Polyurethane aqueous dispersion, adhesive, synthetic artificial leather and coating
By using polyurethane resin particles with specific structures and the ratio of polyisocyanate to polyol in the aqueous polyurethane resin dispersion, the problem of unstable strength under temperature changes is solved, and high storage stability and bonding are achieved Performance polyurethane aqueous dispersion, suitable for adhesives and coatings.
Patent Information
- Application Number
- CN202380036125.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The dispersions of existing polyurethane resins are unstable under temperature changes, and the inclusion of urea bonds during the manufacturing process leads to a decrease in initial viscosity and adhesion, making it difficult to apply to materials exposed to temperature changes such as synthetic artificial leather.
By using polyurethane resin particles with hydroxyl groups at the end and water as dispersion media, combining aliphatic and cycloaliphatic polyisocyanates with specific ratios of polyols, an aqueous polyurethane dispersion is prepared to avoid the formation of urea bonds in the main chain structure, thereby Improve storage stability and adhesive properties.
A cured film and adhesive layer with uneasy strength under temperature changes is realized, providing a polyurethane aqueous dispersion with excellent initial viscosity, adhesion and filler dispersion. It is suitable for adhesives and coatings, improving storage stability and cold resistance.
Smart Images

Figure BDA0005100003430000161 
Figure BDA0005100003430000171 
Figure BDA0005100003430000201
Abstract
Description
Technical Field
[0001] The invention relates to polyurethane aqueous dispersion, adhesive, synthetic leather and coating. Background Art
[0002] Polyurethane resins are resins that are excellent in various physical properties such as wear resistance, bendability, flexibility, softness, processability, adhesion, and chemical resistance, and are also excellent in suitability for various processing methods. Therefore, polyurethane resins that are widely used as materials for synthetic leather (a general term for artificial leather and synthetic leather), binders for various coating agents, inks, and coatings, or as materials for films, sheets, and various molded products, and are suitable for various uses, have been proposed.
[0003] Among them, the aqueous dispersion of the hydrophilic polyurethane resin that can be emulsified and dispersed in water is dried after coating, thereby forming a coating with excellent performance such as mechanical properties, durability, chemical resistance and abrasion resistance. Therefore, such an aqueous dispersion of the hydrophilic polyurethane resin (polyurethane aqueous dispersion) is widely used in coatings, adhesives, fiber processing agents, paper treatment agents and inks. For a long time, in these coatings and other uses, solvent-based liquid compositions obtained by dissolving polyurethane resins in organic solvents have been used. However, in order to cope with environmental problems, etc., in recent years, the composition of the solvent system has been continuously switched to the aqueous dispersion.
[0004] As aqueous dispersions of polyurethane resins, various substances are known depending on the required properties. For example, a dispersion of an aqueous polyurethane resin containing a structure derived from a polyamine containing a hydroxyl group or a monoamine containing a hydroxyl group, and a coating composition using the same, etc. have been proposed (Patent Document 1). In addition, a hydroxyl-functional polyurethane obtained by reacting an NCO-functional prepolymer with an amino alcohol component, and a coating and a coating material using the same have been proposed (Patent Document 2). An aqueous coating composition containing an anionic urethane resin emulsion having an acid value of 20 to 50 mgKOH / g has also been proposed (Patent Document 3).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2020-83902
[0008] Patent Document 2: Japanese Patent Application No. 2011-518899
[0009] Patent Document 3: Japanese Patent Application Publication No. 2005-330339 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] However, the viscosity of the polyurethane resin dispersions proposed in Patent Documents 1 to 3 tends to increase over time, and it is not necessarily said that the storage stability is good. It should be noted that these polyurethane resin dispersions can be used as adhesives by combining with curing agents. However, the difference in physical properties such as strength of the cured film (adhesive layer) formed using such an adhesive is large under normal temperature conditions and low temperature conditions, and it is not necessarily appropriate as a material for constituting articles exposed to temperature changes (such as synthetic leather used in cold regions).
[0012] In addition, from the viewpoint of easy synthesis, the polyurethane resin used in the conventional dispersion is produced by reacting polyisocyanate with polyol at a ratio of [NCO group / OH group]>1, and then reacting with a chain extender such as amine. However, the main chain structure of the polyurethane resin produced in this way contains a urea bond, so when the polyurethane resin is used as an adhesive, the initial viscosity (initial adhesion) is reduced, and when it is used as a coating, the adhesion to a substrate such as PVC is reduced.
[0013] The present invention has been made in view of the problems existing in the prior art, and its subject is to provide an adhesive, coating, etc. that can form a cured film, i.e., an adhesive layer whose physical properties such as strength are not easily changed even when the temperature changes, and a polyurethane aqueous dispersion that is particularly useful as an additive for imparting adhesiveness to the main agent of the adhesive or coating and has excellent storage stability. In addition, the present invention aims to provide an adhesive, synthetic leather, and coating that use the polyurethane aqueous dispersion and have excellent initial tack adhesion and filler dispersibility.
[0014] Solutions for solving problems
[0015] That is, the present invention provides the following polyurethane aqueous dispersion.
[0016] [1] A polyurethane aqueous dispersion comprising: resin particles formed of a polyurethane having a hydroxyl group at its terminal and water as a dispersion medium, wherein the polyurethane comprises: a structural unit derived from a polyol including a polyether polyol; a structural unit derived from a polyisocyanate including an aliphatic polyisocyanate and an alicyclic polyisocyanate; and a structural unit derived from a polyol containing an acidic group, wherein the acid value of the polyurethane is 40 mgKOH / g or less, and the polyurethane is a reactant obtained by reacting the polyisocyanate with the polyol in a ratio of isocyanate groups (NCO groups) in the polyisocyanate to hydroxyl groups (OH groups) in the polyol such that 0.5 ≤ [NCO groups / OH groups (molar ratio)] ≤ 0.95, wherein the polyol further comprises a polycarbonate polyol, and the mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D) = 20:80 to 95:5.
[0017] [2] The polyurethane aqueous dispersion according to [1], wherein the molar ratio of the aliphatic polyisocyanate (A) to the alicyclic polyisocyanate (B) is (A):(B)=10:90 to 90:10.
[0018] [3] The polyurethane aqueous dispersion according to [1] or [2], wherein the mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=25:75 to 90:10.
[0019] [4] The polyurethane aqueous dispersion according to any one of [1] to [3], wherein the polyurethane does not have a urea bond in its main chain skeleton.
[0020] [5] The polyurethane aqueous dispersion according to any one of [1] to [4], wherein the cumulative 50% particle size (D 50 ) is 5~500nm.
[0021] [6] The polyurethane aqueous dispersion according to any one of [1] to [5], which is used as a thickener.
[0022] Furthermore, according to the present invention, there are provided the following adhesives, synthetic leathers, and coating materials.
[0023] [7] An adhesive comprising: an aqueous dispersion containing a polyurethane resin used as a main component of the adhesive; the polyurethane aqueous dispersion according to [6]; and an isocyanate curing agent.
[0024] [8] The adhesive according to [7], wherein the content of the resin particles is 5 to 30 parts by mass based on 100 parts by mass of the polyurethane resin.
[0025] [9] A synthetic artificial leather comprising an adhesive layer formed of the adhesive according to [7] or [8].
[0026]
[10] A coating comprising: an aqueous dispersion containing a polyurethane resin used as a main agent of the coating; and the polyurethane aqueous dispersion described in [6].
[0027] Effects of the Invention
[0028] The present invention provides an adhesive, coating, etc. that can form a cured film, i.e., an adhesive layer, whose physical properties such as strength are not easily changed even when the temperature changes, and is particularly useful as an additive for imparting adhesiveness to a main agent of an adhesive or coating (e.g., a commercially available aqueous dispersion containing polyurethane resin particles described below), and has excellent storage stability. In addition, the present invention provides an adhesive, synthetic leather, and coating that are excellent in initial viscosity, adhesion, and filler dispersibility, etc. using the polyurethane aqueous dispersion. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a schematic diagram for explaining the form of a sample used for evaluation in Examples.
[0030] Figure 2 This is a schematic diagram for explaining the form of a Girard oven used for evaluation in Examples. DETAILED DESCRIPTION
[0031] <Polyurethane aqueous dispersion>
[0032] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. One embodiment of the polyurethane aqueous dispersion of the present invention contains resin particles formed of a polyurethane having a hydroxyl group at its terminal and water as a dispersion medium. The polyurethane has: a structural unit derived from a polyol including a polyether polyol; a structural unit derived from a polyisocyanate including an aliphatic polyisocyanate and an alicyclic polyisocyanate; and a structural unit derived from a polyol containing an acidic group. The acid value of the polyurethane is 40 mgKOH / g or less. In addition, the polyurethane is a reactant obtained by reacting a polyisocyanate with a polyol in a ratio of an isocyanate group (NCO group) in the polyisocyanate to a hydroxyl group (OH group) in the polyol such that 0.5≤[NCO group / OH group (molar ratio)]≤0.95. Hereinafter, the details of the polyurethane aqueous dispersion of the present embodiment will be described.
[0033] (Polyurethane)
[0034] The polyurethane water dispersion of the present embodiment contains resin particles formed of polyurethane (polyurethane resin particles). That is, the polyurethane water dispersion of the present embodiment is an aqueous dispersion in which polyurethane resin particles are dispersed in an aqueous dispersion medium containing water.
[0035] [Polyol]
[0036] Polyurethane has a structural unit derived from a polyol. A polyol is a compound having two or more hydroxyl groups (OH groups) in one molecule. In consideration of environmental load, etc., a polyol derived from biomass may also be used.
[0037] Polyols (except for the "acidic group-containing polyol" described later) include polyether polyols. Polyether polyols are polyols having ether bonds in the molecule. Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene glycol-polytetramethylene ether glycol (block or random), polytetramethylene ether glycol, and polyhexamethylene ether glycol. Among them, polytetramethylene ether glycol (poly(substituted tetramethylene) glycol) is preferred. These polyethers can be used alone or in combination of two or more.
[0038] In addition, the number average molecular weight of the polyether polyol is preferably 500 to 3000, and more preferably 900 to 2100. When the number average molecular weight of the polyether polyol is too small, the flexibility may be slightly insufficient and the cold resistance may be insufficient. On the other hand, when the number average molecular weight of the polyether polyol is too large, the long-term heat resistance may be reduced.
[0039] The polyol may further include other polyols other than the polyether polyol. Other polyols include polycarbonate polyols and polyester polyols. Among them, the use of polycarbonate polyols, that is, the polyol further includes polycarbonate polyols, can form an adhesive layer with improved long-term thermal durability, and is therefore preferred.
[0040] When the polyol contains a polyether polyol and a polycarbonate polyol, the mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is preferably (C): (D) = 20:80 to 95:5, more preferably 25:75 to 90:10, and particularly preferably 35:65 to 80:20. By using the polyether polyol and the polycarbonate polyol in the above mass ratio, a polyurethane aqueous dispersion is obtained that can prepare a coating material that can form a cured film having excellent cold-resistant flexural properties.
[0041] The polycarbonate polyol is preferably a polycarbonate polyol having a structure derived from at least one of a diol represented by the following general formula (1) and a diol represented by the following general formula (2) and a carbonate bond. The polycarbonate polyol may be used alone or in combination of two or more.
[0042] HO-A1-OH (1)
[0043] HO-A2-OH (2)
[0044] In the general formula (1), A1 represents a divalent aliphatic hydrocarbon group having 2 to 12 carbon atoms. The divalent aliphatic hydrocarbon group having 2 to 12 carbon atoms is preferably a tetramethylene group, a pentamethylene group, or a hexamethylene group. In the general formula (2), A2 represents a divalent cyclic aliphatic hydrocarbon group having 6 to 18 carbon atoms. The divalent cyclic aliphatic hydrocarbon group having 6 to 18 carbon atoms is preferably a 1,4-cyclohexanedimethylene group.
[0045] The diol represented by the general formula (1) is preferably ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, undecanediol and dodecanediol, and more preferably 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol and 1,6-hexanediol. These diols may be used alone or in combination of two or more.
[0046] As the diol represented by the general formula (2), 1,3-cyclohexanediol, 1,4-cyclohexanediol and 1,4-cyclohexanedimethanol are preferred, and 1,4-cyclohexanedimethanol is more preferred. These diols may be used alone or in combination of two or more.
[0047] Examples of the polyester polyol include polyethylene adipate diol, polybutylene adipate diol, polyethylene butylene adipate diol, polyhexamethyleneisophthalate adipate diol, polyethylene succinate diol, polybutylene succinate diol, polyethylene sebacate diol, polybutylene sebacate diol, poly-ε-caprolactone diol, poly(3-methyl-1,5-pentanediol adipate) diol, and condensates of 1,6-hexanediol and dimer acid.
[0048] <Polyisocyanate>
[0049] Polyurethane has structural units derived from polyisocyanates. Polyisocyanates are compounds having two or more isocyanate groups (NCO groups) in one molecule. Polyisocyanates include aliphatic polyisocyanates and alicyclic polyisocyanates. That is, polyurethane has both structural units derived from aliphatic polyisocyanates and structural units derived from alicyclic polyisocyanates.
[0050] By using alicyclic polyisocyanates, the cohesive force of the obtained polyurethane can be reduced. Thus, the cohesion between the resin particles (latex particles) becomes difficult to occur, the thickening of the polyurethane aqueous dispersion over time can be suppressed, and the storage stability can be improved. However, if alicyclic polyisocyanates are not used in combination and only alicyclic polyisocyanates are used, the physical property changes of the cured film (adhesive layer) based on temperature become easy to occur and the cold resistance is reduced. In contrast, by using aliphatic polyisocyanates and alicyclic polyisocyanates in combination, the storage stability of the polyurethane aqueous dispersion can be improved, and the physical property changes based on temperature of the cured film (adhesive layer) formed by the adhesive using the polyurethane aqueous dispersion can be difficult to occur.
[0051] Aliphatic polyisocyanates (excluding alicyclic polyisocyanates) are isocyanate compounds having a linear or branched alkyl group. Examples of aliphatic polyisocyanates include ethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), decamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethylhexanoate, bis(2-isocyanatoethyl)fumarate, bis(2-isocyanatoethyl)carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate.
[0052] Alicyclic polyisocyanates are isocyanate compounds having a cyclic alkyl group. Examples of alicyclic polyisocyanates include isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12-MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, 2,5-norbornane diisocyanate, and 2,6-norbornane diisocyanate.
[0053] In the polyol, the molar ratio of the aliphatic polyisocyanate (A) to the alicyclic polyisocyanate (B) is preferably (A): (B) = 10:90 to 90:10, and more preferably 30:70 to 70:30. When the proportion of the aliphatic polyisocyanate in the polyol is excessive, the physical property changes of the formed cured film (adhesive layer) due to temperature become less likely to occur, while the storage stability of the polyurethane aqueous dispersion may be slightly reduced.
[0054] [Polyol containing acidic group]
[0055] Polyurethane has a structural unit derived from a polyol containing an acidic group. A polyol containing an acidic group is a polyol having one or more acidic groups in one molecule. Therefore, polyurethane is a resin having an acidic group in its molecule and an acid value within a specified range. As an acidic group, there are carboxylic acid group, sulfonic acid group, phosphoric acid group, and phenolic hydroxyl group. As a polyol containing an acidic group, in addition to dimethylol alkanoic acids such as 2,2-dimethylol propionic acid and 2,2-dimethylol butyric acid, N,N-bishydroxyethyl glycine, N,N-bishydroxyethyl alanine, 3,4-dihydroxybutanesulfonic acid and 3,6-dihydroxy-2-toluenesulfonic acid can also be listed. Among them, from the viewpoint of easy availability, an alkanoic acid having 4 to 12 carbon atoms containing two methylol groups (dimethylol alkanoic acid) is preferred, and 2,2-dimethylol propionic acid (2,2-bis (hydroxymethyl) propionic acid) is more preferred.
[0056] [Polyurethane]
[0057] Polyurethane is a reactant that can be obtained by reacting raw material compounds including polyisocyanate and polyol according to a conventional method. More specifically, polyurethane is a reactant having a hydroxyl group at its terminal that is obtained by reacting polyisocyanate and polyol so that the ratio of isocyanate group (NCO group) in the polyisocyanate and the hydroxyl group (OH group) in the polyol is 0.5≤[NCO group / OH group (molar ratio)]≤0.95, preferably 0.6≤[NCO group / OH group (molar ratio)]≤0.9, and further preferably 0.7≤[NCO group / OH group (molar ratio)]≤0.85.
[0058] By setting the value of [NCO group / OH group (molar ratio)] within the above range, a hydroxyl group can be introduced at the end of the obtained polyurethane. In addition, by using a polyurethane having a hydroxyl group at its end, the hydrophilicity of the formed resin particles is improved, and the particle size of the resin particles can be reduced, the sedimentation and aggregation of the resin particles are suppressed, and the storage stability of the polyurethane water dispersion can be improved. Furthermore, when a polyurethane having a hydroxyl group at its end is used, the adhesive layer (cured film) cured in combination with a curing agent becomes relatively soft. Therefore, it is possible to prepare a polyurethane water dispersion that can provide an adhesive that can form an adhesive layer with improved initial viscosity, a coating that can form a coating film (cured film) with improved adhesion to a substrate, and a coating with improved dispersibility of various matting agents (fillers, etc.). It should be noted that when the value of [NCO group / OH group (molar ratio)] when making polyisocyanate react with polyol is too large (for example, greater than 1.0), there is no hydroxyl group at the end of the obtained polyurethane, and the storage stability of the polyurethane water dispersion is reduced.
[0059] The polyurethane constituting the resin particles preferably does not substantially have a urea bond (-NH-C(=O)-NH-) in its main chain skeleton. By using resin particles formed from a polyurethane having substantially no urea bond in its main chain skeleton, it is possible to produce a polyurethane aqueous dispersion that can provide an adhesive capable of forming an adhesive layer with further improved initial tack, a coating capable of forming a coating film (cured film) with further improved adhesion to a substrate such as PVC, and the like. In addition, by using a polyurethane aqueous dispersion containing resin particles formed from a polyurethane having substantially no urea bond in its main chain skeleton, it is possible to make the physical property changes of the cured film (adhesive layer) due to temperature less likely to occur.
[0060] The acid value of the polyurethane is 40 mgKOH / g or less, preferably 3 to 37 mgKOH / g, more preferably 5 to 35 mgKOH / g, and particularly preferably 10 to 25 mgKOH / g. It should be noted that the polyurethane has a structural unit derived from a polyol containing an acidic group, so the acid value of the polyurethane is usually greater than 0 mgKOH / g. When the acid value of the polyurethane is too high, the proportion of the hard segment becomes excessive. Therefore, the temperature-based physical property changes of the adhesive layer obtained by curing the polyurethane with a curing agent become easy to occur, and the flexibility and adhesion are reduced. On the other hand, when the acid value of the polyurethane is too low, the storage stability of the polyurethane aqueous dispersion becomes insufficient. It should be noted that the "acid value of the polyurethane" in this specification is a physical property value (calculated value) calculated by the following formula (1).
[0061] Acid value of polyurethane (mgKOH / g)
[0062] ={(W / M)×56110} / Y···(1)
[0063] W: Amount of polyol containing acidic groups used (g)
[0064] M: Molecular weight of the polyol containing the acid group
[0065] Y: Total usage of polyurethane constituent materials (g)
[0066] There are hydroxyl groups at the molecular chain ends of polyurethane. The hydroxyl value of polyurethane is usually 0.5 to 60 mgKOH / g, preferably 2 to 45 mgKOH / g, and more preferably 10 to 35 mgKOH / g. It should be noted that the "hydroxyl value of polyurethane" in this specification is a physical property value (calculated value) calculated by the following formula (2).
[0067] Hydroxyl value of polyurethane (mgKOH / g)
[0068] ={(AB)×56110} / Y···(2)
[0069] A: The amount of hydroxyl groups in the raw materials (mol)
[0070] B: The amount of isocyanate group in the raw material (mol)
[0071] Y: Total usage of polyurethane constituent materials (g)
[0072] In the above formula (2), A is the total amount (mol) of substances derived from hydroxyl groups of the respective raw materials (component 1, component 2, ..., component n) calculated by the following formula (2a).
[0073] A n =(a n / Mn )×F n ···(2a)
[0074] A n : The amount of substance derived from the hydroxyl group of component n (mol)
[0075] a n :Usage amount of ingredient n (g)
[0076] M n : Molecular weight of component n
[0077] F n : Number of functional groups of component n
[0078] In the above formula (2), B is the total amount (mol) of substances derived from isocyanate groups of the raw materials (component 1, component 2, ..., component n) calculated by the following formula (2b).
[0079] B n =(b n / M n )×F n ···(2b)
[0080] B n : The amount of the substance derived from the isocyanate group of component n (mol)
[0081] b n :Usage amount of ingredient n (g)
[0082] M n : Molecular weight of component n
[0083] F n : Number of functional groups of component n
[0084] The cumulative 50% particle size (D 50 ) is preferably 5 to 500 nm, more preferably 10 to 450 nm, and particularly preferably 50 to 350 nm. 50 When the median particle size is less than 5 nm, the viscosity of the aqueous dispersion increases excessively. 50 Resin particles having a (median particle size) larger than 500 nm may tend to settle easily.
[0085] The content of the resin particles in the polyurethane aqueous dispersion is preferably 5 to 70% by mass, more preferably 10 to 60% by mass, based on the entirety of the aqueous dispersion. By adding the polyurethane aqueous dispersion of the present embodiment to a commercially available polyurethane-based aqueous adhesive or polyurethane-based aqueous coating containing polyurethane resin particles, further adhesion can be imparted to an adhesive layer or coating (cured film) formed by these adhesives or the like. Therefore, the polyurethane aqueous dispersion of the present embodiment is useful as a tackifier added to a polyurethane-based aqueous adhesive or coating.
[0086] (Dispersion Medium)
[0087] The polyurethane aqueous dispersion of the present embodiment is an aqueous dispersion of resin particles of polyurethane dispersed in a water-based dispersion medium containing water. As water, ion exchange water, distilled water, pure water, and ultrapure water can be used. Among them, ion exchange water is preferred from the viewpoint of the dispersion stability of the resin particles. The aqueous dispersion medium may further contain an organic solvent in a range that does not reduce the dispersibility and stability of the resin particles. As organic solvents, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, dioxane, dimethyl formamide, dimethyl sulfoxide, N-methyl pyrrolidone, N-ethyl pyrrolidone, β-alkoxy propionamide, dipropylene glycol dimethyl ether, and ethyl acetate can be listed.
[0088] (Method for producing polyurethane aqueous dispersion)
[0089] The polyurethane aqueous dispersion of the present embodiment can be produced by the same method as the conventionally known method for producing an aqueous dispersion of resin particles formed of polyurethane. The method for producing the polyurethane aqueous dispersion comprises, for example, a step (1): reacting a polyol, a polyisocyanate, and a polyol containing an acidic group, and then neutralizing the acidic group with a neutralizing agent to form a polyurethane; and a step (2): dispersing the formed polyurethane resin particles in a dispersion medium containing water.
[0090] The neutralizing agent used to neutralize the acidic group can be appropriately selected according to the type of the acidic group, etc. Examples of the neutralizing agent include organic amines such as trimethylamine, triethylamine, triisopropylamine, and tributylamine; inorganic alkali salts such as sodium hydroxide and potassium hydroxide; ammonia; etc. Among them, organic amines are preferred, and triethylamine is more preferred.
[0091] <Adhesive>
[0092] One embodiment of the adhesive of the present invention contains: an aqueous dispersion of a polyurethane resin used as a main agent of the adhesive, the aforementioned polyurethane aqueous dispersion, and an isocyanate curing agent. The adhesive of this embodiment contains the aforementioned polyurethane aqueous dispersion as a tackifier, so that an adhesive layer as a cured film whose physical properties such as strength are not easily changed even when the temperature changes can be formed, and the initial viscosity is excellent. Therefore, the adhesive of this embodiment is suitable as an adhesive for manufacturing synthetic leather and various laminates.
[0093] There is no particular limitation on the type of aqueous dispersion containing a polyurethane resin used as a main agent of an adhesive, and commercially available aqueous dispersions containing polyurethane resin particles can be used, for example. Specific examples of aqueous dispersions containing polyurethane resins include the following trade names: RESAMINE D-1063 (above, Dainichi Seika Industries); HYDRAN WLA-408, WLA-515AR, WLA-535 (above, manufactured by DIC Corporation); etc.
[0094] As the isocyanate curing agent, a known substance can be used as the isocyanate curing agent. Commercially available products of the isocyanate curing agent include the following trade names: DURANATE WT30-100, DURANATE WB40-100, DURANATE WL70-100, DURANATE WR80-70P (all manufactured by Asahi Kasei Corporation); Aquanate 105, Aquanate 130, Aquanate 140, Aquanate 200, Aquanate 210 (all manufactured by Tosoh Corporation); TAKENATE WD-725, TAKENATE WD-730, TAKENATE WD-726 (all manufactured by Mitsui Chemicals, Inc.); etc.
[0095] The content of the isocyanate curing agent in the adhesive can be appropriately set according to the purpose. Specifically, the content of the isocyanate curing agent in the adhesive is preferably 1 to 50 parts by mass, and more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the total (solid content) of the polyurethane resin used as the main agent and the resin particles (resin particles used in the polyurethane aqueous dispersion of the present embodiment).
[0096] The content of the resin particles in the adhesive (resin particles used in the polyurethane aqueous dispersion of the present embodiment) is preferably 5 to 30 parts by mass, more preferably 7 to 25 parts by mass, and particularly preferably 10 to 20 parts by mass, relative to 100 parts by mass of the polyurethane resin (solid content) used as the main agent.
[0097] The adhesive of the present embodiment may contain appropriate amounts of various additives such as a thermoplastic resin, a tackifying resin, a catalyst, a pigment, an antioxidant, an ultraviolet absorber, a surfactant, a flame retardant, a filler, and a foaming agent as required.
[0098] The adhesive of this embodiment can be applied to the surface of the adherend to facilitate bonding of adherends. Examples of adherends other than the above-mentioned substrate layer for synthetic leather include metal and non-metal (polycarbonate, glass, etc.) substrates.
[0099] <Synthetic leather>
[0100] One embodiment of the synthetic leather of the present invention comprises an adhesive layer formed by the above-mentioned adhesive. The adhesive forming the adhesive layer contains the above-mentioned polyurethane aqueous dispersion, so that even if the temperature changes, the physical properties such as strength are not easily changed. Therefore, the synthetic leather of this embodiment comprising the adhesive layer is not easily changed in physical properties such as strength even if the temperature changes, and has excellent cold resistance.
[0101] The synthetic leather comprises, for example, a skin layer, an adhesive layer provided on the skin layer, and a base layer such as a base fabric provided on the adhesive layer. Examples of the base fabric constituting the base fabric include fabrics formed by twill weave, plain weave, etc., raised fabrics obtained by mechanically raising the cotton texture of the fabric, rayon fabric, nylon fabric, polyester fabric, Kevlar (registered trademark) fabric, non-woven fabrics (polyester, nylon, various latex), various films, sheets, etc. In addition, examples of the skin layer include a skin layer formed by a coating for skin layer formation such as solvent-based polyurethane, water-based polyurethane, TPU, etc.
[0102] Synthetic artificial leather can be manufactured, for example, as follows. First, a coating for forming an epidermis layer is applied to release paper by known methods such as comma coating, knife coating, roller coating, gravure coating, die coating, and spraying. The applied coating is suitably dried to form an epidermis layer, and then the aforementioned adhesive is applied to the formed epidermis layer by known methods such as comma coating, knife coating, and roller coating. After the applied adhesive is crimped to the substrate layer, aging (aging) is performed under specified conditions. Then, by peeling from the release paper, the synthetic artificial leather as the purpose can be obtained. The synthetic artificial leather of the present embodiment is suitable as a material constituting shoes, clothing, bags, furniture, vehicle interior materials (such as dashboards, doors, consoles, seats), etc.
[0103] <Paint>
[0104] One embodiment of the coating of the present invention contains: an aqueous dispersion of a polyurethane resin used as a main agent of the coating, and the aforementioned polyurethane aqueous dispersion. The coating of this embodiment contains the aforementioned polyurethane aqueous dispersion as a tackifier, so after being applied to the coated surface, aging is performed as required, thereby forming a cured film (film) with excellent cold resistance, which is not easy to change even when the temperature changes, and the physical properties such as strength. In addition, the adhesion to the coated surface (the surface of the substrate formed by PVC, etc.) is extremely high. Therefore, the coating of this embodiment is useful as a coating agent for coating various coated substrate surfaces.
[0105] There is no particular limitation on the type of aqueous dispersion containing polyurethane resin used as a main agent, and commercially available aqueous dispersion containing polyurethane resin particles can be used. Specific examples of aqueous dispersion containing polyurethane resin include the following trade names: RESAMIN ED-6065NP (made by Dainichi Seika Industries, Ltd.); HYDRAN WLS-290SG, WLS-210, WLS-213 (made by DIC Corporation); etc.
[0106] The coating of the present embodiment may further contain a curing agent (hereinafter, also referred to as a "crosslinking agent"). As a crosslinking agent, in addition to isocyanate crosslinking agents, carbodiimide crosslinking agents, oxazoline crosslinking agents, and epoxy crosslinking agents may also be used. When the content of the crosslinking agent in the coating is too much, problems such as plasticization or embrittlement of the coating may occur due to unreacted crosslinking agent. Therefore, the content of the crosslinking agent in the coating (converted as solid content) is preferably 40 parts by mass or less, more preferably 0.5 to 35 parts by mass relative to 100 parts by mass of the polyurethane resin.
[0107] The coating may also contain various additives as required. Examples of additives include: matting agents; antioxidants such as hindered phenol, phosphite, and thioether; light stabilizers such as hindered amine; ultraviolet absorbers such as benzophenone and benzotriazole; gas discoloration stabilizers such as hydrazine; metal deactivators; and the like.
[0108] As the matting agent, there can be listed resin particles, silica particles, talc, aluminum hydroxide, calcium sulfate, calcium silicate, calcium carbonate, magnesium carbonate, barium carbonate, aluminum silicate, molecular sieves, kaolin, mica, and mica, etc. By using a coating containing a matting agent, a coating of a matte-tone surface material or the like can be formed.
[0109] Example
[0110] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to the following Examples. It should be noted that "parts" and "%" in Examples and Comparative Examples are based on mass unless otherwise specified.
[0111] <Material preparation>
[0112] Prepare the materials shown below.
[0113] Polyether polyol: poly(oxytetramethylene) glycol, number average molecular weight 1000
[0114] Polycarbonate polyol: polyhexamethylene carbonate diol, trade name "ETERNACOLL UH-100", manufactured by Ube Industries, Ltd., number average molecular weight 1000
[0115] ·HDI: Hexamethylene diisocyanate
[0116] IPDI: Isophorone diisocyanate
[0117] BisMPA: 2,2-bis(hydroxymethyl)propionic acid
[0118] ·TEA: Triethylamine
[0119] MEK: Methyl Ethyl Ketone
[0120] <Reference Example 1A>
[0121] 100 parts of polyether polyol, 6.4 parts of BisMPA, 9.3 parts of HDI and 12.3 parts of IPDI were added to a reaction container equipped with a stirrer, a thermometer, a gas inlet pipe and a reflux condenser. MEK was added in such a way that the solid content became 30%, and after being uniformly dissolved, it was reacted at 60°C. The reaction was carried out until the isocyanate group (NCO group) disappeared, and then it was cooled to room temperature, and 4.8 parts of TEA were added and stirred. After adding an appropriate amount of water for emulsification, vacuum degassing was performed to remove MEK to obtain a polyurethane aqueous dispersion PUD1 (solid content 30%) containing polyurethane resin particles. The acid value of the polyurethane forming the polyurethane resin particles is 20.0 mgKOH / g, and the hydroxyl value is 31.2 mgKOH / g. In addition, the average particle size (D 50 ) is 80nm.
[0122] (Examples 2 to 10, Comparative Examples 1 to 7)
[0123] Except for setting the compounding shown in Tables 1-1 and 1-2, the same method as in the aforementioned Reference Example 1A was used to obtain polyurethane water dispersions PUD2 to 17 (solid content 30%) containing polyurethane resin particles. It should be noted that for Comparative Example 6, no polyol containing an acidic group (BisMPA) was used, so a good water dispersion (emulsion) could not be obtained. Various physical properties are shown in Tables 1-1 and 1-2.
[0124] <Evaluation of polyurethane aqueous dispersion>
[0125] (Storage stability)
[0126] The polyurethane aqueous dispersion was stored at 10° C. for 1 month. The viscosity of the polyurethane aqueous dispersion after storage at 25° C. was measured using a B-type viscometer (rotor #2, 30 rpm), and the storage stability was evaluated according to the following evaluation criteria. The results are shown in Tables 1-1 and 1-2.
[0127] 1 (very good): less than 150 mPa·s.
[0128] 2 (good): greater than 150 mPa·s and less than 300 mPa·s
[0129] 3 (normal): greater than 300 mPa·s and less than 800 mPa·s
[0130] 4 (allowed): greater than 800 mPa·s and less than 1000 mPa·s
[0131] 5 (unqualified): greater than 1000mPa·s or sedimentation / separation
[0132] Table 1-1
[0133]
[0134] Table 1-2
[0135]
[0136] <Manufacturing of adhesives and production of films>
[0137] A commercially available polyurethane aqueous dispersion (trade name "RESAMINE D-1063", manufactured by Dainichi Seika Industries, 45% solid content) was used as the matrix PUD. The prepared matrix PUD, the manufactured polyurethane aqueous dispersion, and the isocyanate curing agent (trade name "DURANATE WT30-100", manufactured by Asahi Kasei Corporation) were mixed in the amounts shown in Tables 2-1 to 2-3, and then degassed to obtain an adhesive. The obtained adhesive was applied on release paper, dried at 70°C for 3 minutes and at 100°C for 1 minute. Furthermore, it was aged at 50°C for 24 hours to cure, and then the release paper was removed to obtain a film with a thickness of 30 μm.
[0138] <Evaluation of adhesive>
[0139] (Rate of change of physical properties)
[0140] The produced film was cut into a test piece with a width of 15 mm and a length of 60 mm. The strength (100% M) of the test piece was measured at a tensile speed of 200 mm / min using a tensile testing machine (trade name "Autograph AGS-500NS", manufactured by Shimadzu Corporation). The temperature conditions were set to 25°C, -10°C, and -30°C. Next, the property change rate A and property change rate B were calculated using the following calculation formula and the property change rate was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3.
[0141] ·Property change rate A(%)
[0142] ={(100%M at -10°C) / (100%M at 25°C)}×100
[0143] ·Property change rate B (%)
[0144] ={(100%M at -30°C) / (100%M at 25°C)}×100
[0145] [Evaluation criteria of physical property change rate A]
[0146] 1 (very good): less than 155%
[0147] 2 (good): greater than 155% and less than 165%
[0148] 3 (usually): greater than 165% and less than 180%
[0149] 4 (Allowed): Greater than 180% and less than 200%
[0150] 5 (failed): greater than 200%
[0151] [Evaluation criteria of property change rate B]
[0152] 1 (very good): less than 170%
[0153] 2 (good): more than 170% and less than 200%
[0154] 3 (normal): greater than 200% and less than 230%
[0155] 4 (Allowed): greater than 230% and less than 250%
[0156] 5 (Unqualified): Greater than 250%
[0157] (Long-term heat resistance)
[0158] The film was cut into a test piece with a width of 10 cm and a length of 10 cm. After the test piece was kept at 120°C for 400 hours, the strength (100% M) was measured at a tensile speed of 200 mm / min using a tensile testing machine (trade name "Autograph AGS-500NS", manufactured by Shimadzu Corporation). The temperature condition was set to 25°C. Then, the change rate was calculated using the following calculation formula and the long-term heat resistance was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3.
[0159] Change rate (%) = {(100%M after holding) / (100%M before holding)}×100
[0160] 1 (very good): more than 90%
[0161] 2 (good): 80% or more and less than 90%
[0162] 3 (usually): 70% or more and less than 80%
[0163] 4 (Allowed): 60% or more and less than 70%
[0164] 5 (Unqualified): Less than 60%
[0165] (Adhesion)
[0166] The urethane resin for synthetic leather (trade name "RESAMINE NE-8875-30M", manufactured by Dainichi Seika Industries) was applied on release paper and dried at 120°C to form an epidermis layer with a thickness of 50 μm. After applying the adhesive on the formed epidermis layer, it was dried at 70°C for 3 minutes and at 100°C for 1 minute to form an adhesive layer with a thickness of 100 μm. A base fabric of polyester mesh material was attached to the surface of the formed adhesive layer. After aging for 24 hours at 50°C, the release paper was peeled off to obtain the synthetic leather for the test. The obtained synthetic leather was cut into 2 cm width as a test piece. Then, a T-peel test of the epidermis layer / base fabric was performed at 25°C and a tensile speed of 200 mm / min using a tensile testing machine (trade name "Autograph AGS-500NS", manufactured by Shimadzu Corporation), and the adhesion was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3.
[0167] 1 (very good): 1.0kgf / cm or more or the material is broken
[0168] 2 (good): 0.7kgf / cm or more and less than 1.0kgf / cm
[0169] 3 (normal): 0.5kgf / cm or more and less than 0.7kgf / cm
[0170] 4 (allowed): 0.2kgf / cm3 or more and less than 0.5kgf / cm3
[0171] 5 (unqualified): less than 0.2kgf / cm
[0172] (Initial viscosity)
[0173] The urethane resin for synthetic leather (trade name "RESAMINE NE-8875-30M", manufactured by Dainichi Seika Industries) was coated on release paper and dried at 120°C to form an epidermis layer with a thickness of 50 μm. After the adhesive was coated on the formed epidermis layer, it was dried at 70°C for 3 minutes and at 100°C for 1 minute to form an adhesive layer with a thickness of 100 μm. Using a probe viscosity tester (trade name "TE-6001", manufactured by TESTER SANGYO CO,.LTD), the surface of the formed adhesive layer was contacted with a cylindrical SUS rod (diameter 5 mmφ) with a load of 20g for 1 second, and then the probe viscosity test was performed by pulling it upward at a moving speed of 1 cm / second. The strength (N / 5 mmφ) of the SUS rod when it was pulled upward was measured, and the initial viscosity was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 to 2-3. 1 (very good): 5N / 5mmφ or more 2 (good): 4N / 5mmφ or more and less than 5N / 5mmφ 3 (normal): 3N / 5mmφ or more and less than 4N / 5mmφ 4 (allowable): 2N / 5mmφ or more and less than 3N / 5mmφ 5 (unacceptable): less than 2N / 5mmφ
[0174] Table 2-1: Composition and evaluation of adhesives
[0175]
[0176] Table 2-2: Composition and evaluation of adhesives
[0177]
[0178] Table 2-3: Composition and evaluation of adhesives
[0179]
[0180] <Manufacturing of coating materials and preparation of test pieces>
[0181] Prepare a polyurethane aqueous dispersion (trade name "RESAMINE D-6065NP", manufactured by Dainichi Seika Industries, with a solid content of 30%) as a matrix PUD. For 100 parts of the prepared matrix PUD, add 9 parts of a matting agent (trade name "ACEMATT TS-100", manufactured by Evonik Industries, with a volume average particle size of 9.5 μm) and an appropriate amount of ion exchange water and mix them to obtain an aqueous surface treatment agent (solid content 20%). For 100 parts of the obtained surface treatment agent, mix the manufactured polyurethane aqueous dispersion in the amounts shown in Tables 3-1 to 3-3 to prepare a coating. Use a rod coater to apply the prepared coating to a PVC sheet. Use a dryer to dry at 120°C for 1 minute to obtain a test piece with a coating having a thickness of 10 μm.
[0182] <Evaluation of coatings>
[0183] (PVC adhesion)
[0184] The PVC adhesion of the coating film was evaluated using the test piece according to the cross-cut method in accordance with JIS K 5600. Specifically, the test piece with cuts at intervals of 2 mm was visually observed, and the PVC adhesion of the coating film was evaluated according to the evaluation criteria shown below. The results are shown in Tables 3-1 to 3-3.
[0185] 1 (Very Good): The edges of the cut are completely smooth and all grids are not peeled off.
[0186] 2 (good): Small peeling occurred at the intersection of the cuts.
[0187] 3 (normal): The coating film peeled off at least at the edge and intersection of the cut.
[0188] 4 (Allowed): The coating is partially or completely peeled off along the edge of the cut.
[0189] 5 (Unacceptable): The coating film is completely peeled off, regardless of the incision.
[0190] (Dispersion)
[0191] The appearance of the test piece was visually observed and the touch of the surface was confirmed, and the dispersibility was evaluated according to the following evaluation criteria. The results are shown in Tables 3-1 to 3-3.
[0192] 1 (very good): No white spots due to aggregation of the matting agent are observed in appearance, and no coarse particles are felt to the touch.
[0193] 2 (good): 1 to 5 white spots are found in an area of 5 cm x 5 cm. No coarse particles can be felt by touch.
[0194] 3 (normal): 1 to 5 white spots are found in an area of 5 cm x 5 cm. Slightly coarse particles are felt to the touch.
[0195] 4 (permissible): 5 to 10 white spots are found in an area of 5 cm x 5 cm. Coarse particles are clearly felt by touch.
[0196] 5 (Unqualified): The coating film is white and not transparent.
[0197] (Cold resistance and bending)
[0198] A test piece with a width of 50 mm and a length of 150 mm was cut out from the test piece. A bending test was performed using a DE MATTIA testing machine under the conditions of a bending stroke of 100 mm and -10°C, and cold-resistant bending properties were evaluated according to the following evaluation criteria. The results are shown in Tables 3-1 to 3-3.
[0199] 1 (very good): no whitening or cracking after 30,000 cycles
[0200] 2 (Good): Whitening or cracking occurred at 20,000 or more and less than 30,000 times
[0201] 3 (normal): Whitening or cracking occurs between 10,000 and 20,000 times
[0202] 4 (Allowable): Whitening or cracking occurs at 5,000 or more times but less than 10,000 times
[0203] 5 (Unqualified): Whitening or cracking occurred when the number of cycles was less than 5,000.
[0204] (Resistance to heat discoloration)
[0205] The test piece was aged at 80° C. for 500 hours. The gray scale of the test piece before and after aging was compared, and the heat discoloration resistance was evaluated according to the following evaluation criteria. The results are shown in Tables 3-1 to 3-3.
[0206] 1 (very good): grayscale 5
[0207] 2 (good): Grayscale 4
[0208] 3 (usually): grayscale level 3
[0209] 4 (allowed): Grayscale 2
[0210] 5 (Unqualified): Gray Scale 1
[0211] Table 3-1: Composition and evaluation of coatings
[0212]
[0213] Table 3-2: Composition and evaluation of coatings
[0214]
[0215] Table 3-3: Composition and evaluation of coatings
[0216]
[0217] Industrial Applicability
[0218] The polyurethane aqueous dispersion of the present invention is useful, for example, as a material for forming an adhesive layer of various products such as synthetic leather, and is also useful as various coating agents, paints, etc. that can form a cured film with excellent abrasion resistance and cold-resistant flexural properties, and as a thickener added to these coatings, adhesives, etc.
Claims
1. A polyurethane aqueous dispersion comprising: resin particles formed of polyurethane having hydroxyl groups at their terminals and water as a dispersion medium, The polyurethane has a structural unit derived from a polyol including a polyether polyol, a structural unit derived from a polyisocyanate including an aliphatic polyisocyanate and an alicyclic polyisocyanate, and a structural unit derived from a polyol containing an acidic group. The acid value of the polyurethane is less than 40 mgKOH / g, The polyurethane is a reactant obtained by reacting the polyisocyanate with the polyol so that the ratio of isocyanate groups (NCO groups) in the polyisocyanate to hydroxyl groups (OH groups) in the polyol is 0.5≤[NCO groups / OH groups (molar ratio)]≤0.95, The polyol further comprises a polycarbonate polyol, The mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=20:80-95:
5.
2. The polyurethane aqueous dispersion according to claim 1, wherein The molar ratio of the aliphatic polyisocyanate (A) to the alicyclic polyisocyanate (B) is (A):(B)=10:90 to 90:
10.
3. The polyurethane aqueous dispersion according to claim 1 or 2, wherein The mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=25:75-90:
10.
4. The polyurethane aqueous dispersion according to any one of claims 1 to 3, wherein The polyurethane does not have a urea bond in its main chain skeleton.
5. The polyurethane aqueous dispersion according to any one of claims 1 to 4, wherein The cumulative 50% particle size (D 50 ) is 5~500nm. 6 . The polyurethane aqueous dispersion according to claim 1 , which is used as a tackifier.
7. An adhesive comprising: A water dispersion containing a polyurethane resin used as a main agent of an adhesive; The polyurethane aqueous dispersion according to claim 6; and Isocyanate curing agent.
8. The adhesive according to claim 7, wherein The content of the resin particles is 5 to 30 parts by mass based on 100 parts by mass of the polyurethane resin. 9 . A synthetic artificial leather comprising an adhesive layer formed of the adhesive according to claim 7 or 8 .
10. A coating comprising: An aqueous dispersion comprising a polyurethane resin used as a main agent for a coating; and The polyurethane aqueous dispersion according to claim 6.
Citation Information
Patent Citations
Aqueous polyurethane resin dispersion and method for producing the same
CN104031226A
Aqueous polyurethane resin dispersion and method for producing same, paint, film arrangement, and structure
CN112088178A
Blocked polyisocyanate composition, aqueous coating composition and coating film
JP2020143231A
Polyurethane resin aqueous dispersion
WO2021172485A1