Polyurethane aqueous dispersion, adhesive, synthetic artificial leather and coating
By preparing a polyurethane aqueous dispersion containing hydroxyl polyurethane resin particles, combining the reaction of polyisocyanate and polyol, the problem of the change in strength of the polyurethane resin aqueous dispersion when the temperature changes is changed, and a stable cured film and high storage stability are achieved. Suitable for synthetic leather and coatings.
Patent Information
- Application Number
- CN202380036126.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-04-07
AI Technical Summary
The existing polyurethane resin aqueous dispersions are prone to change in strength and physical properties when temperature changes, and the storage stability is insufficient, making it difficult to meet the needs of synthesis of materials such as artificial leather.
By preparing a polyurethane aqueous dispersion containing hydroxy polyurethane resin particles, reacting with polyols using a urethane prepolymer, combining aliphatic and alicyclic polyisocyanates, controlling the acid value and isocyanate content of the polyurethane to form a stable resin Granules, bonding agent and coatings to prepare adhesives and coatings.
It realizes a cured film that does not easily change even when the temperature changes, improves storage stability and cold resistance, and is suitable for synthetic leather and coatings and other materials.
Smart Images

Figure BDA0005100003980000151 
Figure BDA0005100003980000161 
Figure BDA0005100003980000171
Abstract
Description
Technical Field
[0001] The invention relates to polyurethane aqueous dispersion, adhesive, synthetic leather and coating. Background Art
[0002] Polyurethane resins are resins that are excellent in various physical properties such as wear resistance, bendability, flexibility, softness, processability, adhesion, and chemical resistance, and are also excellent in suitability for various processing methods. Therefore, polyurethane resins that are widely used as materials for synthetic leather (a general term for artificial leather and synthetic leather), binders for various coating agents, inks, and coatings, or as materials for films, sheets, and various molded products, and are suitable for various uses, have been proposed.
[0003] Among them, the aqueous dispersion of the hydrophilic polyurethane resin that can be emulsified and dispersed in water is dried after coating, thereby forming a coating with excellent performance such as mechanical properties, durability, chemical resistance and abrasion resistance. Therefore, such an aqueous dispersion of the hydrophilic polyurethane resin (polyurethane aqueous dispersion) is widely used in coatings, adhesives, fiber processing agents, paper treatment agents and inks. For a long time, in these coatings and other uses, solvent-based liquid compositions obtained by dissolving polyurethane resins in organic solvents have been used. However, in order to cope with environmental problems, etc., in recent years, the composition of the solvent system has been continuously switched to the aqueous dispersion.
[0004] As aqueous dispersions of polyurethane resins, various substances are known depending on the required properties. For example, a dispersion of an aqueous polyurethane resin containing a structure derived from a polyamine containing a hydroxyl group or a monoamine containing a hydroxyl group, and a coating composition using the same, etc. have been proposed (Patent Document 1). In addition, a hydroxyl-functional polyurethane obtained by reacting an NCO-functional prepolymer with an amino alcohol component, and a coating and a coating material using the same have been proposed (Patent Document 2). An aqueous coating composition containing an anionic urethane resin emulsion having an acid value of 20 to 50 mgKOH / g has also been proposed (Patent Document 3).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2020-83902
[0008] Patent Document 2: Japanese Patent Application No. 2011-518899
[0009] Patent Document 3: Japanese Patent Application Publication No. 2005-330339 Summary of the invention
[0010] Problem that the invention aims to solve
[0011] However, the viscosity of the polyurethane resin dispersions proposed in Patent Documents 1 to 3 tends to increase over time, and it is not necessarily said that the storage stability is good. It should be noted that these polyurethane resin dispersions can be used as adhesives by combining with curing agents. However, the difference in physical properties such as strength of the cured film (adhesive layer) formed using such adhesives is large under normal temperature conditions and low temperature conditions, and it is not necessarily suitable as a material for constituting articles exposed to temperature changes (such as synthetic leather used in cold regions).
[0012] The present invention has been made in view of the problems existing in the prior art, and its subject is to provide an aqueous polyurethane dispersion having excellent storage stability, which can prepare an adhesive, a coating, etc., which can form a cured film, i.e., an adhesive layer, whose physical properties such as strength are not easily changed even when the temperature changes. Another subject of the present invention is to provide an adhesive, a synthetic leather, and a coating using the aqueous polyurethane dispersion.
[0013] Solutions for solving problems
[0014] That is, the present invention provides the following polyurethane aqueous dispersion.
[0015] [1] A polyurethane aqueous dispersion comprising: resin particles formed of a polyurethane having a hydroxyl group at its terminal and water as a dispersion medium, wherein the polyurethane has a structure derived from a urethane prepolymer, wherein the urethane prepolymer has: a structural unit derived from a polyol including a polyether polyol; a structural unit derived from a polyisocyanate including an aliphatic polyisocyanate and an alicyclic polyisocyanate; and a structural unit derived from a polyol containing an acidic group, wherein the acid value of the polyurethane is 30 mgKOH / g or less, and the polyol further comprises a polycarbonate polyol, wherein the mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=20:80 to 95:5.
[0016] [2] The polyurethane aqueous dispersion according to the above [1], wherein the urethane prepolymer is a reactant having an isocyanate group at its terminal, obtained by reacting the polyisocyanate with the polyol in a ratio of [NCO group] in the polyisocyanate to a hydroxyl group (OH group) in the polyol such that [NCO group / OH group (molar ratio)]>1, and the polyurethane is a reactant obtained by reacting the urethane prepolymer with an alkanolamine.
[0017] [3] The polyurethane aqueous dispersion according to [2] above, wherein the polyurethane is a reaction product obtained by reacting 10 mol % or more of the alkanolamine relative to the isocyanate groups in the urethane prepolymer.
[0018] [4] The aqueous polyurethane dispersion according to [2] or [3], wherein the alkanolamine is an alkanolmonoamine.
[0019] [5] The polyurethane aqueous dispersion according to any one of [2] to [4] above, wherein the urethane prepolymer is a reactant obtained by reacting the polyisocyanate and the polyol so that the ratio of isocyanate groups (NCO groups) in the polyisocyanate to hydroxyl groups (OH groups) in the polyol is 1<[NCO groups / OH groups (molar ratio)]≤1.7.
[0020] [6] The polyurethane aqueous dispersion according to any one of [1] to [5] above, wherein the molar ratio of the aliphatic polyisocyanate (A) to the alicyclic polyisocyanate (B) is (A):(B)=10:90 to 90:10.
[0021] [7] The polyurethane aqueous dispersion according to any one of [1] to [6] above, wherein the mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=25:75 to 90:10.
[0022] [8] The polyurethane aqueous dispersion according to any one of [1] to [7], wherein the cumulative 50% particle size (D 50 ) is 5~500nm.
[0023] Furthermore, according to the present invention, there are provided the following adhesives, synthetic leathers, and coating materials.
[0024] [9] An adhesive comprising the polyurethane aqueous dispersion according to any one of [1] to [8] and an isocyanate curing agent.
[0025]
[10] A synthetic artificial leather comprising an adhesive layer formed of the adhesive according to [9] above.
[0026]
[11] A coating material comprising the polyurethane aqueous dispersion according to any one of [1] to [8] above.
[0027] Effects of the Invention
[0028] The present invention provides an adhesive, coating, etc. that can form a cured film, i.e., an adhesive layer, whose physical properties such as strength are not easily changed even when the temperature changes, and has excellent storage stability. In addition, the present invention can provide an adhesive, synthetic leather, and coating using the polyurethane aqueous dispersion. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1This is a schematic diagram for explaining the form of a sample used for evaluation in Examples.
[0030] Figure 2 This is a schematic diagram for explaining the form of a Girard oven used for evaluation in Examples. DETAILED DESCRIPTION
[0031] <Polyurethane aqueous dispersion>
[0032] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments. One embodiment of the polyurethane aqueous dispersion of the present invention contains resin particles formed of a polyurethane having a hydroxyl group at its terminal and water as a dispersion medium. The polyurethane has a structure derived from a urethane prepolymer. The urethane prepolymer has: a structural unit derived from a polyol including a polyether polyol; a structural unit derived from a polyisocyanate including an aliphatic polyisocyanate and an alicyclic polyisocyanate; and a structural unit derived from a polyol containing an acidic group. In addition, the acid value of the polyurethane is 30 mgKOH / g or less. Hereinafter, the details of the polyurethane aqueous dispersion of this embodiment will be described.
[0033] (Polyurethane)
[0034] The polyurethane water dispersion of the present embodiment contains resin particles (polyurethane resin particles) formed of polyurethane having a structure derived from a urethane prepolymer. That is, the polyurethane water dispersion of the present embodiment is an aqueous dispersion in which polyurethane resin particles are dispersed in an aqueous dispersion medium containing water.
[0035] [Polyol]
[0036] The urethane prepolymer has a structural unit derived from a polyol. A polyol is a compound having two or more hydroxyl groups (OH groups) in one molecule. In consideration of environmental load, etc., a polyol derived from biomass may also be used.
[0037] Polyols (except for the "polyols containing an acidic group" described later) include polyether polyols. Polyether polyols are polyols having an ether bond in the molecule. Examples of polyether polyols include polyethylene glycol, polypropylene glycol, polyethylene glycol-polytetramethylene ether glycol (block or random), polytetramethylene ether glycol, and polyhexamethylene ether glycol. Among them, polytetramethylene ether glycol (poly(oxytetramethylene) glycol) is preferred. These polyethers can be used alone or in combination of two or more.
[0038] The number average molecular weight of the polyether polyol is more preferably 500 to 3000, and more preferably 900 to 2100. When the number average molecular weight of the polyether polyol is too small, the flexibility may be slightly insufficient and the cold resistance may be insufficient. On the other hand, when the number average molecular weight of the polyether polyol is too large, the solvent resistance and long-term heat resistance may be reduced.
[0039] The polyol may also include other polyols other than polyether polyol. Other polyols include polycarbonate polyols, polyester polyols, etc. Among them, the use of polycarbonate polyols, that is, the polyol further includes polycarbonate polyols, can form an adhesive layer with improved solvent resistance and long-term thermal durability, and is therefore preferred.
[0040] When the polyol contains a polyether polyol and a polycarbonate polyol, the mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is preferably (C):(D)=20:80 to 95:5, more preferably 25:75 to 90:10, and particularly preferably 35:65 to 80:20. By using the polyether polyol and the polycarbonate polyol in the above mass ratio, a polyurethane aqueous dispersion can be prepared that can prepare a coating material that can form a cured film having excellent abrasion resistance and cold-resistant flexural properties.
[0041] The polycarbonate polyol is preferably a polycarbonate polyol having a structure derived from at least one of a diol represented by the following general formula (1) and a diol represented by the following general formula (2) and a carbonate bond. The polycarbonate polyol may be used alone or in combination of two or more.
[0042] HO-A1-OH (1)
[0043] HO-A2-OH (2)
[0044] In the general formula (1), A1 represents a divalent aliphatic hydrocarbon group having 2 to 12 carbon atoms. The divalent aliphatic hydrocarbon group having 2 to 12 carbon atoms is preferably a tetramethylene group, a pentamethylene group, or a hexamethylene group. In the general formula (2), A2 represents a divalent cyclic aliphatic hydrocarbon group having 6 to 18 carbon atoms. The divalent cyclic aliphatic hydrocarbon group having 6 to 18 carbon atoms is preferably a 1,4-cyclohexanedimethylene group.
[0045] The diol represented by the general formula (1) is preferably ethylene glycol, propylene glycol, butanediol, pentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, undecanediol and dodecanediol, and more preferably 2-methyl-1,3-propanediol, 1,4-butanediol, 1,5-pentanediol and 1,6-hexanediol. These diols may be used alone or in combination of two or more.
[0046] As the diol represented by the general formula (2), 1,3-cyclohexanediol, 1,4-cyclohexanediol and 1,4-cyclohexanedimethanol are preferred, and 1,4-cyclohexanedimethanol is more preferred. These diols may be used alone or in combination of two or more.
[0047] Examples of the polyester polyol include polyethylene adipate diol, polybutylene adipate diol, polyethylene butylene adipate diol, polyhexamethyleneisophthalate adipate diol, polyethylene succinate diol, polybutylene succinate diol, polyethylene sebacate diol, polybutylene sebacate diol, poly-ε-caprolactone diol, poly(3-methyl-1,5-pentanediol adipate) diol, and condensates of 1,6-hexanediol and dimer acid.
[0048] <Polyisocyanate>
[0049] The urethane prepolymer has a structural unit derived from a polyisocyanate. Polyisocyanate is a compound having two or more isocyanate groups (NCO groups) in one molecule. Polyisocyanates include aliphatic polyisocyanates and alicyclic polyisocyanates. That is, the urethane prepolymer has both a structural unit derived from an aliphatic polyisocyanate and a structural unit derived from an alicyclic polyisocyanate.
[0050] By using alicyclic polyisocyanates, the cohesive force of the obtained polyurethane can be reduced. Thus, the cohesion between the resin particles (latex particles) becomes difficult to occur, the thickening of the polyurethane aqueous dispersion over time can be suppressed, and the storage stability can be improved. However, if alicyclic polyisocyanates are not used in combination and only alicyclic polyisocyanates are used, the physical property changes of the cured film (adhesive layer) based on temperature become easy to occur and the cold resistance is reduced. In contrast, by using aliphatic polyisocyanates and alicyclic polyisocyanates in combination, the storage stability of the polyurethane aqueous dispersion can be improved, and the physical property changes based on temperature of the cured film (adhesive layer) formed by the adhesive using the polyurethane aqueous dispersion can be difficult to occur.
[0051] Aliphatic polyisocyanates (excluding alicyclic polyisocyanates) are isocyanate compounds having a linear or branched alkyl group. Examples of aliphatic polyisocyanates include ethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), decamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, 2,6-diisocyanatomethylhexanoate, bis(2-isocyanatoethyl)fumarate, bis(2-isocyanatoethyl)carbonate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate.
[0052] Alicyclic polyisocyanates are isocyanate compounds having a cyclic alkyl group. Examples of alicyclic polyisocyanates include isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12-MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1,2-dicarboxylate, 2,5-norbornane diisocyanate, and 2,6-norbornane diisocyanate.
[0053] In the polyol, the molar ratio of the aliphatic diisocyanate (A) to the alicyclic diisocyanate (B) is preferably (A):(B) = 10:90 to 90:10, more preferably 30:70 to 70:30. When the proportion of the aliphatic diisocyanate in the polyol is excessive, the physical property changes of the formed cured film (adhesive layer) due to temperature become less likely to occur, while the storage stability of the polyurethane aqueous dispersion may be slightly reduced.
[0054] [Polyol containing acidic group]
[0055] The urethane prepolymer has a structural unit derived from a polyol containing an acidic group. A polyol containing an acidic group is a polyol having one or more acidic groups in one molecule. Therefore, polyurethane is a resin having an acidic group in its molecule and an acid value within a specified range. Examples of the acidic group include a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group. As a polyol containing an acidic group, in addition to dimethylol alkanoic acids such as 2,2-dimethylol propionic acid and 2,2-dimethylol butyric acid, N,N-bishydroxyethyl glycine, N,N-bishydroxyethyl alanine, 3,4-dihydroxybutanesulfonic acid, and 3,6-dihydroxy-2-toluenesulfonic acid can also be listed. Among them, from the viewpoint of easy availability, an alkanoic acid having 4 to 12 carbon atoms containing two methylol groups (dimethylol alkanoic acid) is preferred, and 2,2-dimethylol propionic acid (2,2-bis (hydroxymethyl) propionic acid) is more preferred.
[0056] [Urethane prepolymer]
[0057] Urethane prepolymer is a reactant that can be obtained by reacting raw material compounds including polyisocyanate and polyol according to a conventional method. More specifically, urethane prepolymer is a reactant having an isocyanate group at the terminal, obtained by reacting polyisocyanate with polyol at a ratio of isocyanate group (NCO group) in polyisocyanate and hydroxyl group (OH group) in polyol such that [NCO group / OH group (molar ratio)]>1, preferably 1<[NCO group / OH group (molar ratio)]≤1.7, and more preferably 1.1<[NCO group / OH group (molar ratio)]≤1.5. When the value of [NCO group / OH group (molar ratio)] is too large when polyisocyanate and polyol are reacted, the amount of isocyanate group (terminal isocyanate group (NCO group) content) and urea amount etc. present at the terminal of the obtained urethane prepolymer are excessive. Therefore, the adhesive layer obtained by curing the polyurethane produced using the urethane prepolymer with a curing agent tends to be susceptible to changes in physical properties due to temperature, and the adhesive force tends to be slightly reduced.
[0058] The amount of isocyanate groups present at the terminal of the urethane prepolymer (terminal isocyanate group (NCO group) content) is preferably 1.0 to 10.0% by mass, more preferably 1.5 to 6.0% by mass relative to the resin solid content. When the terminal NCO group content of the urethane prepolymer is too high, the adhesive layer obtained by curing the polyurethane produced using the urethane prepolymer with a curing agent tends to be more susceptible to temperature-dependent changes in physical properties and the adhesive force tends to be slightly reduced.
[0059] [Polyurethane]
[0060] The acid value of the polyurethane is 30 mgKOH / g or less, preferably 3 to 27 mgKOH / g, more preferably 5 to 25 mgKOH / g, and particularly preferably 15 to 25 mgKOH / g. It should be noted that the urethane prepolymer constituting the polyurethane has a structural unit derived from a polyol containing an acidic group, so the acid value of the polyurethane is usually greater than 0 mgKOH / g. When the acid value of the polyurethane is too high, the proportion of the hard segment becomes excessive. Therefore, the temperature-based physical property changes of the adhesive layer obtained by curing the polyurethane with a curing agent become easy to occur and the flexibility and adhesion are reduced. On the other hand, when the acid value of the polyurethane is too low, the storage stability of the polyurethane aqueous dispersion becomes insufficient. It should be noted that the "acid value of the polyurethane" in this specification is a physical property value (calculated value) calculated by the following formula (1).
[0061] Acid value of polyurethane (mgKOH / g)
[0062] ={(W / M)×56110} / Y···(1)
[0063] W: Amount of polyol containing acidic groups used (g)
[0064] M: Molecular weight of the polyol containing the acid group
[0065] Y: Total usage of polyurethane constituent materials (g)
[0066] There are hydroxyl groups at the molecular chain ends of polyurethane. The hydroxyl value of polyurethane is usually 0.5 to 60 mgKOH / g, preferably 2 to 45 mgKOH / g, and more preferably 10 to 35 mgKOH / g. It should be noted that the "hydroxyl value of polyurethane" in this specification is a physical property value (calculated value) calculated by the following formula.
[0067] Hydroxyl value of polyurethane (mgKOH / g)
[0068] ={(A / B)×C×56110} / Y
[0069] A: Amount of alkanolamine used (g)
[0070] B: Molecular weight of alkanolamine
[0071] C: Number of hydroxyl groups in one molecule of alkanolamine
[0072] Y: Total usage of polyurethane constituent materials (g)
[0073] The polyurethane is preferably a product obtained by reacting the urethane prepolymer having an isocyanate group at its terminal with an alkanolamine. The alkanolamine reacts with the terminal isocyanate group of the urethane prepolymer to form a urea bond. Thus, a polyurethane containing a urea bond and having a hydroxyl group at its terminal is formed.
[0074] As the alkanolamine, monoethanolamine, mono-n-butylethanolamine, N-methylethanolamine, N-ethylaminoethanol, N-tert-butylethanolamine, adrenaline, 2-(4-aminophenyl)ethyl alcohol, trishydroxymethylaminomethane, 2-amino-2-methyl-1-propanol, 1-amino-2-propanol, 3-amino-1,2-propanediol, 2-amino-1-butanol, 1-amino-2-butanol, 5-amino-1-pentanol and the like alkanoldiamines such as N-(β-aminoethyl)ethanolamine, 3,5-diaminobenzyl alcohol, 1,3-diamino-2-propanol, 2,2'-(ethylenebisimino)bisethanol and the like can be used. Among them, alkanolmonoamines are preferred, and monoethanolamine is more preferred from the viewpoint of easy availability. By using alkanol monoamine, a polyurethane aqueous dispersion having a better balance between storage stability and cold resistance of the formed adhesive layer (properties such as strength that are not easily changed even when the temperature changes) can be obtained. In contrast, when alkanol diamine is used, the storage stability of the obtained polyurethane aqueous dispersion tends to be slightly reduced.
[0075] Polyurethane is a reactant obtained by reacting alkanolamine in an amount of preferably 1 to 100 mol%, more preferably 5 to 95 mol%, particularly preferably 25 to 70 mol%, and most preferably 40 to 60 mol% relative to the isocyanate group in the urethane prepolymer. By setting the amount of the reacted alkanolamine to the above range, a polyurethane aqueous dispersion of an adhesive having further improved storage stability and capable of preparing an adhesive layer having excellent solvent resistance and heat resistance can be obtained. When the amount of the reacted alkanolamine is too small, there will be a situation where the degree of crosslinking is slightly reduced, the formed network structure becomes insufficient, and the amount of hydroxyl groups introduced into the end of the polyurethane is slightly insufficient. On the other hand, when the amount of the reacted alkanolamine is too much, there will be a situation where unreacted alkanolamine is likely to cause adverse conditions, or the physical properties become easily changed due to temperature changes.
[0076] The cumulative 50% particle size (D 50 ) is preferably 5 to 500 nm, more preferably 10 to 450 nm, and particularly preferably 50 to 350 nm. 50 When the median particle size is less than 5 nm, the viscosity of the aqueous dispersion increases excessively. 50 Resin particles having a (median particle size) larger than 500 nm may tend to settle easily.
[0077] The content of the resin particles in the polyurethane aqueous dispersion is preferably 5 to 70% by mass, more preferably 10 to 60% by mass, based on the entire aqueous dispersion.
[0078] (Dispersion Medium)
[0079] The polyurethane aqueous dispersion of the present embodiment is an aqueous dispersion of resin particles of polyurethane dispersed in a water-based dispersion medium containing water. As water, ion exchange water, distilled water, pure water, and ultrapure water can be used. Among them, ion exchange water is preferred from the viewpoint of the dispersion stability of the resin particles. The aqueous dispersion medium may further contain an organic solvent in a range that does not reduce the dispersibility and stability of the resin particles. As organic solvents, acetone, methyl ethyl ketone, methyl isobutyl ketone, tetrahydrofuran, dioxane, dimethyl formamide, dimethyl sulfoxide, N-methyl pyrrolidone, N-ethyl pyrrolidone, β-alkoxy propionamide, dipropylene glycol dimethyl ether, and ethyl acetate can be listed.
[0080] (Method for producing polyurethane aqueous dispersion)
[0081] The polyurethane aqueous dispersion of the present embodiment can be produced by the same method as the conventionally known method for producing an aqueous dispersion of resin particles formed of polyurethane. Specifically, the target polyurethane aqueous dispersion can be obtained by a prepolymer method in which a urethane prepolymer having an isocyanate group at its terminal is prepared and then reacted with an alkanolamine acting as a chain extender.
[0082] The method for producing a polyurethane aqueous dispersion based on the prepolymer method includes, for example, step (1): reacting a polyol, a polyisocyanate and a polyol containing an acidic group to obtain a urethane prepolymer; step (2): neutralizing the acidic groups in the obtained urethane prepolymer with a neutralizing agent, and then reacting the obtained urethane prepolymer with an alkanolamine to form a polyurethane; and step (3): dispersing resin particles of the formed polyurethane in a dispersion medium containing water.
[0083] The neutralizing agent used to neutralize the acidic groups in the urethane prepolymer may be appropriately selected according to the type of the acidic groups, etc. Examples of the neutralizing agent include organic amines such as trimethylamine, triethylamine, triisopropylamine, and tributylamine; inorganic alkali salts such as sodium hydroxide and potassium hydroxide; ammonia; etc. Among them, organic amines are preferred, and triethylamine is more preferred.
[0084] <Adhesive>
[0085] One embodiment of the adhesive of the present invention comprises the aforementioned polyurethane aqueous dispersion and an isocyanate curing agent. The adhesive of this embodiment contains the aforementioned polyurethane aqueous dispersion, and thus can form an adhesive layer as a cured film whose physical properties such as strength are not easily changed even when the temperature changes. Therefore, the adhesive of this embodiment is suitable as an adhesive for manufacturing synthetic leather and various laminates.
[0086] As the isocyanate curing agent, a known substance can be used as the isocyanate curing agent. Commercially available products of the isocyanate curing agent include the following trade names: DURANATE WT30-100, DURANATE WB40-100, DURANATE WL70-100, DURANATE WR80-70P" (above, manufactured by Asahi Kasei Corporation); Aquanate 105, Aquanate 130, Aquanate 140, Aquanate 200, Aquanate 210 (above, manufactured by Tosoh Corporation); TAKENATE WD-725, TAKENATE WD-730, TAKENATE WD-726 (above, manufactured by Mitsui Chemicals, Inc.); etc.
[0087] The content of the isocyanate curing agent in the adhesive can be appropriately set according to the purpose. Specifically, the content of the isocyanate curing agent in the adhesive is preferably 1 to 50 parts by mass, more preferably 10 to 40 parts by mass, based on 100 parts by mass of the polyurethane (solid content).
[0088] The adhesive of the present embodiment may contain appropriate amounts of various additives such as a thermoplastic resin, a tackifying resin, a catalyst, a pigment, an antioxidant, an ultraviolet absorber, a surfactant, a flame retardant, a filler, and a foaming agent as required.
[0089] The adhesive of this embodiment can be applied to the surface of the adherend to facilitate bonding of adherends. Examples of adherends other than the above-mentioned substrate layer for synthetic leather include metal and non-metal (polycarbonate, glass, etc.) substrates.
[0090] <Synthetic leather>
[0091] One embodiment of the synthetic leather of the present invention comprises an adhesive layer formed by the above-mentioned adhesive. The adhesive forming the adhesive layer contains the above-mentioned polyurethane aqueous dispersion, so that even if the temperature changes, the physical properties such as strength are not easily changed. Therefore, the synthetic leather of this embodiment comprising the adhesive layer is not easily changed in physical properties such as strength even if the temperature changes, and has excellent cold resistance.
[0092] The synthetic leather comprises, for example, a skin layer, an adhesive layer provided on the skin layer, and a base layer such as a base fabric provided on the adhesive layer. Examples of the base fabric constituting the base fabric include fabrics formed by twill weave, plain weave, etc., raised fabrics obtained by mechanically raising the cotton texture of the fabric, rayon fabric, nylon fabric, polyester fabric, Kevlar (registered trademark) fabric, non-woven fabrics (polyester, nylon, various latex), various films, sheets, etc. In addition, examples of the skin layer include a skin layer formed by a coating for skin layer formation such as solvent-based polyurethane, water-based polyurethane, TPU, etc.
[0093] Synthetic artificial leather can be manufactured, for example, as follows. First, the coating for forming the epidermis layer is applied to release paper by known methods such as comma coating, knife coating, roller coating, gravure coating, die coating, and spraying. The applied coating is suitably dried to form the epidermis layer, and then the aforementioned adhesive is applied to the formed epidermis layer by known methods such as comma coating, knife coating, and roller coating. After the applied adhesive is crimped to the substrate layer, it is aged (aged) under specified conditions. Then, it is peeled off by release paper to obtain the synthetic artificial leather as the purpose. The synthetic artificial leather of the present embodiment is suitable as a material constituting shoes, clothes, bags, furniture, vehicle interior materials (such as dashboards, doors, consoles, seats), etc.
[0094] <Paint>
[0095] One embodiment of the coating of the present invention contains: the aforementioned polyurethane aqueous dispersion. The coating of this embodiment contains the aforementioned polyurethane aqueous dispersion, so after being applied to the coated surface, aging is performed as needed, thereby forming a cured film (film) with excellent cold resistance, whose physical properties such as strength are not easily changed even if the temperature changes. Therefore, the coating of this embodiment is useful as a coating agent for coating the surface of various coated substrates.
[0096] The coating preferably further contains a curing agent (hereinafter also referred to as a "crosslinking agent") in order to improve the mechanical properties, durability and other physical properties of the formed cured film (film). As the crosslinking agent, in addition to the isocyanate crosslinking agent, a carbodiimide crosslinking agent, an oxazoline crosslinking agent, and an epoxy crosslinking agent can also be listed.
[0097] When the content of the crosslinking agent in the coating is too high, problems such as plasticization or embrittlement of the coating film may occur due to unreacted crosslinking agent. Therefore, the content of the crosslinking agent in the coating (in terms of solid content) is preferably 40 parts by mass or less, more preferably 0.5 to 35 parts by mass, relative to 100 parts by mass of the polyurethane resin.
[0098] The coating may also contain various additives as required. Examples of additives include: matting agents; antioxidants such as hindered phenol, phosphite, and thioether; light stabilizers such as hindered amine; ultraviolet absorbers such as benzophenone and benzotriazole; gas discoloration stabilizers such as hydrazine; metal deactivators; and the like.
[0099] As the matting agent, there can be listed resin particles, silica particles, talc, aluminum hydroxide, calcium sulfate, calcium silicate, calcium carbonate, magnesium carbonate, barium carbonate, aluminum silicate, molecular sieves, kaolin, mica, and mica, etc. By using a coating containing a matting agent, a coating of a matte-tone surface material or the like can be formed.
[0100] Example
[0101] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to the following Examples. It should be noted that "parts" and "%" in Examples and Comparative Examples are based on mass unless otherwise specified.
[0102] <Material preparation>
[0103] Prepare the materials shown below.
[0104] Polyether polyol (1): poly(oxytetramethylene) glycol, number average molecular weight 2000
[0105] Polyether polyol (2): poly(oxytetramethylene) glycol, number average molecular weight 1000
[0106] Polyether polyol (3): poly(oxytetramethylene) glycol, number average molecular weight 3500
[0107] Polyether polyol (4): poly(oxytetramethylene) glycol, number average molecular weight 250
[0108] Polycarbonate polyol: polyhexamethylene carbonate diol, trade name "ETERNACOLL UH-100", manufactured by Ube Industries, Ltd., number average molecular weight 1000
[0109] ·HDI: Hexamethylene diisocyanate
[0110] IPDI: Isophorone diisocyanate
[0111] BisMPA: 2,2-bis(hydroxymethyl)propionic acid
[0112] ·MEA: Monoethanolamine
[0113] MBM: Mono-n-butylethanolamine
[0114] EA: N-(β-aminoethyl)ethanolamine
[0115] ·TEA: Triethylamine
[0116] MEK: Methyl Ethyl Ketone
[0117] <Production of Polyurethane Aqueous Dispersion>
[0118] (Example 1)
[0119] 150 parts of polyether polyol (2), 150 parts of polycarbonate polyol, 22.1 parts of BisMPA, 28.2 parts of HDI and 86.8 parts of IPDI were added to a reaction vessel equipped with a stirrer, a thermometer, a gas introduction pipe and a reflux cooler. MEK was added in such a way that the solid content was 30%, and after it was uniformly dissolved, it was reacted at 60°C for 7 hours. After confirming that the isocyanate group (NCO group) reached the specified content, the reaction liquid was cooled to room temperature. 16.7 parts of TEA was added and stirred to obtain a liquid containing a carbamate prepolymer. The terminal NCO group content of the carbamate prepolymer in the obtained liquid was 0.54% (1.8% relative to the resin solid content). It should be noted that the terminal NCO group content of the carbamate prepolymer was calculated as follows: after the NCO group at the terminal of the carbamate prepolymer reacted with an excess amount of dibutylamine, the remaining amount of dibutylamine was titrated with hydrochloric acid.
[0120] 5.7 parts of MEA were added to the obtained liquid, and stirred to react. After adding an appropriate amount of water for emulsification, vacuum degassing was performed to remove MEK, and a polyurethane aqueous dispersion containing polyurethane resin particles (solid content 30%) was obtained. The acid value of the polyurethane forming the polyurethane resin particles was 20.0 mgKOH / g, and the hydroxyl value was 11.4 mgKOH / g. In addition, the average particle size (D 50 ) is 200nm.
[0121] (Examples 2, 3, 5 to 18, Reference Example 4, Comparative Examples 1 to 7)
[0122] The polyurethane water dispersion (solid content 30%) containing polyurethane resin particles was obtained in the same manner as in Example 1 except that the mixture was set to the mixture shown in Tables 1-1 to 1-3. It should be noted that for Comparative Example 4, a surfactant (nonionic polyoxyalkylene ether, trade name "Pionin D-1110DIR", manufactured by TAKEMOTO OIL & FAT CO., LTD.) was added in an amount of 10% relative to the resin solid content for emulsification. Various physical properties are shown in Tables 1-1 to 1-3.
[0123] Table 1-1
[0124]
[0125] Table 12
[0126]
[0127] Table 1-3
[0128]
[0129] <Evaluation of polyurethane aqueous dispersion>
[0130] (Storage stability)
[0131] The polyurethane aqueous dispersion was stored at 10° C. for 1 month. The viscosity of the polyurethane aqueous dispersion after storage at 25° C. was measured using a B-type viscometer (rotor #2, 30 rpm), and the storage stability was evaluated according to the following evaluation criteria. The results are shown in Tables 2-1 and 2-2.
[0132] 1 (very good): less than 150 mPa·s.
[0133] 2 (good): greater than 150 mPa·s and less than 300 mPa·s
[0134] 3 (normal): greater than 300 mPa·s and less than 800 mPa·s
[0135] 4 (allowed): greater than 800 mPa·s and less than 1000 mPa·s
[0136] 5 (unqualified): greater than 1000mPa·s or sedimentation / separation
[0137] <Manufacturing of adhesives and production of films>
[0138] After adding 100 parts of an isocyanate curing agent (trade name "DURANATE WT30-100", manufactured by Asahi Kasei Corporation) to 100 parts of the polyurethane aqueous dispersion (i.e., 33.3 parts per 100 parts of the polyurethane resin (solid content)), the adhesive was obtained by mixing and degassing. The obtained adhesive was applied on release paper, dried at 70°C for 3 minutes and at 100°C for 1 minute. Furthermore, it was cured by aging at 50°C for 24 hours to obtain a film with a thickness of 30 μm.
[0139] <Evaluation of adhesive>
[0140] (Rate of change of physical properties)
[0141] The film was cut into a test piece with a width of 15 mm and a length of 60 mm. The strength (100% M) of the test piece was measured at a tensile speed of 200 mm / min using a tensile testing machine (trade name "Autograph AGS-500NS", manufactured by Shimadzu Corporation). The temperature conditions were set to 25°C, -10°C, and -30°C. Next, the property change rate A and property change rate B were calculated using the following calculation formula and the property change rate was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 and 2-2.
[0142] ·Property change rate A(%)
[0143] ={(100%M at -10°C) / (100%M at 25°C)}×100
[0144] ·Property change rate B (%)
[0145] ={(100%M at -30°C) / (100%M at 25°C)}×100
[0146] [Evaluation criteria of physical property change rate A]
[0147] 1 (very good): less than 155%
[0148] 2 (good): greater than 155% and less than 165%
[0149] 3 (usually): greater than 165% and less than 180%
[0150] 4 (Allowed): Greater than 180% and less than 200%
[0151] 5 (failed): greater than 200%
[0152] [Evaluation criteria of property change rate B]
[0153] 1 (very good): less than 170%
[0154] 2 (good): more than 170% and less than 200%
[0155] 3 (normal): greater than 200% and less than 230%
[0156] 4 (Allowed): greater than 230% and less than 250%
[0157] 5 (Unqualified): Greater than 250%
[0158] (Solvent resistance)
[0159] The prepared film was cut into a test piece with a width of 15 mm and a length of 60 mm. The test piece was immersed in acetone for 10 minutes, and the length of the test piece before and after the immersion was measured. Then, the linear swelling rate was calculated using the following formula, and the solvent resistance was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 and 2-2.
[0160] Linear swelling ratio (%) = {(length of the test piece after immersion) / (length of the test piece before immersion)}×100
[0161] 1 (very good): less than 120%
[0162] 2 (good): more than 120% and less than 125%
[0163] 3 (usually): greater than 125% and less than 130%
[0164] 4 (Allowed): Greater than 130% and less than 140%
[0165] 5 (Unqualified): Greater than 140%
[0166] (Long-term heat resistance)
[0167] The film was cut into a test piece with a width of 10 cm and a length of 10 cm. After the test piece was kept at 120°C for 400 hours, the strength (100% M) was measured at a tensile speed of 200 mm / min using a tensile testing machine (trade name "Autograph AGS-500NS", manufactured by Shimadzu Corporation). The temperature condition was set to 25°C. Then, the change rate was calculated using the following calculation formula and the long-term heat resistance was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 and 2-2.
[0168] Change rate (%) = {(100%M after holding) / (100%M before holding)}×100
[0169] 1 (very good): more than 90%
[0170] 2 (good): 80% or more and less than 90%
[0171] 3 (usually): 70% or more and less than 80%
[0172] 4 (Allowed): 60% or more and less than 70%
[0173] 5 (Unqualified): Less than 60%
[0174] (Heat resistance)
[0175] The prepared film was cut into pieces with a width of 15 mm and a length of 60 mm as test pieces. Figure 1 As shown, the film 10 is mounted with a clamp 12 above and below, and the clamp 12 is further fixed with a glass tape. When suspended from a clamp 12, a 450g / cm 2 A weight 14 such as a load of 10000 was placed to prepare a sample 16. It should be noted that the central portion (2 cm) of the film 10 was not covered by the glass ribbon.
[0176] Then, if Figure 2 As shown, the fixture 12 of the sample 16 without the weight 14 was mounted on the rotating disk 22 of the Gill oven 20. Then, the rotating disk 22 was rotated at 5 rpm and the temperature in the Gill oven 20 was raised from room temperature at a rate of 3°C / min. The temperature (softening point (°C)) when the film 10 was cut or when the film 10 was stretched to 2 times was measured, and the heat resistance was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 and 2-2.
[0177] 1 (very good): above 220℃
[0178] 2 (good): 200°C or higher and less than 220°C
[0179] 3 (usually): 180°C or higher and less than 200°C
[0180] 4 (allowed): 160°C or higher and less than 180°C
[0181] 5 (unqualified): less than 160℃
[0182] (Adhesion)
[0183] The urethane resin for synthetic leather (trade name "RESAMINE NE-8875-30M", manufactured by Dainichi Seika Industries) was applied on release paper and dried at 120°C to form an epidermis layer with a thickness of 50 μm. After applying the adhesive on the formed epidermis layer, it was dried at 70°C for 3 minutes and at 100°C for 1 minute to form an adhesive layer with a thickness of 100 μm. A base fabric of polyester mesh material was attached to the surface of the formed adhesive layer. After aging for 24 hours at 50°C, the release paper was peeled off to obtain the synthetic leather for the test. The obtained synthetic leather was cut into 2 cm width as a test piece. Then, a tensile tester (trade name "Autograph AGS-500NS", manufactured by Shimadzu Corporation) was used to perform a T-peel test of the epidermis layer / base fabric at 25°C and a tensile speed of 200 mm / min, and the adhesion was evaluated according to the evaluation criteria shown below. The results are shown in Tables 2-1 and 2-2.
[0184] 1 (very good): 1.0kgf / cm or more or the material is broken
[0185] 2 (good): 0.7kgf / cm or more and less than 1.0kgf / cm
[0186] 3 (normal): 0.5kgf / cm or more and less than 0.7kgf / cm
[0187] 4 (allowed): 0.2kgf / cm3 or more and less than 0.5kgf / cm3
[0188] 5 (unqualified): less than 0.2kgf / cm
[0189] <Manufacturing of paint and preparation of test pieces>
[0190] 1.8 parts of matting agent (trade name "ACEMATT TS-100", manufactured by Evonik Industries, volume average particle size 9.5 μm) and ion exchange water were added to 20 parts of polyurethane aqueous dispersion to obtain an aqueous surface treatment agent (solid content 20%). 2.0 parts of isocyanate curing agent (trade name "DURANATE WT30-100", manufactured by Asahi Kasei Corporation) were added to 100 parts of the obtained surface treatment agent (i.e., 33.3 parts relative to 100 parts of polyurethane resin (solid content)) to prepare a coating. The prepared coating was applied to a PVC sheet using a rod coater. Using a dryer, it was dried at 120°C for 1 minute to obtain a test piece with a film having a thickness of 10 μm.
[0191] <Evaluation of paint>
[0192] (Abrasion resistance)
[0193] A test piece with a width of 70 mm and a length of 300 mm was cut from the test piece. The test piece was placed on the cushioning material of the flat wear table of the flat wear tester for surface cloth materials of JASO M403 / 88 / piece (B method, manufactured by Daiei Kagaku Seiki Manufacturing Co., Ltd.), and fixed with pliers in a way that no cracking occurs. A friction piece with No. 6 cotton canvas of JIS L 3102 (cotton canvas) was brought into contact with the test piece. The following wear test was carried out: the pressing load containing the friction piece was set to 9.81 N (1 kgf), and reciprocated 10,000 times under the conditions of a stroke of 140 mm and a speed of 60±10 reciprocations / minute. The results of evaluating the wear resistance according to the evaluation criteria shown below are shown in Tables 2-1 and 2-2.
[0194] 1 (very good): No change in appearance
[0195] 2 (Good): No scratches, slight changes in appearance
[0196] 3 (usually): no scratches, no noticeable changes in appearance
[0197] 4 (Allowed): One or more but less than five scratches can be confirmed
[0198] 5 (Unacceptable): 5 or more scratches can be confirmed
[0199] (Dispersion)
[0200] The appearance of the test piece was visually observed and the touch of the surface was confirmed, and the dispersibility was evaluated according to the following evaluation criteria. The results are shown in Tables 2-1 and 2-2.
[0201] 1 (very good): No white spots due to aggregation of the matting agent are observed in appearance, and no coarse particles are felt to the touch.
[0202] 2 (good): 1 to 5 white spots are found in an area of 5 cm x 5 cm. No coarse particles can be felt by touch.
[0203] 3 (normal): 1 to 5 white spots are found in an area of 5 cm x 5 cm. Slightly coarse particles are felt to the touch.
[0204] 4 (permissible): 5 to 10 white spots are found in an area of 5 cm x 5 cm. Coarse particles are clearly felt by touch.
[0205] 5 (Unqualified): The coating film is white and not transparent.
[0206] (Cold resistance and bending)
[0207] A test piece with a width of 50 mm and a length of 150 mm was cut out from the test piece. A bending test was performed using a DE MATTIA testing machine under the conditions of a bending stroke of 100 mm and -10°C, and the cold-resistant bending property was evaluated according to the following evaluation criteria. The results are shown in Tables 2-1 and 2-2.
[0208] 1 (very good): no whitening or cracking at 30,000 times
[0209] 2 (Good): Whitening or cracking occurred at 20,000 or more and less than 30,000 times
[0210] 3 (normal): Whitening or cracking occurs between 10,000 and 20,000 times
[0211] 4 (Allowable): Whitening or cracking occurs at 5,000 or more times but less than 10,000 times
[0212] 5 (Unqualified): Whitening or cracking occurred when the number of cycles was less than 5,000.
[0213] Table 2-1
[0214]
[0215] Table 2-2
[0216]
[0217] Industrial Applicability
[0218] The polyurethane aqueous dispersion of the present invention is useful as a material for forming an adhesive layer of various products such as synthetic leather, and is also useful as various coating agents and paints capable of forming a cured film having excellent abrasion resistance and cold-resistant flexural properties.
[0219] Description of Reference Numerals
[0220] 10: Film
[0221] 12: Fixture
[0222] 14: Heavy Objects
[0223] 16: Sample
[0224] 20: Gill oven
[0225] 22: Rotating disk
Claims
1. A polyurethane aqueous dispersion comprising: resin particles formed of polyurethane having hydroxyl groups at their terminals and water as a dispersion medium, The polyurethane has a structure derived from a urethane prepolymer, The urethane prepolymer has a structural unit derived from a polyol including a polyether polyol, a structural unit derived from a polyisocyanate including an aliphatic polyisocyanate and an alicyclic polyisocyanate, and a structural unit derived from a polyol containing an acidic group. The acid value of the polyurethane is less than 30 mgKOH / g, The polyol further comprises a polycarbonate polyol, The mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=20:80-95:
5.
2. The polyurethane aqueous dispersion according to claim 1, wherein The urethane prepolymer is a reactant having an isocyanate group at its terminal, obtained by reacting the polyisocyanate with the polyol so that the isocyanate group (NCO group) in the polyisocyanate and the hydroxyl group (OH group) in the polyol are in a ratio of [NCO group / OH group (molar ratio)]>1. The polyurethane is a reaction product obtained by reacting the urethane prepolymer with an alkanolamine.
3. The polyurethane aqueous dispersion according to claim 2, wherein The polyurethane is a reaction product obtained by reacting 10 mol % or more of the alkanolamine relative to the isocyanate groups in the urethane prepolymer.
4. The polyurethane aqueous dispersion according to claim 2 or 3, wherein The alkanolamine is an alkanolmonoamine.
5. The polyurethane aqueous dispersion according to any one of claims 2 to 4, wherein The urethane prepolymer is a reaction product obtained by reacting the polyisocyanate and the polyol so that the ratio of isocyanate groups (NCO groups) in the polyisocyanate and hydroxyl groups (OH groups) in the polyol is 1<[NCO group / OH group (molar ratio)]≤1.
7.
6. The polyurethane aqueous dispersion according to any one of claims 1 to 5, wherein The molar ratio of the aliphatic polyisocyanate (A) to the alicyclic polyisocyanate (B) is (A):(B)=10:90 to 90:
10.
7. The polyurethane aqueous dispersion according to any one of claims 1 to 6, wherein The mass ratio of the polyether polyol (C) to the polycarbonate polyol (D) is (C):(D)=25:75-90:
10.
8. The polyurethane aqueous dispersion according to any one of claims 1 to 7, wherein The cumulative 50% particle size (D 50 ) is 5~500nm. 9 . An adhesive comprising the polyurethane aqueous dispersion according to claim 1 and an isocyanate curing agent. 10 . A synthetic artificial leather comprising an adhesive layer formed of the adhesive according to claim 9 .
11. A coating material comprising the polyurethane aqueous dispersion according to any one of claims 1 to 8.
Citation Information
Patent Citations
Aqueous polyurethane resin dispersion, process for production thereof, and use thereof
CN102597040A
Polyurethane prepolymer, adhesive and synthetic imitation leather
CN111902443A
Aqueous polyurethane dispersion and coating agent
CN113574129A
Aqueous polyurethane-resin dispersion and uses thereof
WO2016039396A1
Cited By
Method for producing breathing waterproofing aqueous material and waterproofing aqueous resin
TWI919661B