Resin composition and alumina powder used therefor
By using alumina powder with different particle sizes and structures optimized in the resin composition, the heat dissipation characteristics of the alumina powder are improved, and the problem of increasing the content of alumina powder in the resin composition is solved, and the efficient heat dissipation effect is achieved.
Patent Information
- Application Number
- CN202380036631.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-20
- Publication Date
- 2024-12-06
AI Technical Summary
When the content of alumina powder is increased to improve heat dissipation characteristics in the conventional resin composition, it is difficult to maintain the desired shape, and insufficient resin between the alumina particles leads to a decrease in binding force, which affects molding.
Alumina powder containing alumina particles of different particle sizes was used to determine the first alumina particles with a specific surface area of Kr-BET higher than 0.085m2/g and the second alumina particles with a Kr-BET ratio of 0.1 μm to 1.0 μm were used to determine the first alumina particles with a specific surface area of 0.0 μm and the second alumina particles with a 0.1 μm to 1.0 μm were combined with the The third alumina particles optimize the particle size distribution and pore volume distribution to improve the heat dissipation characteristics of the resin composition.
The heat dissipation characteristics of the resin composition are improved without increasing the content of alumina powder, the bonding force between alumina particles and the thermal conductivity of the resin are enhanced, and the thermal conductivity of the composition is improved.
Smart Images

Figure BDA0005102743480000181 
Figure BDA0005102743480000182 
Figure HDA0005102743490000011
Abstract
Description
Technical Field
[0001] The present disclosure relates to a resin composition and an alumina powder used therein. Background Art
[0002] Heat generated by energizing the electronic component is dissipated via the heat sink. In order to improve heat dissipation efficiency, a technique of filling a heat dissipation material between the electronic component and the heat sink is known.
[0003] As one of the heat dissipating members, there is a heat dissipating resin composition containing a resin and an inorganic powder, and it is known that an alumina powder can be used as the inorganic powder (for example, Patent Documents 1 to 3).
[0004] Patent Document 1 discloses an alumina powder having an α-phase content of 40% or less, an average circularity of 0.95 or more, and an average particle size of 100 μm or less as an alumina powder capable of improving fluidity when highly filled in a resin. In the use of semiconductor sealing materials containing alumina powder in epoxy resin, the content of alumina powder is preferably 40% or more by volume, more preferably 65 to 90% by volume, relative to 100% by volume of the resin composition. In addition, in the use of heat dissipation components containing alumina powder in silicone resin or silicone rubber, the content of alumina powder is preferably 65% or more by volume, more preferably 70 to 80% by volume, relative to 100% by volume of the resin composition.
[0005] Patent Document 2 discloses an alumina powder having an average sphericity of 0.93 or more and an α ratio of alumina of 95% or more as an alumina powder capable of improving the viscosity and fluidity of a composition when blended with a resin, etc. In the thermal conductive composition blended with the alumina powder, the alumina powder is preferably blended in an amount of 50 to 95% by mass, particularly preferably 70 to 93% by mass.
[0006] Patent Document 3 discloses a method for obtaining round fused alumina particles having an average particle size of 5 to 4000 μm by crushing fused alumina using a jet mill and removing the edges of the fused alumina particles. In the high thermal conductivity resin containing the round fused alumina particles, the content of the round fused alumina particles is preferably 80% by mass or more. In the embodiment, 200 g (80% by mass) of the round fused alumina particles are blended with respect to 50 g of the silicone resin.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2009 / 133904
[0010] Patent Document 2: International Publication No. 2008 / 053536
[0011] Patent Document 3: Japanese Patent Application Publication No. 2006-169090
[0012] In order to further improve the heat dissipation characteristics of the resin composition, for example, it is conceivable to further increase the content of the alumina powder in the resin composition. However, if the content of the alumina powder is too high, it is difficult to form the resin composition into a desired shape for the following reasons.
[0013] In a general method for manufacturing a resin composition, an aluminum oxide powder and an (uncured) resin are mixed, the obtained mixture is molded into a desired shape, and the resin in the molded body is cured to obtain a resin composition of the desired shape. In order to increase the content of the aluminum oxide powder in the resin composition, it is also necessary to increase the content of the aluminum oxide powder in the mixture as its precursor, and as a result, the content of the resin in the mixture is reduced. In the mixture, a plurality of aluminum oxide particles in the aluminum oxide powder are mutually bonded via the resin, and thus can be molded into a desired shape, but if the content of the resin is reduced, the aluminum oxide particles cannot be fully bonded to each other, and as a result, the mixture cannot sometimes be molded into a desired shape.
[0014] Therefore, it is expected to improve the heat dissipation characteristics by other methods instead of increasing the content of the aluminum oxide powder in the resin composition. Summary of the invention
[0015] Therefore, an object of one embodiment of the present invention is to provide a resin composition capable of improving heat dissipation characteristics without increasing the content of aluminum oxide powder.
[0016] Another embodiment of the present invention aims to provide an alumina powder suitable for producing the resin composition of the above embodiment.
[0017] A first aspect of the present invention is a resin composition comprising a resin and an alumina powder, wherein the alumina powder comprises: a particle size D50 greater than 100 μm and a BET specific surface area measured by a krypton adsorption method greater than 0.085 m 2 / g of first alumina particles and second alumina particles having a particle size D50 of 0.1 μm or more and 1.0 μm or less.
[0018] Aspect 2 of the present invention is the resin composition according to aspect 1, wherein the alumina powder satisfies the following formula (1):
[0019] A>B(1)
[0020] Here, A and B are the contents (mass %) of the first aluminum oxide particles and the second aluminum oxide particles, respectively, when the total amount of the aluminum oxide powder is 100 mass %.
[0021] A third aspect of the present invention is the resin composition according to the first or second aspect, wherein the first alumina particles satisfy the following formula (2):
[0022] L2 / L1×100>100.0(%) (2)
[0023] Here, L1 is the length of the outer edge of the first alumina particle obtained from the SEM-EBSD image, and L2 is the total length of the boundary lines included in the first alumina particle obtained from the SEM-EBSD image.
[0024] A fourth aspect of the present invention is the resin composition according to any one of aspects 1 to 3, wherein the pore volume of the first alumina particles measured by a krypton adsorption method is 0.00005 cm 3 / g or above.
[0025] A fifth aspect of the present invention is the resin composition according to any one of aspects 1 to 4, wherein in the pore volume distribution of the first alumina particles measured by a krypton adsorption method, a peak height existing between pore diameters of 2 to 10 nm is greater than 0.000055 cm 3 / g.
[0026] A sixth aspect of the present invention is the resin composition according to any one of aspects 1 to 5, wherein the alumina powder further includes third alumina particles having a particle size D50 of 3 μm or more and 70 μm or less.
[0027] A seventh aspect of the present invention is an aluminum oxide powder comprising: a particle size D50 greater than 100 μm and a BET specific surface area greater than 0.085 m2 as measured by a krypton adsorption method; 2 / g of first alumina particles and second alumina particles having a particle size D50 of 0.1 μm or more and 1.0 μm or less.
[0028] Aspect 8 of the present invention is the alumina powder according to aspect 7, which satisfies the following formula (1):
[0029] A>B(1)
[0030] Here, A and B are the contents (mass %) of the first aluminum oxide particles and the second aluminum oxide particles, respectively, when the total amount of the aluminum oxide powder is 100 mass %.
[0031] A ninth aspect of the present invention is the alumina powder according to the seventh or eighth aspect, wherein the first alumina particles satisfy the following formula (2):
[0032] L2 / L1×100>100.0(%) (2)
[0033] Here, L1 is the length of the outer edge of the first alumina particle obtained from the SEM-EBSD image, and L2 is the total length of the boundary lines included in the first alumina particle obtained from the SEM-EBSD image.
[0034] A tenth aspect of the present invention is the alumina powder according to any one of aspects 7 to 9, wherein the pore volume of the first alumina particles measured by a krypton adsorption method is 0.00005 cm 3 / g or above.
[0035] Aspect 11 of the present invention is the alumina powder according to any one of aspects 7 to 10, wherein in the pore volume distribution of the first alumina particles measured by a krypton adsorption method, the peak height existing between pore diameters of 2 to 10 nm is greater than 0.000055 cm 3 / g.
[0036] A twelfth aspect of the present invention is the alumina powder according to any one of aspects 7 to 11, further comprising third alumina particles having a particle size D50 of 3 μm or more and 70 μm or less.
[0037] Effects of the Invention
[0038] According to one embodiment of the present invention, a resin composition capable of improving heat dissipation characteristics without increasing the content of aluminum oxide powder can be provided.
[0039] According to another embodiment of the present invention, an alumina powder suitable for producing the resin composition of the above embodiment can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a schematic diagram showing an apparatus for producing alumina particles by a flame fusion method. DETAILED DESCRIPTION
[0041] The present inventors conducted intensive research to solve the problem that the content of alumina powder cannot be increased due to the problem of reduced moldability of a mixture containing alumina powder and (uncured) resin. As a result, they found that by using alumina powder containing two or more alumina particles with different particle sizes (first alumina particles with a large D50 and second alumina particles with a small D50) and making the Kr-BET specific surface area of the first alumina particles higher than a specified value, the heat dissipation characteristics can be improved without increasing the content of alumina powder, thereby completing the present invention.
[0042] Hereinafter, the resin composition according to the embodiment will be described.
[0043] [Resin composition]
[0044] The resin composition of the embodiment includes a resin and an alumina powder. Suitable alumina powder and suitable resin for constituting the resin composition are described in order.
[0045] [Alumina powder]
[0046] The “alumina powder” in this specification refers to both the alumina powder before being mixed with the resin and the alumina powder after being mixed with the resin (for example, the alumina powder in a state of being mixed in a resin composition).
[0047] The alumina powder includes first alumina particles and second alumina particles.
[0048] The particle size D50 of the first alumina particles is greater than 100 μm, and the particle size D50 of the second alumina particles is greater than 0.1 μm and less than 1.0 μm. It should be noted that "particle size D50" refers to the particle size of the cumulative particle size distribution at 50% from the microparticle side. In this specification, particle size D50 is sometimes referred to as "D50".
[0049] The first alumina particles have a BET specific surface area measured by a krypton adsorption method (hereinafter sometimes referred to as “Kr-BET specific surface area”) of greater than 0.085 m 2 The BET specific surface area is an index for understanding the degree of surface irregularities of the alumina particles, and therefore it is known that the first alumina particles have irregularities on the particle surfaces.
[0050] When the alumina powder containing such first alumina particles is used, the thermal conductivity of the mixture containing the alumina powder and the resin becomes good. The reason for this is not clear, but it is presumed to be the following mechanism.
[0051] When there is no resin with low thermal conductivity on the heat dissipation path when heat passes through the inside of the resin composition, or when the existing resin is thin, the thermal conductivity of the resin composition becomes higher (the heat dissipation characteristics are improved). The first alumina particles have concave-convex portions on the particle surface, so the resin is absorbed in the concave portions, and the amount of resin present between the alumina particles is reduced. Therefore, the resin present between adjacent alumina particles becomes thinner, which can improve the heat dissipation characteristics of the resin composition.
[0052] It should be noted that, as the amount of resin between adjacent alumina particles decreases, the bonding force between the alumina particles is generally reduced. However, the resin has been absorbed by the concave portion on the particle surface of the first alumina particle, so the bonding force between the resin and the first alumina particle increases. As a result, even if the amount of resin between adjacent alumina particles decreases, the bonding force between the alumina particles is difficult to decrease.
[0053] For this reason, by using Kr-containing materials having a BET specific surface area of more than 0.085 m 2 / g of the alumina powder of the first alumina particles can improve the heat dissipation characteristics of the resin composition.
[0054] It should be noted that in this embodiment, the Kr-BET specific surface area of the first alumina particles and the second alumina particles contained in the alumina powder, especially the first alumina particles, is specified because the first alumina particles with a large D50 have a large contact area with the resin and therefore have a large impact on the amount of absorbed resin.
[0055] The Kr-BET specific surface area of the first alumina particles is preferably greater than 0.085 m 2 / g, more preferably greater than 0.100m 2 The upper limit of the Kr-BET specific surface area is not particularly limited, and may be, for example, 1.000 m 2 / g or less, and can be further 0.200m 2 / g or less.
[0056] It should be noted that, in the embodiment, when measuring the BET specific surface area of the first alumina particles, krypton gas is used as the adsorption gas instead of nitrogen gas, so that the BET specific surface area of the first alumina particles can be measured more accurately.
[0057] The ratio of the Kr-BET specific surface area of the second alumina particles to the Kr-BET specific surface area of the first alumina particles is preferably greater than 10, more preferably greater than 25, preferably less than 200, and more preferably less than 75. The ratio of the Kr-BET specific surface area of the third alumina particles to the Kr-BET specific surface area of the first alumina particles is preferably greater than 1.0, more preferably greater than 2.5, preferably less than 20, and more preferably less than 7.5.
[0058] As described above, the particle size D50 of the first alumina particles is greater than 100 μm, preferably 105 μm or more, more preferably 110 μm or more, and particularly preferably 115 μm or more. In addition, the upper limit of the particle size D50 of the first alumina particles is not particularly limited, but from the viewpoint of good kneading properties with the resin, it is preferably 160 μm or less, more preferably 155 μm or less, more preferably 150 μm or less, further preferably 140 μm or less, and particularly preferably 135 μm or less.
[0059] As described above, the particle size D50 of the second alumina particles is 0.1 μm or more and 1.0 μm or less, preferably 0.2 μm or more, more preferably 0.3 μm or more, preferably 0.9 μm or less, more preferably 0.6 μm or less.
[0060] The alumina powder may further include third alumina particles having a particle size D50 of 3 μm or more and 70 μm or less.
[0061] The particle size D50 of the third alumina particles is preferably 4 μm or more, more preferably 8 μm or more, preferably 80 μm or less, more preferably 50 μm or less, and further preferably 20 μm or less.
[0062] Regarding the D50 of the first aluminum oxide particles, the second aluminum oxide particles, and the third aluminum oxide, the particle size distribution of each aluminum oxide particle is measured based on the principle of dynamic image analysis according to ISO 13322-2, and the cumulative particle size distribution obtained from the measurement results is used to calculate the cumulative 50% particle size (D50) from the microparticle side. As a measuring device, for example, a CAMSIZER (manufactured by Verder Scientific) is used, and samples are sequentially introduced into the device, and the particles passing in front of the camera are measured while the agglomerated particles are dispersed by dry air. In addition, a laser particle size distribution measuring device ["Microtrac: MT-3300" manufactured by Nikkiso Co., Ltd.] can also be used to measure the particle size distribution by a laser diffraction method.
[0063] When the alumina powder includes first alumina particles and second alumina particles, at least two peaks, a first peak derived from the first alumina particles and a second peak derived from the second alumina particles, may exist in the particle size distribution of the alumina powder. The position of the first peak may be close to the D50 value of the first alumina particles, and the position of the second peak may be close to the D50 value of the second alumina particles.
[0064] When the alumina powder contains third alumina particles in addition to the first alumina particles and the second alumina particles, three peaks may exist in the particle size distribution of the alumina powder, namely, a first peak derived from the first alumina particles, a second peak derived from the second alumina particles, and a third peak derived from the third alumina particles. The position of the first peak may be close to the value of D50 of the first alumina particles, the position of the second peak may be close to the value of D50 of the second alumina particles, and the position of the third peak may be close to the value of D50 of the third alumina particles.
[0065] In this way, it can be confirmed from the particle size distribution of the alumina powder that the alumina powder contains the first alumina particles, the second alumina particles, and the third alumina particles.
[0066] As described below, the alumina powder is prepared by mixing the first alumina particles, the second alumina particles, and any third alumina particles. Therefore, by measuring the particle size D50 of each alumina particle before mixing, the particle size D50 of each alumina particle contained in the alumina powder after mixing can be known.
[0067] On the other hand, as a method for determining the particle size D50 of each alumina particle from the mixed alumina powder, as an example, each alumina particle can be simply sieved by a wet sieving method using a first sieve with a mesh of 100 μm and a second sieve with a mesh of 5 μm, and the D50 of each alumina particle after sieving can be measured.
[0068] If the alumina powder is sieved with a first sieve with a mesh size of 100 μm, the first alumina particles become the sieve-surface material, and the third alumina particles and the second alumina particles become the sieve-underface material. Then, the sieve-underface material is sieved with a second sieve with a mesh size of 5 μm, whereby the third alumina particles become the sieve-surface material and the second alumina particles become the sieve-underface material. For the three alumina particles sieved in this way, D50 and various physical property values can be measured respectively. In addition, the content of each alumina particle contained in the alumina powder can also be measured.
[0069] In the case of an alumina powder contained in a resin composition, the resin is removed from the resin composition to obtain an alumina powder, and the particle size distribution of the alumina powder is measured, or the individual alumina particles in the alumina powder can be confirmed or separated by sieving. In this case, the D50 of the alumina particles is confirmed from the peak position of the particle size distribution. If a plurality of alumina particles are contained, the size of the mesh can be appropriately selected according to the value of each D50, so that the alumina particles can be sieved and separated.
[0070] In the case of the alumina powder before mixing with the resin, the particle size distribution can be directly measured or sieved.
[0071] When the total amount of the aluminum oxide powder is 100 mass %, the preferred content of each of the first aluminum oxide particles, the second aluminum oxide particles, and the third aluminum oxide particles is as follows.
[0072] The content of the first aluminum oxide particles is preferably 50.0 mass % or more and 99.0 mass % or less, and more preferably 50.0 mass % or more and 70.0 mass % or less.
[0073] The content of the second aluminum oxide particles is preferably 5.0% by mass or more and 49.9% by mass or less, and more preferably 8.0% by mass or more and 35.0% by mass or less.
[0074] The content of the third aluminum oxide particles is preferably 0 mass % to 49.9 mass %, more preferably 5.0 mass % to 40.0 mass %, particularly preferably 5.0 mass % to 35.0 mass %.
[0075] The second alumina particles are preferably polyhedral. "Polyhedral" means a polyhedron with an average sphericity (or roundness) of 0.70 or more. If the polyhedron is in a polyhedral shape, the viscosity increase when mixed with the resin can be suppressed, and the particles in the resin composition are in surface contact with each other, so the thermal conductivity is improved.
[0076] The content (mass %) of the first alumina particles in the alumina powder is preferably greater than the content (mass %) of the second alumina particles. That is, the alumina powder preferably satisfies the following formula (1).
[0077] A>B(1)
[0078] Here, A and B are the contents (mass %) of the first aluminum oxide particles and the second aluminum oxide particles, respectively, when the total amount of the aluminum oxide powder is 100 mass %.
[0079] By making the content of the first alumina particles in the alumina powder larger than the content of the second alumina particles, the heat dissipation characteristics of the resin composition can be further improved.
[0080] The ratio (expressed as a percentage (%)) of the total length L2 of the boundary line inside the particle to the length L1 of the outer edge of the first alumina particle is preferably greater than 100.0%. That is, the first alumina particle preferably satisfies the following formula (2). It should be noted that the expression "L2 / L1 (%)" means that it is obtained by the left side of the formula (2) (L2 / L1×100).
[0081] L2 / L1×100>100.0(%) (2)
[0082] Here, L1 is the length of the outer edge of the first alumina particle obtained from the SEM-EBSD image, and L2 is the total length of the boundary lines included in the first alumina particle obtained from the SEM-EBSD image.
[0083] The "total length L2 of the boundary lines" is the sum of the boundary lines included in the interior of the first alumina particle, excluding the outer edge of the first alumina particle. The total length L2 of the boundary lines is set to the sum of the total length L3 of the boundary lines of the grain boundaries and the total length L4 of the inner wall of the void (when there is a void in the interior of the first alumina particle) in the SEM-EBSD image of the first alumina particle (i.e., L2 = L3 + L4).
[0084] L2 / L1 is more preferably greater than 0.8 (ie, greater than 80.0%), further preferably greater than 1.0 (ie, greater than 100.0%), and particularly preferably greater than 1.5 (ie, greater than 150.0%).
[0085] The L2 / L1 (%) of the second alumina particles is preferably 50.0% or less, more preferably 20.0% or less, and further preferably 10.0% or less.
[0086] L2 / L1 of the third alumina particles is preferably 200.0% or less, more preferably 150.0% or less, further preferably 50.0% or less, particularly preferably 10.0% or less.
[0087] The total L2 / L1 (%) of the first alumina particles, the second alumina particles, and the third alumina particles as the alumina particles of the present embodiment is preferably 150.0% or less, more preferably 100.0% or less, further preferably 75.0% or less, and particularly preferably 50.0% or less.
[0088] When the pore volume of the first alumina particles is measured by a krypton adsorption method, the pore volume is preferably 0.00005 cm 3 / g or above.
[0089] The pore volume is an index for understanding the degree of unevenness of the particle surface, similar to the Kr-BET specific surface area. By controlling the pore volume of the first alumina particles to be within the above range, the heat dissipation characteristics of the resin composition can be further improved.
[0090] The pore volume is preferably greater than 0.00009 cm 3 / g, more preferably 0.0001cm 3 The upper limit of the pore volume is not particularly limited, and can be, for example, 10 cm 3 / g or less, and can be further 1cm 3 / g or less.
[0091] The pore volume of the second alumina particles is preferably 0.001 cm 3 / g or more, preferably 0.004cm 3 / g or less.
[0092] The pore volume of the third alumina particles is preferably 0.0001 cm 3 / g or more, preferably less than 0.001cm 3 / g.
[0093] In addition, the ratio of the pore volume of the second alumina particles to the pore volume of the first alumina particles is preferably greater than 10, more preferably 15 or more, preferably 35 or less, and more preferably 25 or less. In addition, the ratio of the pore volume of the third alumina particles to the pore volume of the first alumina particles is preferably 1.0 or more, more preferably 2.0 or more, preferably 10 or less, and more preferably 7 or less. Thus, a resin composition capable of improving heat dissipation characteristics can be provided.
[0094] When the pore volume distribution of the first alumina particles is measured by a krypton adsorption method, the peak height between pore diameters of 2 and 10 nm in the pore volume distribution is preferably greater than 0.000055 cm 3 / g.
[0095] The peak between pore diameters of 2 and 10 nm can be used as an indicator of the ease with which the resin can penetrate. Therefore, by controlling the peak value within the above range, the heat dissipation characteristics of the resin composition can be further improved.
[0096] The peak height is preferably greater than 0.000055 cm 3 The upper limit of the pore volume is not particularly limited, and may be, for example, 0.00012 cm 3 / g or less, and can be further 0.00010cm 3 / g or less.
[0097] The peak height of the second alumina particles is preferably 0.0003 cm 3 / g or more, preferably 0.003cm 3 / g or less.
[0098] The peak height of the third alumina particles is preferably 0.00006 cm 3 / g or more, preferably 0.0003cm 3 / g or less.
[0099] In addition, the ratio of the peak height of the second alumina particles to the peak height of the first alumina particles is preferably greater than 5, more preferably greater than 15, preferably less than 45, and more preferably less than 30. The ratio of the peak height of the third alumina particles to the peak height of the first alumina particles is preferably greater than 1.0, more preferably greater than 1.5, preferably less than 5, and more preferably less than 3.5. Thus, a resin composition capable of improving heat dissipation characteristics can be provided. It should be noted that these peak heights represent the height of the highest peak existing between pore diameters of 2 and 10 nm.
[0100] The alumina powder preferably has a high content of α-alumina. α-alumina has high thermal conductivity, so by increasing the content of α-alumina in the alumina powder, the thermal conductivity of the alumina powder can be increased. In the alumina powder of the embodiment of the present invention, the α-alumina content index, i.e., the α-ratio, is preferably within the following range for the first alumina particles, the second alumina particles, and the third alumina particles.
[0101] The alpha conversion rate of the first alumina particles is preferably 90% or more, more preferably 92% or more, and particularly preferably 94% or more.
[0102] The alpha conversion rate of the second alumina particles is preferably 90% or more, more preferably 92% or more, and particularly preferably 94% or more.
[0103] The alpha conversion rate of the third alumina particles is preferably 90% or more, more preferably 92% or more, and particularly preferably 94% or more.
[0104] In this specification, the "alpha conversion ratio" refers to the content ratio (volume %) of α-alumina relative to the total alumina contained in the alumina particles.
[0105] The alpha conversion rate is measured by powder X-ray diffraction of alumina particles, and the peak height (I25.6) of the α phase (012 plane) appearing at 2θ=25.6° and the peak height (I46) of the γ phase, η phase, χ phase, κ phase, θ phase and δ phase appearing at 2θ=46° are obtained from the obtained diffraction spectrum and calculated by the following formula (3).
[0106] Alpha conversion rate (%) = I 25.6 / (I 25.6 +I 46 )×100(3)
[0107] Alumina particles may contain aluminum oxides other than α-alumina (δ-alumina, θ-alumina, etc.). Alumina other than α-alumina may be contained in any manner. For example, α-alumina and aluminum oxides other than α-alumina may be contained in one alumina particle at the same time. In addition, one alumina particle may consist of only α-alumina, and another alumina particle may consist of only aluminum oxides other than α-alumina, and these alumina particles may also be mixed.
[0108] The roundness of the alumina particles is preferably 0.70 or more, which can improve the kneading property with the resin and suppress the viscosity increase of the composite. Furthermore, the wear of other parts caused by the alumina particles can also be reduced. The roundness of the first alumina particles, the second alumina particles, and the third alumina particles as the alumina particles of this embodiment is preferably 0.70 or more, more preferably 0.75 or more, particularly preferably 0.80 or more, and particularly preferably 0.85 or more.
[0109] The roundness of the alumina particles can be measured simultaneously with the particle size distribution using a measuring device based on the principle of dynamic image analysis in accordance with ISO 13322-2 (e.g., CAMSIZER X2 (manufactured by VERDER Scientific)). The roundness (SPHT) is analyzed in accordance with ISO 9276-6 and is expressed by SPHT = 4πA / P 2Calculated. A in the formula is the measured value of the area of the projected particle image, and P is the measured value of the outer perimeter of the particle projected image. The roundness can also be calculated by SEM observation of the particles. In addition, it can also be calculated by SEM cross-sectional observation of the resin composition.
[0110] By using such an alumina powder in a resin composition, a resin composition having improved heat dissipation characteristics can be produced.
[0111] The various physical properties of the above-mentioned alumina powder can be measured directly as long as it is the alumina powder before mixing with the resin. In addition, after mixing with the resin (for example, the state of the mixture of the resin and the alumina powder, or the state of the resin composition obtained by curing the mixture), the alumina powder after removing the resin can be measured.
[0112] [Method for producing alumina powder]
[0113] The method for producing an alumina powder includes mixing first alumina particles, second alumina particles, and any third alumina particles.
[0114] The mixing method is not particularly limited, and a mixing method such as mixing in a mortar, mixing by rotation and revolution under vacuum, etc. can be used.
[0115] When mixing two kinds of aluminum oxide particles, the prescribed amounts of each are weighed and put into a mixing container for mixing. When mixing three kinds of aluminum oxide particles, the prescribed amounts of each can be weighed and all added to the mixing container for mixing at the same time, or can be added and mixed sequentially.
[0116] [Method for producing alumina particles]
[0117] The method for producing the alumina particles (first alumina particles, second alumina particles, and any third alumina particles) constituting the alumina powder is not particularly limited, and the alumina particles may be produced by any production method as long as the physical properties required of each alumina particle can be achieved.
[0118] In addition, commercially available alumina particles may be used as the respective alumina particles.
[0119] It should be noted that when manufacturing the first alumina particles, it is preferred to use particles formed by agglomeration of fine α-alumina as a raw material and manufacture them by a flame melting method. The alumina particles thus obtained have fine irregularities on the surface, so that a Kr-BET specific surface area of more than 0.085 m 2 / g of alumina particles.
[0120] In the production of the first alumina particles by the flame fusion method, for example, Figure 1 The device shown.
[0121] In order to produce the first alumina particles having a D50 greater than 100 μm by the flame melting method, first, alumina particles having a D50 of 70 μm or more are used as raw materials, preferably 90 μm or more. After flame melting, the particles are sieved with a 100 μm sieve, and the particles on the sieve are recovered.
[0122] The D50 of the alumina raw material particles can be measured by the same method as the above-mentioned method for measuring the D50 of the alumina particles.
[0123] The supply rate of the fuel gas (such as LPG gas) used in the flame melting is preferably 20 Nm 3 / hour or more. According to the supply amount of fuel gas, the flame length can be changed. The more the fuel gas is supplied, the longer the flame length is, and the longer the residence time of the particles in the flame is. The smaller the supply amount of fuel gas is, the shorter the flame length is, and the residence time of the particles in the flame can be shortened. In other words, the residence time of the alumina raw material particles in the flame can be changed, and the melting degree (time) of the alumina raw material particles in the flame can be changed. In addition, the surface of the alumina particles can be made to have unevenness while maintaining the crystal structure of the raw material particles of the alumina raw material particles, and a Kr-BET specific surface area greater than 0.085m 2 / g of alumina particles.
[0124] [Resin]
[0125] The resin used in the resin composition can be selected from thermoplastic resins, thermoplastic elastomers, and thermosetting resins. The resins may be used alone or in combination of two or more.
[0126] Examples of the thermoplastic resin include polyolefin resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; fluorine-based polymers such as polymethylpentene, polyvinyl chloride, polyvinylidene chloride, polyvinyl acetate, ethylene-vinyl acetate copolymers, polyvinyl alcohol, polyvinyl acetal, polyvinylidene fluoride, and polytetrafluoroethylene; polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polystyrene, polyacrylonitrile, styrene-acrylonitrile copolymers, acrylonitrile-butadiene-styrene copolymer (ABS) resins, polyphenylene ether copolymer (PPE) resins, modified PPE resins, aliphatic polyamides, aromatic polyamides, polyimides, polyamide-imides, polymethacrylic acid, polymethyl methacrylate, and other polymethacrylates; polyacrylic acids, polycarbonates, polyphenylene sulfide, polysulfones, polyethersulfones, polyether nitrile, polyether ketones, polyketones, liquid crystal polymers, silicone resins, ionomers, and the like.
[0127] Examples of the thermoplastic elastomer include styrene-butadiene block copolymers or hydrogenated products thereof, styrene-isoprene block copolymers or hydrogenated products thereof, styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, polyester-based thermoplastic elastomers, polyurethane-based thermoplastic elastomers, and polyamide-based thermoplastic elastomers.
[0128] Examples of the thermosetting resin include crosslinked rubber, epoxy resin, phenolic resin, polyimide resin, unsaturated polyester resin, diallyl phthalate resin, etc. Specific examples of the crosslinked rubber include natural rubber, acrylic rubber, butadiene rubber, isoprene rubber, styrene-butadiene copolymer rubber, nitrile rubber, hydrogenated nitrile rubber, chloroprene rubber, ethylene-propylene copolymer rubber, chlorinated polyethylene rubber, chlorosulfonated polyethylene rubber, butyl rubber, halogenated butyl rubber, fluororubber, polyurethane rubber, and silicone rubber.
[0129] From the viewpoint of processability and properties, polyolefin resins, acrylic resins, polyimide resins, polyamide resins, polyamideimide resins, epoxy resins, phenolic resins, and silicone resins are preferably used.
[0130] Furthermore, in these resin compositions, as required, known additives such as a plasticizer, a curing accelerator, a coupling agent, a filler, a pigment, a flame retardant, an antioxidant, a surfactant, a compatibilizer, a weathering agent, an anti-blocking agent, an antistatic agent, a leveling agent, a release agent, etc. may be appropriately formulated alone or in combination within a range that does not impair the effects of the invention.
[0131] When the resin composition is 100 mass %, the content of the resin is preferably 4 mass % to 15 mass %, more preferably 6 mass % to 10 mass %. Within this range, the effect of improving the heat dissipation characteristics by using the first alumina particles having surface irregularities is significant.
[0132] The content of the resin contained in the resin composition can be obtained based on the mass of the resin composition measured in advance and the mass of the alumina powder obtained by removing the resin from the resin composition. Specific methods for removing the resin from the resin composition include a method of removing the resin by dissolving it with a solvent, a method of removing the resin by incinerating the resin composition, and the like.
[0133] [Method for producing resin composition]
[0134] The method for producing the resin composition includes a mixing step of mixing alumina powder and a resin.
[0135] In the mixing step, a commonly used known method can be used to mix the resin and the alumina powder to obtain a resin composition.
[0136] For example, when the resin is liquid (such as liquid epoxy resin), the liquid resin, alumina particles and a curing agent are mixed and then cured by heat or ultraviolet rays to obtain a resin composition. The curing agent, mixing method and curing method can use known substances and methods.
[0137] On the other hand, when the resin is solid (for example, polyolefin resin, acrylic resin, etc.), the target resin composition can be obtained by mixing the resin and alumina particles and then kneading them by a known method such as melt kneading.
[0138] The alumina powder used in the resin composition has a particle size D50 greater than 100 μm and a BET specific surface area measured by a krypton adsorption method greater than 0.085 m 2 / g and second alumina particles having a particle size D50 of 0.1 μm or more and 1.0 μm or less are mixed.
[0139] The first alumina particles and the second alumina particles may be mixed before or simultaneously with the mixing step of mixing the alumina powder and the resin.
[0140] For example, before the mixing step, the first alumina particles and the second alumina particles may be mixed in advance to prepare an alumina powder, and then the mixing step of mixing the resin and the alumina powder may be performed.
[0141] In another example, in the step of mixing the resin and the alumina powder, the resin, the first alumina particles, and the second alumina particles may be placed in a mixing container and mixed. Thus, the resin and the alumina powder including the first alumina particles and the second alumina particles may be substantially mixed.
[0142] When the alumina powder contains third alumina particles in addition to the first alumina particles and the second alumina particles, the order and timing of mixing these three types of alumina particles can be arbitrarily selected.
[0143] Regarding the order of mixing the three types of alumina particles, for example, the first alumina particles, the second alumina particles, and the third alumina particles may be mixed simultaneously to prepare the alumina powder.
[0144] In another example, the alumina powder may be prepared by sequentially adding the other two types of alumina particles to any one type of alumina particles and mixing them.
[0145] The timing for mixing the three types of alumina particles may be before and / or during the mixing step of mixing the alumina powder and the resin.
[0146] For example, before the mixing step, a mixing step may be performed in which three types of alumina particles are mixed in advance to prepare an alumina powder, and then the resin and the alumina powder are mixed.
[0147] In another example, two kinds of mixed alumina particles obtained by mixing two kinds of alumina particles in advance may be prepared, and then the two kinds of mixed alumina particles, the remaining one kind of alumina particles, and the resin may be added to a mixing container and mixed.
[0148] In another example, the resin and three types of alumina particles may be placed in a mixing container and mixed.
[0149] Example
[0150] 1. Preparation of test samples
[0151] 1) Preparation of alumina particles
[0152] Alumina particles No. 1a, 1b, 2a, and 3a were prepared having the properties shown in Table 1. Alumina particle No. 1a was prepared by the following procedure, and commercially available alumina particles were used for the other alumina particles.
[0153] 2) Preparation of Alumina Particle No.1a
[0154] Alumina particles No. 1a were produced by a flame fusion method.
[0155] First, raw material particles made of single-crystalline aluminum oxide are prepared. The aluminum oxide raw material particles have an angular shape.
[0156] The alumina raw material particles were sieved with a sieve having an opening of 132 μm, and the alumina raw material particles on the sieve were used as a raw material of alumina particles No. 1a.
[0157] use Figure 1 The apparatus shown in the figure produces aluminum oxide particles No. 1a from raw materials. Figure 1 In the device, oxygen from the oxygen supply system 10 is split, one side (carrier oxygen 11) is supplied to the feeder 30, and the other side (combustion oxygen 12) is supplied to the burner 41 of the flame melting furnace 40. The raw material supplied to the feeder 30 is transported to the burner 41 of the flame melting furnace 40 by the carrier oxygen 11. In addition, the gas supply system 20 is supplied with less than 20Nm 3 / hour, the fuel gas (LPG) is supplied to the burner 41. In the burner 41, a high-temperature flame of 2150°C or higher is formed by the fuel gas and the combustion oxygen 12, and the raw material dispersed in the carrier gas oxygen 11 is supplied thereto. As a result, the raw material is melted and spheroidized in the flame melting furnace 40. Then, the spheroidized alumina particles are classified by the cyclone separator 50, and the cyclone separator 50 is replenished with alumina particles No. 1a.
[0158] 3) Preparation of Alumina Particle No. 1b
[0159] Regarding alumina particles No. 1b, polycrystalline alumina particles (D50: 95 μm) produced by the Bayer process were used as a raw material, and the flow rate of the fuel gas (LPG) was set to 40 Nm 3 / hour, except that the spheroidization was performed by flame melting method under the same conditions as No.1a. The spheroidized alumina particles were captured in cyclone separator 50, and the recovered alumina particles were sieved with a sieve with a mesh size of 100 μm. The alumina raw material particles on the sieve were used as alumina particles No.1b.
[0160] 4) Preparation of alumina powder
[0161] Alumina powder (Examples 1 to 2 and Reference Example 1) is prepared by mixing first alumina particles (alumina particles No. 1a or 1b; both are spherical), second alumina particles (alumina particles No. 2a; polyhedral spheres) and third alumina particles (alumina particles No. 3a; spherical) in the proportion (ratio of the content of each alumina particle) shown in Table 2.
[0162] 5) Preparation of a mixture of alumina powder and resin (mixed sample)
[0163] Alumina powder and resin are mixed according to the mixing ratio (ratio of the content of alumina powder to resin) shown in Table 2, and kneaded using an auto-rotation and revolution mixer (ARV-310) manufactured by THINKY Co., Ltd. to obtain a mixture of alumina powder and resin (mixed samples of Examples 1 to 2 and Reference Example 1).
[0164] As the resin, room temperature curing embedding resin 53 type epoxy resin (manufactured by Sankei Co., Ltd.) was used.
[0165] 2. Determination of particle size D50 of alumina particles
[0166] The particle size distribution of alumina particles No. 1a, 1b, 2a, and 3a was measured to determine the particle size D50. The measurement results are shown in Table 1.
[0167] The particle size distribution of the alumina particles is measured by a device CAMSIZER X2 (manufactured by VERDER Scientific) based on the principle of dynamic image analysis according to ISO 13322-2. The measurement is dry, and the samples are put into the device in sequence, and the particles passing in front of the camera are measured while the agglomerated particles are dispersed by 50kPa dry air. Weigh 3g of the measurement sample and measure it once. Repeat the same measurement 3 times, and analyze the particle size distribution based on the cumulative average of these results. The particle size is the equivalent circle particle size. The equivalent circle particle size refers to the particle size of a true circle with the same area as the projected particle image. In addition, the benchmark of the particle size is set to volume.
[0168] 3. Determination of Kr-BET specific surface area, pore volume distribution and pore volume of alumina particles
[0169] The pore volume distribution, Kr-BET specific surface area and pore volume of alumina particles No. 1a, 1b, 2a and 3a were measured.
[0170] The method for measuring the specific surface area of powder (solid) based on gas adsorption is based on JIS Z 8830:2013, using Kr as the adsorption gas. During the measurement, 1 g of alumina particles is placed in a sample tube, and the adsorption-desorption isotherm is obtained. The Kr-BET specific surface area (m 2 The Kr-BET specific surface area and pore volume were determined by pore volume distribution analysis. In addition, the peak height between pore diameters of 2 and 10 nm was determined from the pore volume distribution. The respective measurement results are shown in Table 1.
[0171] 4. Measurement of the total length L1 of the outer edge of the alumina particle and the length L2 of the boundary line inside the particle
[0172] Alumina particles No. 1a, 1b, 2a, and 3a were used to prepare cross-sectional observation samples. In the preparation of cross-sectional observation samples, the alumina particles were embedded in resin, and then the resin and the alumina particles were cut with a diamond tool. Then, Pt was vapor-deposited on the cross section as a protective film, the cross section was prepared by Ar ion milling, and it was fixed on the SEM sample stage with Cu double-sided tape, and SEM-EBSD measurement was performed without vapor deposition. The observation position was determined in such a way that more than two alumina particles completely entered the observation area (that is, more than two alumina particles did not contact the frame of the observation area).
[0173] The following equipment was used for sample preparation and EBSD measurement.
[0174] Use of equipment
[0175] Ion milling device: IM-4000 (manufactured by Hitachi, Ltd.)
[0176] Ion sputtering device: E-1030 (manufactured by Hitachi, Ltd.)
[0177] Ultra-high-resolution field emission scanning electron microscope: JSM-7800F Prime (manufactured by JEOL Ltd.)
[0178] Backscattered electron diffraction device: Digiview V (manufactured by TSL)
[0179] The conditions for EBSD measurement are as follows.
[0180] ·Measurement area: 500.0μm×400.0μm
[0181] Accelerating voltage: 20.0 kV
[0182] ·Magnification:×500
[0183] Low vacuum: 30Pa
[0184] In the obtained EBSD image, select two or more alumina particles that are not in contact with the frame of the observation area. Use the image processing software Image J (manufactured by the National Institute of Health) to find the length L1 of the outer edge of each alumina particle and calculate its average value. In addition, the total length L2 of the boundary lines of each alumina particle is also found using the same image processing software, and their average value is calculated. "The total length L2 of the boundary lines" is the sum of the boundary lines contained in the interior of the alumina particles, excluding the outer edges of the alumina particles. The total length L2 of the boundary lines is obtained by adding the total length of the grain boundaries inside the alumina particles and the total length of the inner wall of the void (when there is a void inside the alumina particles).
[0185] The ratio L2 / L1 (%) of the total length L2 (average value) of the boundary line to the length L1 (average value) of the outer edge was calculated (ie, L2L1×100).
[0186] 5. Determination of thermal conductivity
[0187] A sample piece for measuring thermal conductivity was prepared from the mixed samples of Examples 1 to 2 and Reference Example 1 shown in Table 2. 2 g of the mixed sample was placed in a mold with a diameter of 20 mm, molded under a pressure of 30 MPa, and left at room temperature for 24 hours to cure the resin.
[0188] The solidified molded body was processed into a size of 10 mm square × 2 mm thick, and the surface-polished test piece was used as the test piece. The thermal conductivity in the thickness direction of the test piece was measured by the laser flash method using a xenon flash analyzer (LFA467 manufactured by NETZSCH). The measurement was performed under the condition of 25°C in the air atmosphere.
[0189] Table 1
[0190]
[0191] Table 2
[0192]
[0193] Table 3
[0194] Test No. Thermal conductivity (w / mK) Example 1 4.2 Example 2 5.2 Reference Example 1 2.56
[0195] In Examples 1 and 2, since the alumina powder satisfying the conditions of the present embodiment is used, the thermal conductivity of the resin composition is high.
[0196] Although the thermal conductivity of the resin composition prepared in Reference Example 1 is high enough to be used as a heat dissipation member, the thermal conductivities of Examples 1 and 2 are significantly higher than those of Reference Example 1. This shows that the effect of controlling the Kr-BET specific surface area of the first alumina particles is high.
[0197] Description of Reference Numerals
[0198] 10Oxygen supply system
[0199] 11Carrier gas oxygen
[0200] 12 Combustion Oxygen
[0201] 20Fuel gas supply system
[0202] 30 feeder
[0203] 40 Flame Melting Furnace
[0204] 50 Cyclone separator
Claims
1. A resin composition comprising a resin and an aluminum oxide powder, in, The aluminum oxide powder comprises: The particle size D50 is greater than 100 μm and the BET specific surface area measured by krypton adsorption method is greater than 0.085 m 2 / g of first alumina particles, and The second alumina particles have a particle diameter D50 of 0.1 μm or more and 1.0 μm or less.
2. The resin composition according to claim 1, in, The aluminum oxide powder satisfies the following formula (1): A>B(1) Here, A and B are the contents of the first aluminum oxide particles and the second aluminum oxide particles, respectively, in mass % when the total amount of the aluminum oxide powder is 100 mass %.
3. The resin composition according to claim 1 or 2, in, The first aluminum oxide particles satisfy the following formula (2): L2 / L1×100>100.0(%) (2) Here, L1 is the length of the outer edge of the first alumina particle obtained from the SEM-EBSD image, and L2 is the total length of the boundary lines included in the first alumina particle obtained from the SEM-EBSD image.
4. The resin composition according to claim 1 or 2, in, The pore volume of the first alumina particles measured by a krypton adsorption method was 0.00005 cm 3 / g or above.
5. The resin composition according to claim 1 or 2, in, In the pore volume distribution of the first alumina particles measured by the krypton adsorption method, the peak height existing between pore diameters of 2 and 10 nm is greater than 0.000055 cm 3 / g.
6. The resin composition according to claim 1 or 2, in, The alumina powder further includes third alumina particles having a particle size D50 of 3 μm or more and 70 μm or less.
7. An aluminum oxide powder comprising: a particle size D50 greater than 100 μm and a BET specific surface area measured by a krypton adsorption method greater than 0.085 m 2 / g of first alumina particles, and The second alumina particles have a particle diameter D50 of 0.1 μm or more and 1.0 μm or less.
8. The aluminum oxide powder according to claim 7, which satisfies the following formula (1): A>B(1) in, A and B are the contents of the first aluminum oxide particles and the second aluminum oxide particles, respectively, in mass % when the total amount of the aluminum oxide powder is 100 mass %.
9. The aluminum oxide powder according to claim 7 or 8, in, The first aluminum oxide particles satisfy the following formula (2): L2 / L1×100>100.0(%) (2) Here, L1 is the length of the outer edge of the first alumina particle obtained from the SEM-EBSD image, and L2 is the total length of the boundary lines included in the first alumina particle obtained from the SEM-EBSD image.
10. The aluminum oxide powder according to claim 7 or 8, in, The pore volume of the first alumina particles measured by a krypton adsorption method was 0.00005 cm 3 / g or above.
11. The aluminum oxide powder according to claim 7 or 8, in, In the pore volume distribution of the first alumina particles measured by the krypton adsorption method, the peak height existing between pore diameters of 2 and 10 nm is greater than 0.000055 cm 3 / g. 12 . The aluminum oxide powder according to claim 7 , further comprising third aluminum oxide particles having a particle size D50 of 3 μm or more and 70 μm or less.