiene, 1,3-hexadiene, 2,3-dimethyl-1,3-butadiene, 2-ethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene and 2,4-hexadiene, and as a specific example, may be 1,3-butadiene.

[0063] According to one embodiment of the present invention, the polymerization in step S10 may be performed using coordinated anion polymerization, and the polymerization environment may be bulk polymerization, solution polymerization, suspension polymerization or emulsion polymerization, and as a specific example, may be solution polymerization.

[0064] According to one embodiment of the present invention, the polymerization of step S10 can be carried out at a temperature above -20°C, above -10°C, above 0°C, above 10°C, above 20°C, above 30°C, above 40°C, above 50°C or above 60°C. In addition, it can be carried out at a temperature below 200°C, below 150°C, below 120°C or below 90°C. Within the above range, the cis-1,4 bond content of the prepared conjugated diene polymer can be ensured while smoothly controlling the polymerization reaction.

[0065] According to one embodiment of the present invention, the polymerization of step S10 can be carried out for 15 minutes or longer, 20 minutes or longer, 30 minutes or longer, 40 minutes or longer, 50 minutes or longer, or 1 hour or longer. In addition, it can be carried out for 3 hours or less, 2 hours and 30 minutes or less, or 2 hours or less.

[0066] According to one embodiment of the present invention, the conjugated diene-based polymer formed by the polymerization in step S10 may be a living polymer including sites activated by the catalyst composition.

[0067] According to one embodiment of the present invention, the method for preparing a polymer composition may include a step S11 of reacting a living polymer with a denaturant. The denaturant may be a known denaturant that can be used to prepare a conjugated diene polymer using a catalyst composition comprising an organic metal compound.

[0068] According to one embodiment of the present invention, step S20 can be carried out by mixing the branched conjugated diene polymers after the monomer, the polymerization solution in the polymerization process or the polymerization of the compound containing tert-butylphenol group with the polymerization of step S10.At this time, there is no particular restriction on the method for mixing the compound containing tert-butylphenol group, the compound containing tert-butylphenol group can be added after premixing with monomer or solvent in step S10, can be added in polymerization process in step S10, can be mixed by directly adding to the solution phase of the branched conjugated diene polymer prepared in step S10, can be mixed when removing solvent in step S10, can be mixed after the branched conjugated diene polymer prepared in step S10 is obtained with rubber phase, or can be mixed by adding in the process of rubber blending after the branched conjugated diene polymer prepared in step S10 is obtained with rubber phase.That is, step S20 does not necessarily have to be carried out after step S10, and can be carried out simultaneously with step S10, or as required, carried out at an appropriate time point after step S10.

[0069] According to one embodiment of the present invention, as the compound containing tert-butylphenol group, any compound having tert-butyl as substituent in phenol group is applicable, and now, tert-butyl group can be present in ortho-position, meta-position or para-position.In addition, except the tert-butyl group in phenol group, the compound containing tert-butylphenol group can also include (maximum four) another substituent, and now, described another substituent can be the alkyl with 1 to 30, 1 to 20 or 1 to 10 carbon atom.As a specific example, the compound containing tert-butylphenol group can be tert-butylcatechol, butylated hydroxytoluene or their mixture.

[0070] According to one embodiment of the present invention, in step S20, based on 100 parts by weight of conjugated diene monomers or branched conjugated diene polymers, the compound containing tert-butylphenol group can be mixed with a content of 0.0001 to 0.005 parts by weight. As a specific example, in step S20, the compound containing tert-butylphenol group can be mixed with more than 0.0001 parts by weight, more than 0.0005 parts by weight, more than 0.001 parts by weight, more than 0.0015 parts by weight, more than 0.002 parts by weight, more than 0.0025 parts by weight, more than 0.003 parts by weight, more than 0.0035 parts by weight, or more than 0.004 parts by weight, in addition, less than 0.005 parts by weight or less than 0.004 parts by weight, and within these ranges, there is a significant effect of preventing yellowing without reducing the physical properties of the polymer composition.

[0071] Polymer composition

[0072] The present invention provides a polymer composition.

[0073] According to one embodiment of the present invention, the polymer composition may include a metal-catalyzed branched conjugated diene-based polymer and a tert-butylphenol group.

[0074] According to one embodiment of the present invention, the polymer composition may include a metal-catalyzed branched conjugated diene polymer. As a specific example, the metal-catalyzed branched conjugated diene polymer is a branched conjugated diene polymer prepared in step S10 of the polymer composition preparation method, and may be a metal-catalyzed branched conjugated diene polymer.

[0075] According to one embodiment of the present invention, the metal-catalyzed branched conjugated diene polymer may include a conjugated diene monomer unit, which refers to a repeating unit formed by polymerization of a conjugated diene monomer.

[0076] According to one embodiment of the present invention, the metal-catalyzed branched conjugated diene polymer may contain 80 wt % or more, 85 wt % or more, 90 wt % or more, 95 wt % or more or 100 wt % of 1,3-butadiene monomer units, and may selectively contain 20 wt % or less, 15 wt % or less, 10 wt % or less or 5 wt % or less of another conjugated diene monomer unit copolymerizable with the 1,3-butadiene monomer, and within these ranges, a reduction in the cis-1,4 bond content in the conjugated diene polymer may be prevented. The 1,3-butadiene monomer can be 1,3-butadiene or a derivative thereof, such as 2,3-dimethyl-1,3-butadiene or 2-ethyl-1,3-butadiene, and another conjugated diene monomer copolymerizable with 1,3-butadiene can be 2-methyl-1,3-pentadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene or 2,4-hexadiene.

[0077] According to one embodiment of the present invention, the metal-catalyzed branched conjugated diene polymer can be a conjugated diene polymer catalyzed by a catalyst composition comprising an organic metal compound. That is, the conjugated diene polymer can be a conjugated diene polymer comprising an organic metal site activated by a catalyst composition comprising an organic nickel compound.

[0078] According to one embodiment of the present invention, the weight average molecular weight (Mw) of the metal-catalyzed branched conjugated diene polymer may be 1.0×10 5 g / mol or more, 2.0×10 5 g / mol or more, 3.0×10 5 g / mol or more, 4.0×10 5 g / mol or more, 5.0×10 5 g / mol or more, 6.0×10 5 g / mol or more, 7.0×10 5 g / mol or more, 8.0×10 5 g / mol or above or 9.0×10 5 g / mol or more, in addition, 1.0×10 6 g / mol or less, 9.0×10 5 g / mol or less, 8.0×10 5 g / mol or less, 7.0×10 5 g / mol or less, 6.0×10 5 g / mol or less, 5.0×10 5 g / mol or less, 4.0×10 5 g / mol or less or 3.0×10 5g / mol or less. In addition, the number average molecular weight (Mn) of the conjugated diene polymer may be 1.0×10 5 g / mol or more, 2.0×10 5 g / mol or more, 3.0×10 5 g / mol or more, 4.0×10 5 g / mol or above or 5.0×10 5 g / mol or more, in addition, 6.0×10 5 g / mol or less, 5.0×10 5 g / mol or less, 4.0×10 5 g / mol or less, 3.0×10 5 g / mol or less, 2.0×10 5 g / mol or less or 1.0×10 5 Within these ranges, when applied to a polymer composition, the tensile properties are excellent, and the processing properties are excellent, thereby improving the processability of the polymer composition, thereby making it easy to knead, so as to have an excellent balance between the mechanical properties and the physical properties of the polymer composition.

[0079] According to one embodiment of the present invention, the molecular weight distribution (Mw / Mn) of the branched conjugated diene polymer of the metal catalysis can be more than 1.0, more than 1.5, more than 2.0, more than 2.1, more than 2.2 or more than 2.3, in addition, less than 4.0, less than 3.5, less than 3.0 or less than 2.5. Molecular weight distribution can be calculated by the ratio (Mw / Mn) of weight average molecular weight (Mw) and number average molecular weight (Mn). At this time, number average molecular weight (Mn) is the general average value of the single polymer molecular weight calculated by measuring the molecular weight of n polymer chains, obtaining the sum of molecular weight, and dividing the sum by n, and weight average molecular weight (Mw) represents the molecular weight distribution of polymer composition. All molecular weight averages can be represented by grams / mole (g / mol). In addition, weight average molecular weight and number average molecular weight can each refer to the molecular weight converted by the polystyrene analyzed by gel permeation chromatography (GPC).

[0080] According to one embodiment of the present invention, when the metal-catalyzed branched conjugated diene polymer satisfies both the weight average molecular weight (Mw) and number average molecular weight conditions as well as the molecular weight distribution, when applied to a polymer composition, it has excellent tensile properties, viscoelastic properties and processing properties relative to the polymer composition, and has the effect of excellent balance of physical properties therebetween.

[0081] According to one embodiment of the present invention, the cis-1,4 bond content of the metal-catalyzed branched conjugated diene polymer can be 95.0 wt% or more, 95.5 wt% or more, 96.0 wt% or more, 96.5 wt% or more, 97.0 wt% or more, or 97.5 wt% or more, and in addition, 100.0 wt% or less, 99.5 wt% or less, or 99.0 wt% or less.

[0082] According to one embodiment of the present invention, the Mooney viscosity (ML1+4, @100°C) of the metal-catalyzed branched conjugated diene polymer can be 30 or more, 35 or more, 40 or more or 45 or more, and 70 or less, 65 or less, 60 or less, 55 or less or 50 or less.

[0083] According to one embodiment of the present invention, the polymer composition may contain more than 0.1 wt%, more than 10 wt% or more than 20 wt%, and in addition, less than 100 wt%, less than 95 wt% or less than 90 wt% of a metal-catalyzed branched conjugated diene polymer, and within these ranges, the wear resistance, crack resistance, etc. of molded products manufactured using the polymer composition, for example, tires, can be fully ensured.

[0084] According to one embodiment of the present invention, the compound containing a tert-butylphenol group may be the same as described above in the method for preparing the polymer composition, and the compound containing a tert-butylphenol group may exist in the form of a derivative of the compound containing a tert-butylphenol group in the polymer composition.

[0085] According to one embodiment of the present invention, based on 100 parts by weight of the metal-catalyzed branched conjugated diene polymer, the content of the compound containing a tert-butylphenol group can be 0.0001 parts by weight or more, 0.0005 parts by weight or more, 0.001 parts by weight or more, 0.0015 parts by weight or more, 0.002 parts by weight or more, 0.0025 parts by weight or more, 0.003 parts by weight or more, 0.0035 parts by weight or more, or 0.004 parts by weight or more, and in addition, 0.005 parts by weight or less or 0.004 parts by weight or less, and within these ranges, there is an effect of significantly preventing yellowing without reducing the physical properties of the polymer composition.

[0086] Rubber composition

[0087] The present invention provides a rubber composition.

[0088] According to one embodiment of the present invention, a rubber composition may include the polymer composition.

[0089] According to one embodiment of the present invention, as required, in addition to the polymer composition, the rubber composition may also include another rubber component. At this time, based on the total weight of the rubber composition, the content of the rubber component may be less than 90 weight %. Specifically, based on 100 parts by weight of the polymer composition, 1 to 900 parts by weight of the rubber component may be included.

[0090] According to one embodiment of the present invention, the rubber component may be a natural rubber or a synthetic rubber, for example, the rubber component may be: natural rubber (NR), including cis-1,4-polyisoprene; modified natural rubber, such as epoxidized natural rubber (ENR), deproteinized natural rubber (DPNR), or hydrogenated natural rubber obtained by modifying or refining conventional natural rubber; or synthetic rubber, such as styrene-butadiene copolymer (SBR), polybutadiene (BR), polyisoprene (IR), butyl rubber (IIR), Ethylene-propylene copolymer, polyisobutylene-co-isoprene, chloroprene rubber, poly(ethylene-co-propylene), poly(styrene-co-butadiene), poly(styrene-co-isoprene), poly(styrene-co-isoprene-co-butadiene), poly(isoprene-co-butadiene), poly(ethylene-co-propylene-co-diene), polysulfide rubber, acrylic rubber, polyurethane rubber, silicone rubber, epichlorohydrin rubber, halogenated butyl rubber, etc., and any one of them or a mixture of two or more of them can be used.

[0091] According to one embodiment of the present invention, based on 100 parts by weight of the polymer composition, the rubber composition may include 20 to 90 parts by weight of filler. The filler may be a silica filler, a carbon black filler, or a combination thereof. As a specific example, the filler may be a carbon black filler.

[0092] According to one embodiment of the present invention, the nitrogen adsorption specific surface area of ​​the carbon black filler (measured according to N2SA, JIS K6217-2:2001) may be 20 m 2 / g to 250m 2 / g, and within this range, the processing performance of the rubber composition can be excellent, and the reinforcing performance of the filler can be sufficiently ensured. In addition, the dibutyl phthalate (DBP) adsorption of the carbon black filler can be 80cc / 100g to 200cc / 100g, and within this range, the processing performance of the rubber composition can be excellent, and the reinforcing performance of the filler can be sufficiently ensured.

[0093] According to one embodiment of the present invention, the silica filler may be wet silica (hydrated silicate), dry silica (anhydrous silicate), calcium silicate, aluminum silicate, colloidal silica, etc. As a specific example, the silica filler may be wet silica which has the most significant effect of improving the fracture performance and wet grip performance. In addition, the nitrogen surface area (N2SA) per gram of the silica filler may be 120 m 2 / g to 180m 2 / g, the adsorption specific surface area of ​​hexadecyltrimethylammonium bromide (CTAB) can be 100m 2 / g to 200m 2 / g, within these ranges, the processability of the rubber composition can be excellent and the reinforcing performance of the filler can be sufficiently ensured.

[0094] According to one embodiment of the present invention, when a silica-based filler is used as a filler, a silane coupling agent can be used together to improve the reinforcing performance and low exothermic performance. The silane coupling agent can be bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethylsilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, 3-triethoxysilylpropyl-N,N- Dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide, 3-triethoxysilylpropylbenzoyl tetrasulfide, 3-triethoxysilylpropylmethacrylate monosulfide, 3-trimethoxysilylpropylmethacrylate monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, dimethoxymethylsilylpropylbenzothiazolyl tetrasulfide, and the like. As a specific example, the silane coupling agent may be bis(3-triethoxysilylpropyl)polysulfide or 3-trimethoxysilylpropylbenzothiazolyl tetrasulfide in consideration of the effect of improving the reinforcing property.

[0095] According to one embodiment of the present invention, the rubber composition may be sulfur cross-linkable, and therefore, may further include a vulcanizing agent. Specifically, the vulcanizing agent may be sulfur powder, and may be included in an amount of 0.1 to 10 parts by weight based on 100 parts by weight of the rubber component, and within this range, the elastic modulus and strength required for the vulcanized rubber composition are ensured, and at the same time, low fuel consumption performance may be ensured.

[0096] According to one embodiment of the present invention, in addition to the above components, the rubber composition may also contain various additives commonly used in the rubber industry, specifically, vulcanization accelerators, processing oils, plasticizers, anti-aging agents, scorch retardants, zinc white, stearic acid, thermosetting resins, thermoplastic resins, etc.

[0097] According to one embodiment of the present invention, there is no particular limitation on the vulcanization accelerator, and specifically, thiazole compounds such as 2-mercaptobenzothiazole (M), dibenzothiazinyl disulfide (DM), N-cyclohexyl-2-benzothiazyl sulfenamide (CZ), etc., or guanidine compounds such as diphenylguanidine (DPG), etc. can be used. The vulcanization accelerator can be included in an amount of 0.1 to 5 parts by weight based on 100 parts by weight of the rubber component.

[0098] According to one embodiment of the present invention, the processing oil acts as a softener in the rubber composition, and specific examples thereof may include paraffins, cycloparaffins or aromatic compounds, and as more specific examples thereof, when considering tensile strength and wear resistance, aromatic processing oils may be used, and when considering hysteresis loss and low temperature performance, cycloparaffinic or paraffinic processing oils may be used. Based on 100 parts by weight of the rubber component, the processing oil may be contained in an amount of 100 parts by weight or less, and within this range, the decrease in tensile strength and low heat release performance (low fuel consumption performance) of the vulcanized rubber may be prevented.

[0099] According to one embodiment of the present invention, the anti-aging agent may be N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, a high temperature condensate of diphenylamine and acetone, etc. The anti-aging agent may be used in an amount of 0.1 to 6 parts by weight based on 100 parts by weight of the rubber component.

[0100] According to one embodiment of the present invention, a rubber composition can be obtained by kneading using a kneading machine such as a Banbury mixer, a roller and an internal mixer according to the above mixing formula. In addition, a rubber composition with low heat release and excellent wear resistance can be obtained by a vulcanization process after molding.

[0101] According to one embodiment of the present invention, the rubber composition can be used to manufacture various components of tires, such as tire treads, tire bottoms, sidewalls, carcass coating rubber, belt coating rubber, bead fillers, wipers and bead coating rubber, and various industrial rubber products such as dustproof rubber, conveyor belts and hoses. As a specific example, the molded product made using the rubber composition can include a tire or a tire tread.

[0102] Hereinafter, embodiments of the present invention will be described in detail so that those skilled in the art can easily implement the present invention. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein.

[0103] Preparation Example

[0104] Preparation Example 1: Preparation of Catalyst Composition

[0105] The catalyst composition was prepared by the same method as Example 10 to Example 22 described in US Pat. No. 7,081,504 (Patent Document 1).

[0106] Example

[0107] Example 1

[0108] 500g of 1,3-butadiene and 4.2kg of n-hexane were added to a 20L autoclave reactor, and the temperature in the reactor was raised to 70°C. The catalyst composition prepared in Example 1 was added to the reactor, and then polymerization was carried out. When the polymerization conversion rate reached 98% or more, a n-hexane solution containing 1.0g of a polymerization inhibitor and a solution in which an antioxidant Irganox 1520 (BASF Co., Ltd.) was dissolved in n-hexane at 30% by weight were added to terminate the reaction, and a solution in which tert-butylcatechol (TBC) was dissolved in n-hexane at 0.5% by weight was added so that the content of tert-butylcatechol (TBC) was 1ppm relative to the content of 1,3-butadiene added to the reactor. The polymer thus obtained was placed in hot water heated with steam and stirred to remove the solvent, and then drum dried to remove the residual solvent and water to prepare a butadiene polymer composition.

[0109] Example 2

[0110] A butadiene polymer composition was prepared in the same manner as in Example 1, except that a solution in which tert-butylcatechol was dissolved in n-hexane at 0.5 wt% was added so that the content of tert-butylcatechol (TBC) was 5 ppm instead of 1 ppm relative to the content of 1,3-butadiene charged to the reactor.

[0111] Example 3

[0112] A butadiene polymer composition was prepared in the same manner as in Example 1, except that a solution in which tert-butylcatechol was dissolved in n-hexane at 0.5 wt% was added so that the content of tert-butylcatechol (TBC) was 15 ppm instead of 1 ppm relative to the content of 1,3-butadiene charged to the reactor.

[0113] Example 4

[0114] A butadiene polymer composition was prepared in the same manner as in Example 1, except that a solution in which tert-butylcatechol was dissolved in n-hexane at 0.5 wt% was added so that the content of tert-butylcatechol (TBC) was 20 ppm instead of 1 ppm relative to the content of 1,3-butadiene charged to the reactor.

[0115] Example 5

[0116] A butadiene polymer composition was prepared in the same manner as in Example 1, except that a solution in which tert-butylcatechol was dissolved in n-hexane at 0.5 wt % was added so that the content of tert-butylcatechol (TBC) was 40 ppm instead of 1 ppm relative to the content of 1,3-butadiene charged to the reactor.

[0117] Example 6

[0118] 500g of 1,3-butadiene and 4.2kg of n-hexane were added to a 20L autoclave reactor, and the temperature in the reactor was raised to 70°C. The catalyst composition prepared in Example 1 was added to the reactor, and then polymerization was carried out. When the polymerization conversion reached 98% or more, a n-hexane solution containing 1.0g of a polymerization inhibitor and a solution in which an antioxidant Irganox 1520 (BASF Co., Ltd.) was dissolved in n-hexane at 30% by weight were added to terminate the reaction, and a solution in which butylated hydroxytoluene (BHT) was dissolved in n-hexane at 10% by weight was added, so that the content of butylated hydroxytoluene (BHT) was 10ppm relative to the content of 1,3-butadiene added to the reactor. The polymer thus obtained was placed in hot water heated with steam and stirred to remove the solvent, and then drum dried to remove the residual solvent and water to prepare a butadiene polymer composition.

[0119] Example 7

[0120] 500g of 1,3-butadiene and 4.2kg of n-hexane were added to a 20L autoclave reactor, and the temperature in the reactor was raised to 70°C. A solution in which tert-butylcatechol (TBC) was dissolved in n-hexane at 0.5% by weight was added to the reactor, so that the content of tert-butylcatechol (TBC) was 10ppm relative to the content of 1,3-butadiene added to the reactor. Subsequently, the catalyst composition prepared in Preparation Example 1 was added, and then polymerization was performed. When the polymerization conversion reached more than 98%, a n-hexane solution containing 1.0g of an inhibitor and a solution in which an antioxidant Irganox 1520 (BASF Co., Ltd.) was dissolved in n-hexane at 30% by weight were added to terminate the reaction. The polymer thus obtained was placed in hot water heated with steam and stirred to remove the solvent, and then drum dried to remove the residual solvent and water to prepare a butadiene polymer composition.

[0121] Example 8

[0122] A butadiene polymer composition was prepared in the same manner as in Example 1, except that a solution in which tert-butylcatechol was dissolved in n-hexane at 0.5 wt% was added in Example 7 so that the content of tert-butylcatechol (TBC) was 20 ppm instead of 10 ppm relative to the content of 1,3-butadiene charged to the reactor.

[0123] Comparative Example 1

[0124] 500 g of 1,3-butadiene and 4.2 kg of n-hexane were added to a 20 L autoclave reactor, and the temperature in the reactor was raised to 70 ° C. The catalyst composition prepared in Preparation Example 1 was added to the reactor, and then polymerization was carried out. When the polymerization conversion rate reached 98% or more, a n-hexane solution containing 1.0 g of a polymerization inhibitor and a solution in which an antioxidant Irganox 1520 (BASF Co., Ltd.) was dissolved in n-hexane at 30% by weight were added to terminate the reaction. The polymer thus obtained was placed in hot water heated with steam and stirred to remove the solvent, and then drum dried to remove the residual solvent and water to prepare a butadiene polymer composition.

[0125] Test Example 1: Evaluation of physical properties of polymer compositions

[0126] For the butadiene polymer compositions prepared in Examples 1 to 6 and Comparative Example 1, Mooney viscosity and cis-1,4 bond content were measured in the following manner and are shown in Table 1 below.

[0127] * Mooney viscosity (ML1+4, @100°C): For each polymer, the Mooney viscosity was measured at 100°C using Monsanto MV2000E using a large rotor at a rotor speed of 2±0.02 rpm. The samples used at this time were left at room temperature (23±3°C) for 30 minutes or more, and 27±3 g of each thereof was collected to fill the inside of the mold cavity, and the pressing plate was operated to measure the Mooney viscosity while applying torque.

[0128] * Cis-1,4-bond content: The cis-1,4-bond content of the conjugated diene part was measured by Fourier transform infrared spectroscopy (FT-IR). Specifically, the FT-IR transmission spectrum of the carbon disulfide solution of the conjugated diene polymer prepared at a concentration of 5 mg / mL was measured using carbon disulfide in the same cell as a blank, and then the FT-IR transmission spectrum was measured using about 1130 cm -1 The maximum peak at (a, baseline) and the peak at about 967 cm representing the trans-1,4 bond -1 The minimum peak (b) at about 911 cm-1 represents the vinyl bond. -1 The minimum peak at (c) and the peak at about 736 cm representing the cis-1,4 bond -1 The minimum peak (d) at the bottom was used to obtain the respective contents.

[0129] [Table 1]

[0130]

[0131] As shown in Table 1 above, compared with Comparative Example 1 in which the tert-butylphenol group-containing compound was not mixed with the butadiene polymer, even if the tert-butylphenol group-containing compound was mixed in the polymer composition during or after the preparation of the polymer in Examples 1 to 8, the cis-1,4 bond content of the butadiene polymer was not affected and the Mooney viscosity was not significantly affected, thereby confirming that the Mooney viscosity was maintained at the same level.

[0132] Test Example 2: Measurement of Y / I (Yellowness Index)

[0133] 20 g of the polymer composition prepared in each of Examples 1 to 8 and Comparative Example 1 was thinly spread by a roll kneader with an interval of 2.0 mm, and then 5 g of the composition was cut into a square, placed in a sample mold, and compressed at a temperature of 140° C. to prepare a sample with a thickness of 5 mm. Thereafter, the Y / I of the prepared sample was measured using a colorimeter (Ultrascan Pro, Hunterlab Co., Ltd.), and is shown in Table 2 below.

[0134] Test Example 3: Measurement of Antioxidant Content

[0135] The polymer compositions prepared in each of Examples 1 to 8 and Comparative Example 1 were completely dissolved in chloroform, and then methanol was added thereto to precipitate the polymer compositions. Afterwards, the filtrate was filtered to prepare a sample. The antioxidant standard sample was injected into an HPLC / UV instrument to prepare a calibration curve, and then the prepared sample was injected, and the antioxidant content in the polymer composition was calculated using the calibration curve, and is shown in Table 2 below.

[0136] [Table 2]

[0137]

[0138] As shown in Table 2 above, even after 6 weeks, the Y / I of the polymer compositions prepared in each of Examples 1 to 8 did not increase sharply compared to the Y / I of the polymer composition prepared in Comparative Example 1, and was maintained at an appropriate level, and it was also confirmed that the antioxidant was also maintained at a high content.

[0139] In addition, as can be confirmed in Examples 2 to 4 in which the compound containing a tert-butylphenol group is mixed after the termination of polymerization, and in Examples 7 and 8 in which the compound containing a tert-butylphenol group is mixed before the initiation of polymerization, it can be confirmed that the yellowing phenomenon can be prevented whenever the compound containing a tert-butylphenol group is added.

[0140] The results show that the polymer composition prepared by the method for preparing a polymer composition according to the present invention includes a branched conjugated diene-based polymer, thereby having excellent processability and preventing yellowing.

Claims

1. A method for preparing a polymer composition, the method comprising: S10, preparing a branched conjugated diene polymer by polymerizing a conjugated diene monomer in the presence of a catalyst composition comprising an organic metal compound, an organic aluminum compound, a fluorine-based compound, and a diphenylamine compound; and S20, mixing the monomer before polymerization in step S10, the polymerization solution during polymerization, or the branched conjugated diene polymer after polymerization with a compound containing a tert-butylphenol group.

2. The method according to claim 1, wherein: The organometallic compound is an organonickel compound.

3. The method according to claim 1, wherein: The organometallic compound is one or more selected from nickel benzoate, nickel acetate, nickel cyclohexaneate, nickel octanoate, nickel neodecanoate, bis(α-furanyldioxime)nickel, nickel palmitate, nickel stearate, nickel acetylacetonate, salicylaldehyde nickel, bis(cyclopentadiene)nickel, bis(salicylicaldehyde)ethylenediimine nickel, cyclopentadienyl-nitrosyl nickel, bis(π-allylnickel), bis(π-cyclooct-1,5-diene)nickel, bis(π-allyltrifluoroacetate)nickel and tetracarbonylnickel.

4. The method according to claim 1, wherein: The organoaluminum compound is an alkylaluminum compound represented by the following formula 1: [Formula 1] AlR 1 R 2 R 3 Among them, in the above formula 1, R 1 To R 3 are each independently hydrogen or an alkyl group having 1 to 12 carbon atoms, wherein R 1 To R 3 It's not all hydrogen.

5. The method according to claim 1, wherein: The fluorine-based compound is one or more selected from hydrogen fluoride and boron trifluoride.

6. The method according to claim 1, wherein: The diphenylamine compound is a compound represented by the following formula 2: [Formula 2] Among them, in the above formula 2, R 4 and R 5 Each is independently an alkyl group having 2 to 18 carbon atoms which may be substituted with an aryl group having 6 to 30 carbon atoms.

7. The method according to claim 1, wherein: The compound containing tert-butylphenol group is tert-butylcatechol, butylhydroxytoluene or a mixture thereof.

8. The method according to claim 1, wherein: In step S20 , the tert-butylphenol group-containing compound is mixed in an amount of 0.0001 to 0.005 parts by weight based on 100 parts by weight of the conjugated diene-based monomer or the branched conjugated diene-based polymer.

9. A polymer composition comprising a metal-catalyzed branched conjugated diene polymer and a compound containing a tert-butylphenol group.

10. The polymer composition according to claim 9, wherein The tert-butylphenol group-containing compound is included in an amount of 0.0001 to 0.005 parts by weight based on 100 parts by weight of the metal-catalyzed branched conjugated diene-based polymer.