Photosensitive resin composition, photosensitive element, printed wiring board, and method for producing printed wiring board
By using an acid-modified vinyl-containing resin and a variety of photopolymerization initiators, the problem of the decrease in sensitivity of the photosensitive resin composition in the printed circuit board at different exposure wavelengths and the deterioration of the through-hole shape is solved, and high sensitivity and A good-shaped through-hole opening, suitable for the manufacture of permanent resist for printed circuit boards.
Patent Information
- Application Number
- CN202480002248.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-03-14
- Publication Date
- 2024-12-06
AI Technical Summary
In the production of printed circuit boards, when using a photosensitive resin composition, different exposure wavelengths lead to problems such as degradation of sensitivity and deterioration of through-hole shape.
The photosensitive resin composition containing an acid-modified vinyl-containing resin, an alkylbenzone-based, an oxime-ester-based and a benzophenone-based photopolymerization initiator is adopted, and the ratio and combination of these photopolymerization initiators are adjusted to combine. The thioxanthone compound, a sensitizer, a pigment and an inorganic filler form a negative photosensitive resin composition to improve sensitivity to various exposure wavelengths and the shape quality of the through-hole opening.
Through-hole openings that maintain high sensitivity and good shape under various exposure wavelengths are realized, which are suitable for forming permanent resists and improve the manufacturing efficiency and quality of printed circuit boards.
Smart Images

Figure CN119096200A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a photosensitive resin composition, a photosensitive element, a printed circuit board and a method for manufacturing the printed circuit board. Background Art
[0002] In the field of manufacturing printed wiring boards, a process of forming a permanent resist on a printed wiring board is being carried out. The permanent resist has the function of preventing corrosion of a conductor layer or maintaining electrical insulation between conductor layers when the printed wiring board is used. In recent years, the permanent resist has also become a process of preventing solder from adhering to unnecessary parts of the conductor layer of the printed wiring board in the process of flip-chip mounting, wire bonding mounting, etc. of semiconductor elements on the printed wiring board via solder, that is, as a solder resist film.
[0003] In the past, permanent resists in the manufacture of printed circuit boards were made by screen printing using a thermosetting resin composition or by photographic methods using a photosensitive resin composition. For example, in flexible circuit boards using mounting methods such as FC (FlipChip), TAB (Tape Automated Bonding), and COF (Chip On Film), in addition to IC chips, electronic parts or LCD (Liquid Crystal Display) panels and connection circuit parts, thermosetting resin paste is screen-printed and thermally cured to form a permanent resist (for example, refer to Patent Document 1).
[0004] Furthermore, in semiconductor package substrates such as BGA (Ball Grid Array) and CSP (Chip Size Package) mounted on electronic parts, (1) in order to flip-chip mount the semiconductor element on the semiconductor package substrate via solder, (2) in order to wire-bond the semiconductor element and the semiconductor package substrate, or (3) in order to solder the semiconductor package substrate to the main board substrate, it is necessary to remove the permanent resist of the bonding portion. Therefore, in the formation of the permanent resist, a photographic method is used, which is to selectively irradiate active light such as ultraviolet rays to cure the photosensitive resin composition after applying and drying it, and to form an image by removing only the unirradiated portion through development. The photographic method is suitable for mass production due to its good operability, and is therefore widely used in the electronic materials industry for the image formation of photosensitive resin compositions (for example, refer to Patent Documents 2 and 3). Among the exposure machines used when irradiating active light, there are widely known mask-free projection exposure machines and mask-free direct writing exposure machines. Direct writing exposure machines that do not require a mask are expected to become more widespread in the future due to their high productivity.
[0005] Previous technical literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2003-198105
[0008] Patent Document 2: Japanese Patent Application Publication No. 2011-133851
[0009] Patent Document 3: International Publication No. 2013 / 022068 Summary of the invention
[0010] Technical issues to be solved by the invention
[0011] There are various types of exposure machines for curing photosensitive resin compositions, and as a light source for active light rays, in addition to a light source emitting i-ray monochromatic light (wavelength 365nm), a light source emitting mixed rays including i-ray and h-ray (wavelength 405nm) having a wavelength longer than i-ray is used. In this case, when the same photosensitive resin composition is used for various exposure wavelengths, depending on the exposure wavelength, problems such as a decrease in the sensitivity of the photosensitive resin composition, or a deterioration in the shape of the through-hole opening portion such as a through-hole formed in the permanent resist not opening or a decrease in the taper angle are likely to occur.
[0012] Therefore, an object of the present invention is to provide a photosensitive resin composition having good sensitivity to various exposure wavelengths and capable of forming a through-hole opening having a good shape, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board.
[0013] Means for solving technical problems
[0014] In order to solve the above-mentioned problems, the present invention provides the following photosensitive resin composition, photosensitive element, printed wiring board, and method for producing the printed wiring board.
[0015] [1] A photosensitive resin composition comprising (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound, and (D) a polymerization inhibitor, wherein the (B) photopolymerization initiator comprises (B1) an alkylphenone-based photopolymerization initiator, (B2) an oxime ester-based photopolymerization initiator, and (B3) a benzophenone-based photopolymerization initiator.
[0016] [2] The photosensitive resin composition according to [1] above, wherein
[0017] The content of the (B1) alkylphenone photopolymerization initiator is 30% by mass or more based on the total amount of the (B1) alkylphenone photopolymerization initiator, the (B2) oxime ester photopolymerization initiator, and the (B3) benzophenone photopolymerization initiator.
[0018] [3] The photosensitive resin composition according to [1] or [2] above, wherein
[0019] The content of the (B2) oxime ester photopolymerization initiator is 0.5 to 30% by mass based on the total amount of the (B1) alkylphenone photopolymerization initiator, the (B2) oxime ester photopolymerization initiator, and the (B3) benzophenone photopolymerization initiator.
[0020] [4] The photosensitive resin composition according to any one of [1] to [3] above, wherein
[0021] The content of the benzophenone-based photopolymerization initiator (B3) is 0.2 to 50% by mass based on the total amount of the alkylphenone-based photopolymerization initiator (B1), the oxime ester-based photopolymerization initiator (B2) and the benzophenone-based photopolymerization initiator (B3).
[0022] [5] The photosensitive resin composition according to any one of [1] to [4] above, further comprising (E) a sensitizer.
[0023] [6] The photosensitive resin composition according to any one of [1] to [5] above, further comprising (F) a pigment.
[0024] [7] The photosensitive resin composition according to any one of [1] to [6] above, further comprising (G) an inorganic filler.
[0025] [8] The photosensitive resin composition according to any one of [1] to [7] above, wherein
[0026] The (B) photopolymerization initiator further contains (B4) a thioxanthone compound.
[0027] [9] The photosensitive resin composition according to [8] above, wherein
[0028] The content of the (B4) thioxanthone compound is 0.1 to 50 parts by mass based on 100 parts by mass of the total amount of the (B1) alkylphenone photopolymerization initiator, the (B2) oxime ester photopolymerization initiator, and the (B3) benzophenone photopolymerization initiator.
[0029]
[10] A photosensitive element comprising a support film and a photosensitive layer formed on the support film, wherein the photosensitive layer comprises the photosensitive resin composition according to any one of [1] to [9] above.
[0030]
[11] A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to any one of [1] to [9] above.
[0031]
[12] A method for manufacturing a printed circuit board, comprising:
[0032] The process of forming a photosensitive layer on a substrate using the photosensitive resin composition described in any one of [1] to [9]; exposing and developing the photosensitive layer to form a resist pattern; and curing the resist pattern to form a permanent resist.
[0033]
[13] A method for manufacturing a printed circuit board, comprising:
[0034] The process of forming a photosensitive layer on a substrate using the photosensitive element described in
[10] above; the process of exposing and developing the photosensitive layer to form a resist pattern; and the process of curing the resist pattern to form a permanent resist.
[0035] Effects of the Invention
[0036] According to the present invention, there can be provided a photosensitive resin composition having good sensitivity to various exposure wavelengths and capable of forming a through-hole opening having a good shape, a photosensitive element using the photosensitive resin composition, a printed wiring board, and a method for producing a printed wiring board. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a cross-sectional view schematically showing a photosensitive element according to this embodiment.
[0038] Figure 2 It is a cross-sectional view schematically showing a through hole opening formed in a permanent resist. DETAILED DESCRIPTION
[0039] Hereinafter, the present invention will be described in detail. In this specification, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the expected effect of the process is achieved. Regarding the term "layer", when observed in a top view, in addition to the structure of the shape formed on the entire surface, it also includes a structure of the shape formed on a part. The numerical range represented by "~" indicates a range in which the numerical values recorded before and after "~" are included as the minimum and maximum values, respectively. Within the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be replaced by the upper limit or lower limit of the numerical range of other stages. Within the numerical range recorded in this specification, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiment.
[0040] In the present specification, when the amount of each component in a composition is mentioned, or when a plurality of substances corresponding to each component are present in a composition, unless otherwise specified, the amount refers to the total amount of the plurality of substances present in the composition.
[0041] In this specification, the so-called "(meth)acrylate" refers to at least one of "acrylate" and its corresponding "methacrylate", and the same applies to other similar expressions such as (meth)acrylic acid, (meth)acryloyl, etc. In this specification, "solid content" refers to non-volatile components other than volatile substances (water, solvent, etc.) contained in the photosensitive resin composition, and also includes components that are liquid, syrupy, or waxy at room temperature (about 25°C).
[0042] [Photosensitive resin composition]
[0043] The photosensitive resin composition involved in the present embodiment contains (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound, and (D) a polymerization inhibitor, wherein the (B) photopolymerization initiator includes (B1) an alkylphenone-based photopolymerization initiator, (B2) an oxime ester-based photopolymerization initiator, and (B3) a benzophenone-based photopolymerization initiator. According to the photosensitive resin composition involved in the present embodiment, by having the above-mentioned structure, it has good sensitivity to various exposure wavelengths and can form a through-hole opening with a good shape. The photosensitive resin composition involved in the present embodiment can be used to form a permanent resist. The photosensitive resin composition involved in the present embodiment is a negative photosensitive resin composition, and the cured film of the photosensitive resin composition can be used as a permanent resist. Below, each component used in the photosensitive resin composition of the present embodiment is described in more detail.
[0044] (Component (A): acid-modified vinyl-containing resin)
[0045] The photosensitive resin composition involved in this embodiment contains an acid-modified vinyl-containing resin as component (A). The acid-modified vinyl-containing resin is not particularly limited as long as it has a vinyl group as a photopolymerizable ethylenically unsaturated bond and an alkali-soluble acidic group. As the acidic group possessed by the acid-modified vinyl-containing resin, for example, a carboxyl group, a sulfonic group, and a phenolic hydroxyl group can be cited. Among these, a carboxyl group is preferred from the viewpoint of resolution.
[0046] Examples of the acid-modified vinyl-containing resin include acid-modified vinyl-containing epoxy resins and acid-modified vinyl-containing phenol resins.
[0047] As the acid-modified vinyl-containing epoxy resin, for example, acid-modified epoxy (meth) acrylate can be cited. Acid-modified epoxy (meth) acrylate is a resin obtained by acid-modifying epoxy (meth) acrylate, which is a reaction product of an epoxy resin and an organic acid having a vinyl group. As the acid-modified epoxy (meth) acrylate, for example, an addition reaction product obtained by adding a saturated or unsaturated polybasic acid anhydride (c) to an esterified product obtained by reacting an epoxy resin (a) with a vinyl-containing monocarboxylic acid (b) can be used.
[0048] As epoxy resin (a), for example, bisphenol novolac epoxy resin, novolac epoxy resin, bisphenol A epoxy resin, bisphenol F epoxy resin, trisphenol methane epoxy resin, biphenyl epoxy resin, naphthalene epoxy resin, and dicyclopentadiene epoxy resin can be cited. Among these, from the viewpoint of resolution, epoxy resin (a) preferably contains at least one selected from the group consisting of dicyclopentadiene epoxy resin and bisphenol F novolac epoxy resin. And, from the viewpoint of developability, epoxy resin (a) preferably does not have a fluorene skeleton.
[0049] Examples of the vinyl group-containing monocarboxylic acid (b) include acrylic acid, a dimer of acrylic acid, methacrylic acid, β-furfuryl acrylic acid, β-styryl acrylic acid, cinnamic acid, crotonic acid, α-cyanocinnamic acid and other acrylic acid derivatives; half-ester compounds of reaction products of hydroxyl-containing (meth)acrylates and dibasic acid anhydrides; and half-ester compounds of reaction products of vinyl-containing monoglycidyl ethers or vinyl-containing monoglycidyl esters and dibasic acid anhydrides.
[0050] Examples of the hydroxyl-containing (meth)acrylate, vinyl-containing monoglycidyl ether, and vinyl-containing monoglycidyl ester include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, pentaerythritol pentamethacrylate, glycidyl acrylate, and glycidyl methacrylate.
[0051] Examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.
[0052] As the saturated or unsaturated polybasic acid anhydride (c), for example, succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride can be cited. Among these, tetrahydrophthalic anhydride can also be used as the polybasic acid anhydride from the viewpoint of obtaining a photosensitive resin composition capable of forming a pattern with excellent resolution.
[0053] The acid value of component (A) is not particularly limited. From the viewpoint of improving the solubility of the unexposed portion in an alkaline aqueous solution, the acid value of component (A) may be 30 mgKOH / g or more, 40 mgKOH / g or more, or 50 mgKOH / g or more. From the viewpoint of improving the electrical properties of the cured film, the acid value of component (A) may be 150 mgKOH / g or less, 120 mgKOH / g or less, or 100 mgKOH / g or less.
[0054] The weight average molecular weight (Mw) of the (A) component is not particularly limited. From the viewpoint of improving the adhesion of the cured film, the Mw of the (A) component may be 3000 or more, 4000 or more, or 5000 or more. From the viewpoint of improving the resolution of the photosensitive layer, the Mw of the (A) component may be 30000 or less, 25000 or less, or 18000 or less. Mw can be measured by gel permeation chromatography (GPC).
[0055] From the viewpoint of improving the heat resistance, electrical properties and chemical resistance of the cured film, the content of the component (A) in the photosensitive resin composition may be 20 to 70 mass %, 25 to 60 mass %, or 30 to 50 mass % based on the total solid content of the photosensitive resin composition.
[0056] (Component (B): photopolymerization initiator)
[0057] The photosensitive resin composition according to the present embodiment includes (B1) an alkylphenone-based photopolymerization initiator (hereinafter, also referred to as "component (B1)"), (B2) an oxime ester-based photopolymerization initiator (hereinafter, also referred to as "component (B2)"), and (B3) a benzophenone-based photopolymerization initiator (hereinafter, also referred to as "component (B3)") as component (B). The photosensitive resin composition according to the present embodiment can suppress changes in light absorbance caused by exposure wavelength by using the above-mentioned components (B1), (B2), and (B3) at the same time, and can have good sensitivity even at various exposure wavelengths and form a through-hole opening having a good shape.
[0058] Here, the absorption spectrum of component (B1) reaches more than 300nm, thereby exerting the effect of being able to cure even under exposure conditions in the long wavelength region. From the viewpoint of further improving this effect, component (B1) is preferably a component with maximum absorption above 260nm in the wavelength region above 220nm. In addition, component (B2) can produce free radical species with small size. Since free radical species with small size are easy to move in the resin, the photosensitive resin composition can be effectively cured, and the effect of improving sensitivity can be exerted. In addition, component (B3) can act as a sensitizer and effectively cure the photosensitive resin composition, and the effect of improving sensitivity can be exerted, because of the state crossover from the singlet excited state to the triplet excited state when irradiated with ultraviolet light.
[0059] As (B1) component, for example, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone, 2,2-dimethoxy-2-phenylacetophenone and 2,2-diethoxy-2-phenylacetophenone can be mentioned. In addition, (B1) component is a compound that does not conform to any of (B2) component and (B3) component, that is, a compound that does not have an oxime ester structure and does not have a benzophenone skeleton. These can be used alone or in combination of two or more.
[0060] As the component (B2), for example, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyl oxime), 1-[4-(phenylthio)phenyl]octane-1,2-dione=2-(O-benzoyl oxime) and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime], etc. can be mentioned. These can be used alone or in combination of two or more.
[0061] As (B3) component, for example, benzophenone, 4,4'-bis (dimethylamino) benzophenone (Michler's ketone), 4,4'-bis (diethylamino) benzophenone, 4-methoxy-4'-dimethylamino benzophenone, 4,4'-dichlorobenzophenone, 4-benzoyl-4'-methyl diphenyl sulfide, etc. can be cited. In addition, (B3) component is a compound that does not conform to (B2) component, that is, a compound that does not have an oxime ester structure. These can be used alone or in combination of two or more.
[0062] (B) component may also contain other photopolymerization initiators other than the above-mentioned (B1) component, (B2) component and (B3) component. As other photopolymerization initiators, for example, xanthone compounds, thioxanthone compounds, anthraquinone compounds, ketal compounds, imidazole compounds, acridine compounds, acylphosphine oxide compounds, and tertiary amine compounds can be cited. Among these, (B) component preferably contains (B4) thioxanthone compound (hereinafter, also referred to as "(B4) component").
[0063] Among other photopolymerization initiators, examples of the thioxanthone compound (B4) include thioxanthone, 2-isopropyl thioxanthone, 2-dodecyl thioxanthone, 2-cyclohexyl thioxanthone, 2,4-diethyl thioxanthone, 2,4-dimethyl thioxanthone, 1-phenoxy thioxanthone, 1-methoxycarbonyl thioxanthone, 2-ethoxycarbonyl thioxanthone, 3-(2-methoxyethoxycarbonyl)-thioxanthone, 4-butoxycarbonyl thioxanthone, 3-butoxycarbonyl-7-methyl thioxanthone, 3,4-di-[2-(2-methoxyethoxy)-ethoxycarbonyl]-thioxanthone, 2- Chlorothioxanthone, 1-ethoxycarbonyl-3-ethoxythioxanthone, 1-ethoxycarbonyl-3-chlorothioxanthone, 1-chloro-4-n-propoxythioxanthone, 2-methyl-6-dimethoxymethyl-thioxanthone, 2-methyl-6-(1,1-dimethoxybenzyl)-thioxanthone, 6-ethoxycarbonyl-2-methoxy-thioxanthone, 6-ethoxycarbonyl-2-methylthioxanthone, 1-ethoxycarbonyl-3-(1-methyl-1-morpholinoethyl)-thioxanthone, 2-morpholinomethylthioxanthone, 2-methyl-6-morpholinomethylthioxanthone, and thioxanthone-2-carboxylic acid polyethylene glycol ester.
[0064] The thioxanthone compound as the component (B4) has a triplet energy sensitization effect. By combining it with an appropriate photopolymerization initiator, light on the long wavelength side can also be used to generate free radicals. Therefore, in the photosensitive resin composition, by using the component (B4) in combination with the components (B1), (B2) and (B3), the sensitivity to various exposure wavelengths can be further improved and the shape of the through hole opening can be made better.
[0065] The content of the component (B1) in the component (B) may be 30% by mass or more, 35% to 99% by mass, or 40% to 98% by mass based on the total amount of the components (B1), (B2), and (B3). If the content of the component (B1) is within the above range, there is a tendency to further improve the sensitivity.
[0066] The content of the component (B2) in the component (B) may be 0.5 to 30% by mass, 1.0 to 25% by mass, or 1.5 to 20% by mass based on the total amount of the components (B1), (B2) and (B3). If the content of the component (B2) is within the above range, there is a tendency to further improve the sensitivity to various exposure wavelengths and to make the shape of the through-hole opening more favorable.
[0067] The content of the component (B3) in the component (B) may be 0.2 to 50% by mass, 0.4 to 45% by mass, or 0.6 to 40% by mass based on the total amount of the components (B1), (B2) and (B3). If the content of the component (B3) is within the above range, there is a tendency to further improve the sensitivity to various exposure wavelengths and to make the shape of the through-hole opening more favorable.
[0068] The content of the component (B4) in the component (B) may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 3 parts by mass or more, or 5 parts by mass or less, 40 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, or 10 parts by mass or less, relative to 100 parts by mass of the total amount of the components (B1), (B2) and (B3). If the content of the component (B4) is 0.1 parts by mass or more, there is a tendency to further improve the sensitivity to various exposure wavelengths and to make the shape of the through-hole opening better. If the content of the component (B4) is 50 parts by mass or less, there is a tendency to further improve the sensitivity to various exposure wavelengths. From these viewpoints, the content of the component (B4) in the component (B) can be 0.1 to 50 parts by mass, 0.5 to 40 parts by mass, 1 to 30 parts by mass, 3 to 20 parts by mass, or 5 to 10 parts by mass relative to 100 parts by mass of the total amount of the components (B1), (B2) and (B3).
[0069] The content of the component (B2) in the component (B) may be 0.5 to 60 parts by mass, 1.0 to 55 parts by mass, or 1.5 to 50 parts by mass relative to 100 parts by mass of the component (B1). If the content of the component (B2) is 0.5 parts by mass or more, there is a tendency to further improve the sensitivity, and if the content of the component (B2) is 60 parts by mass or less, there is a tendency to improve the balance between the sensitivity and the shape of the through-hole opening.
[0070] The content of the component (B3) in the component (B) may be 0.2 to 110 parts by mass, 0.4 to 105 parts by mass, or 0.6 to 100 parts by mass relative to 100 parts by mass of the component (B1). If the content of the component (B3) is 0.2 parts by mass or more, there is a tendency to further improve the sensitivity, and if the content of the component (B3) is 110 parts by mass or less, there is a tendency to improve the balance between the sensitivity and the shape of the through-hole opening.
[0071] From the viewpoint of sensitivity, the total content of the components (B1), (B2) and (B3) in the component (B) may be 70% by mass or more, 80% by mass or more, or 90% by mass or more, or may be 100% by mass, less than 100% by mass, 99.5% by mass or less, or 99% by mass or less, based on the total amount of the component (B).
[0072] From the viewpoint of sensitivity, the total content of the components (B1), (B2), (B3) and (B4) in the component (B) may be 70% by mass or more, 80% by mass or more, or 90% by mass or more, or may be 100% by mass, based on the total amount of the component (B).
[0073] The content of the component (B) in the photosensitive resin composition is not particularly limited, and may be 0.2 to 15% by mass, 0.5 to 10% by mass, or 1 to 5% by mass based on the total solid content of the photosensitive resin composition.
[0074] (Component (C): photopolymerizable compound)
[0075] From the viewpoint of improving chemical resistance after exposure and increasing the difference in developer resistance between the exposed portion and the unexposed portion, the photosensitive resin composition of the present embodiment contains a photopolymerizable compound as component (C). Component (C) is not particularly limited as long as it is a photopolymerizable compound having an ethylenically unsaturated group and not having an acidic group.
[0076] Examples of the component (C) include a photopolymerizable compound having one ethylenically unsaturated group, a photopolymerizable compound having two ethylenically unsaturated groups, and a photopolymerizable compound having three or more ethylenically unsaturated groups.
[0077] Examples of the photopolymerizable compound having one ethylenically unsaturated group include (meth)acrylic acid and alkyl (meth)acrylates. Examples of the alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hydroxyethyl (meth)acrylate.
[0078] Examples of the photopolymerizable compound having two ethylenically unsaturated groups include polyethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2-bis(4-(meth)acryloyloxypolyethoxypolypropoxyphenyl)propane, and bisphenol A diglycidyl ether di(meth)acrylate.
[0079] Examples of the photopolymerizable compound having three or more ethylenically unsaturated groups include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from ditrimethylolpropane, such as ditrimethylolpropane tetra(meth)acrylate; and (meth)acrylate compounds having a skeleton derived from diglycerol.
[0080] Among these, from the viewpoint of improving chemical resistance after exposure and increasing the difference in developer resistance between the exposed portion and the unexposed portion, a (meth)acrylate compound having a skeleton derived from dipentaerythritol is preferred, and dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate are more preferred.
[0081] When the photosensitive resin composition of the present embodiment contains the component (C), the content thereof may be 1 to 20% by mass, 2 to 15% by mass, or 4 to 12% by mass based on the total solid content of the photosensitive resin composition.
[0082] (Component (D): polymerization inhibitor)
[0083] The photosensitive resin composition of the present embodiment contains a polymerization inhibitor as the component (D). The photosensitive resin composition of the present embodiment can suppress the curing of the upper part of the through-hole and can cure to the lower part of the through-hole when forming the through-hole, thereby forming a through-hole opening with a good shape without undercutting.
[0084] Examples of the component (D) include 4-tert-butylcatechol, 4-hydroxy-2,2,6,6-tetramethylpiperidinyl-N-oxyl, 4,4'-butylene-bis(6-tert-butyl-m-cresol), hydroquinone, methyl hydroquinone, and hydroquinone monomethyl ether, etc. These may be used alone or in combination of two or more.
[0085] From the viewpoint of improving the sensitivity, resolution and shape of the through-hole opening, the content of component (D) can be 0.01 mass part or more, 0.02 mass part or more, 0.05 mass part or more, or 0.10 mass part or more relative to 100 mass parts of the total amount of components (A) and (B), and from the viewpoint of sensitivity and adhesion, it can be 0.50 mass part or less, 0.40 mass part or less, or 0.30 mass part or less.
[0086] ((E) ingredient: sensitizer)
[0087] The photosensitive resin composition of the present embodiment may further contain a sensitizer as the component (E). When the photosensitive resin composition contains the component (E), the absorption wavelength of the active light used for exposure can be effectively utilized.
[0088] Examples of the component (E) include pyrazoline compounds, anthracene compounds, coumarin compounds, oxazole compounds, benzoxazole compounds, thiazole compounds, benzothiazole compounds, triazole compounds, stilbene compounds, triazine compounds, thiophene compounds, naphthalimide compounds, triarylamine compounds, and aminoacridine compounds.
[0089] Examples of the pyrazoline compound include 1-phenyl-3-(4-methoxyphenylvinyl)-5-(4-methoxyphenyl)pyrazoline, 1-phenyl-3-(4-tert-butylphenylvinyl)-5-(4-tert-butylphenyl)pyrazoline, and 1-phenyl-3-biphenyl-5-(4-tert-butylphenyl)pyrazoline.
[0090] Examples of the anthracene compound include 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, 9,10-dipropoxyanthracene, 9,10-dibutoxyanthracene, and 9,10-dipentyloxyanthracene.
[0091] Examples of the coumarin compound include 3-benzoyl-7-diethylaminocoumarin, 7-diethylamino-4-methylcoumarin, 3,3′-carbonylbis(7-diethylaminocoumarin) and 2,3,6,7-tetrahydro-9-methyl-1H,5H,11H-[1]benzopyrano[6,7,8-ij]quinolizin-11-one.
[0092] From the viewpoint of further improving sensitivity, adhesion and resolution, the content of component (E) may be 0.01 to 1.5 parts by mass, 0.02 to 1.2 parts by mass, or 0.03 to 1.0 parts by mass based on 100 parts by mass of the total amount of components (A) and (B).
[0093] ((F) ingredient: pigment)
[0094] From the viewpoint of improving the recognition or appearance of the manufacturing device, the photosensitive resin composition of the present embodiment may further contain a pigment as the (F) component. As the (F) component, a colorant that develops a desired color when hiding a circuit, etc. can be used. As the (F) component, for example, phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, carbon black, and naphthalene black can be cited.
[0095] From the viewpoint of further concealing the circuit, the content of the component (F) may be 0.05 to 10% by mass, 0.1 to 8% by mass, or 0.2 to 5% by mass based on the total solid content in the photosensitive resin composition.
[0096] ((G) ingredient: inorganic filler)
[0097] The photosensitive resin composition according to the present embodiment may further contain an inorganic filler as the component (G). By containing the component (G), the adhesive strength and reliability of the permanent resist can be improved. The component (G) may be used alone or in combination of two or more.
[0098] As inorganic fillers, for example, silica, aluminum oxide, titanium dioxide, tantalum oxide, zirconium oxide, silicon nitride, barium titanate, barium carbonate, magnesium carbonate, aluminum hydroxide, magnesium hydroxide, lead titanate, lead zirconate titanate, lead lanthanum zirconate titanate, gallium oxide, spinel, mullite, cordierite, talc, aluminum titanate, zirconium oxide containing yttrium oxide, barium silicate, boron nitride, calcium carbonate, barium sulfate, calcium sulfate, zinc oxide, magnesium titanate, hydrotalcite, mica, calcined kaolin, and carbon.
[0099] From the viewpoint of improving the heat resistance of the permanent resist, the component (G) may contain silicon dioxide, and from the viewpoint of improving the heat resistance and adhesive strength of the permanent resist, it may contain barium sulfate. From the viewpoint of improving the dispersibility of the inorganic filler, an inorganic filler that has been surface-treated with alumina or an organosilane compound in advance may also be used.
[0100] The average particle size of the inorganic filler may be 0.01 μm or more, 0.1 μm or more, 0.2 μm or more, or 0.3 μm or more, or 5.0 μm or less, 3.0 μm or less, 2.0 μm or less, or 1.5 μm or less.
[0101] The content of the component (G) may be 5 to 70 mass%, 6 to 60 mass%, 10 to 50 mass%, 20 to 50 mass%, or 30 to 50 mass%, based on the total solid content of the photosensitive resin composition. If the content of the component (G) is within the above range, the low thermal expansion coefficient, heat resistance, film strength, etc. can be further improved. In addition, the more the content of the component (G) is (that is, the content of the component (G) is above the above lower limit), the easier it is for the taper angle of the through hole to become larger, and there is a tendency to form a through hole opening with a better shape.
[0102] ((H) component: thermosetting resin)
[0103] The photosensitive resin composition of the present embodiment may further contain a thermosetting resin as component (H). By using component (H), the heat resistance, adhesion, chemical resistance, etc. of the cured film (permanent resist) formed by the photosensitive resin composition can be improved. Component (H) may be used alone or in combination of two or more.
[0104] Examples of the component (H) include epoxy resins, phenol resins, unsaturated imide resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins.
[0105] Examples of the epoxy resin include bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol S type epoxy resin, novolac type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, hydantoin type epoxy resin, triglycidyl isocyanurate and bixylenol type epoxy resin.
[0106] The content of the component (H) may be 2 to 30 mass %, 5 to 25 mass %, or 8 to 20 mass % based on the total solid content of the photosensitive resin composition. If the content of the component (H) is within the above range, the heat resistance of the formed cured film can be further improved while maintaining good developability.
[0107] ((I) component: elastomer)
[0108] The photosensitive resin composition according to the present embodiment may further contain an elastomer as the component (I). By containing the component (I), a decrease in flexibility and adhesive strength due to deformation (internal stress) inside the resin caused by curing shrinkage of the component (A) can be suppressed.
[0109] As component (I), for example, styrene elastomers, olefin elastomers, urethane elastomers, polyester elastomers, polyamide elastomers, acrylic elastomers, and silicone elastomers can be cited. These elastomers are composed of a hard segment component that contributes to heat resistance and strength and a soft segment component that contributes to flexibility and toughness.
[0110] Examples of the styrene-based elastomer include styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-ethylene-butylene-styrene block copolymers, and styrene-ethylene-propylene-styrene block copolymers. As components constituting the styrene-based elastomer, in addition to styrene, styrene derivatives such as α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene can be used.
[0111] Examples of the olefin elastomer include ethylene-propylene copolymers, ethylene-α-olefin copolymers, ethylene-α-olefin-non-conjugated diene copolymers, propylene-α-olefin copolymers, butene-α-olefin copolymers, ethylene-propylene-diene copolymers, copolymers of non-conjugated dienes such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylene norbornene, ethylidene norbornene, butadiene, and isoprene with α-olefins, and carboxylic acid-modified butadiene-acrylonitrile copolymers.
[0112] As the urethane elastomer, a compound composed of a hard segment formed of a low molecular weight (short chain) diol and a diisocyanate and a soft segment formed of a high molecular weight (long chain) diol and a diisocyanate can be used.
[0113] Examples of the short-chain diol include ethylene glycol, propylene glycol, 1,4-butanediol, and bisphenol A. The number average molecular weight of the short-chain diol is preferably 48 to 500.
[0114] Examples of the long-chain diol include polypropylene glycol, polytetramethylene oxide, poly(1,4-butylene adipate), poly(ethylene-1,4-butylene adipate), polycaprolactone, poly(1,6-hexylene carbonate), and poly(1,6-hexylene-neopentylene adipate). The number average molecular weight of the long-chain diol is preferably 500 to 10,000.
[0115] As the polyester-based elastomer, a compound obtained by polycondensing a dicarboxylic acid or a derivative thereof and a diol compound or a derivative thereof can be used.
[0116] Examples of the dicarboxylic acid include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalene dicarboxylic acid; aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid; and alicyclic dicarboxylic acids such as cyclohexane dicarboxylic acid. The dicarboxylic acid may be used alone or in combination of two or more.
[0117] Examples of the diol compound include aliphatic diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,10-decanediol; alicyclic diols such as 1,4-cyclohexanediol; and aromatic diols such as bisphenol A, bis-(4-hydroxyphenyl)methane, bis-(4-hydroxy-3-methylphenyl)propane, and resorcinol.
[0118] As the polyester elastomer, a multi-block copolymer having an aromatic polyester (e.g., polybutylene terephthalate) as a hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) as a soft segment component can be used. There are different grades of polyester elastomers depending on the type, ratio, and molecular weight of the hard segment and the soft segment.
[0119] Polyamide elastomers are roughly divided into two types: polyether block amide type and polyether ester block amide type, which use polyamide in the hard segment and polyether or polyester in the soft segment. Examples of polyamide include polyamide-6, polyamide-11, and polyamide-12. Examples of polyether include polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene glycol.
[0120] Acrylic elastomers can use compounds containing structural units based on (meth)acrylate as a main component. Examples of (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, methoxyethyl (meth)acrylate, and ethoxyethyl (meth)acrylate. Acrylic elastomers can be compounds obtained by copolymerizing (meth)acrylate and acrylonitrile, or compounds obtained by further copolymerizing a monomer having a functional group that serves as a crosslinking point. Examples of monomers having a functional group include glycidyl methacrylate and allyl glycidyl ether.
[0121] Examples of the acrylic elastomer include acrylonitrile-butyl acrylate copolymer, acrylonitrile-butyl acrylate-ethyl acrylate copolymer, methyl methacrylate-butyl acrylate-methacrylic acid copolymer, and acrylonitrile-butyl acrylate-glycidyl methacrylate copolymer. The acrylic elastomer is preferably acrylonitrile-butyl acrylate-glycidyl methacrylate copolymer or a methyl methacrylate-butyl acrylate-methacrylic acid copolymer, and more preferably a methyl methacrylate-butyl acrylate-methacrylic acid copolymer.
[0122] Silicone elastomers are compounds with organopolysiloxane as the main component. Examples of organopolysiloxanes include polydimethylsiloxane, polymethylphenylsiloxane, and polydiphenylsiloxane. Silicone elastomers may also be compounds obtained by modifying a portion of organopolysiloxane with vinyl, alkoxy, or the like.
[0123] From the viewpoint of improving the adhesiveness of the cured film, the component (I) may contain a carboxylic acid-modified butadiene-acrylonitrile copolymer or a polyester-based elastomer having a hydroxyl group.
[0124] The content of the component (I) may be 2 to 50 parts by mass, 4 to 45 parts by mass, 6 to 40 parts by mass, or 10 to 35 parts by mass relative to 100 parts by mass of the component (A). When the content of the component (I) is within the above range, the elastic modulus of the cured film in the high temperature region is lowered, and the unexposed portion is more easily dissolved in the developer.
[0125] (Other ingredients)
[0126] The photosensitive resin composition of the present embodiment may further contain various additives as required. Examples of additives include thickeners such as bentonite and montmorillonite; silicone, fluorine, and vinyl resin defoamers; silane coupling agents; and flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, phosphate compounds, aromatic condensed phosphate esters, and halogen-containing condensed phosphate esters.
[0127] (Solvent)
[0128] The photosensitive resin composition according to the present embodiment contains a solvent for dissolving and dispersing each component, and thus can be easily applied onto a substrate to form a coating film having a uniform thickness.
[0129] Examples of the solvent include ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether; esters such as ethyl acetate, butyl acetate, butyl cellulosic acetate, and carbitol acetate; aliphatic hydrocarbons such as octane and decane; and petroleum-based solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent petroleum naphtha. The solvent may be used alone or in combination of two or more.
[0130] The amount of the solvent added is not particularly limited, and the ratio of the solvent in the photosensitive resin composition may be 10 to 60% by mass, 20 to 50% by mass, or 25 to 40% by mass.
[0131] The photosensitive resin composition of the present embodiment can be prepared by uniformly mixing the above-mentioned components using a roll mill, a bead mill, or the like.
[0132] [Photosensitive element]
[0133] The photosensitive element of the present embodiment includes a support film and a photosensitive layer formed of the above-mentioned photosensitive resin composition. Figure 1 Schematic diagram of a cross-sectional view of a photosensitive element according to this embodiment. Figure 1 As shown, the photosensitive element 1 includes a support film 10 and a photosensitive layer 20 formed on the support film 10 .
[0134] The photosensitive element 1 can be produced by coating the photosensitive resin composition according to the present embodiment on a support film 10 by a known method such as reverse roll coating, gravure roll coating, comma coating, curtain coating, and then drying the coating to form the photosensitive layer 20 .
[0135] As the support film, for example, polyester films such as polyethylene terephthalate and polybutylene terephthalate, polyolefin films such as polypropylene and polyethylene can be cited. The thickness of the support film can also be, for example, 5 to 100 μm. The thickness of the photosensitive layer can also be, for example, 5 to 50 μm, 5 to 40 μm, or 10 to 30 μm. The surface roughness of the support film is not particularly limited, but the arithmetic mean roughness (Ra) can also be less than 1000 nm, less than 500 nm, or less than 250 nm.
[0136] The coating film may be dried by hot air drying, drying using far infrared rays or near infrared rays. The drying temperature may be 60 to 120° C., 70 to 110° C., or 80 to 100° C. The drying time may be 1 to 60 minutes, 2 to 30 minutes, or 5 to 20 minutes.
[0137] The photosensitive layer 20 may further include a protective film 30 covering the photosensitive layer 20. The photosensitive element 1 may also have a protective film 30 laminated on the surface opposite to the surface in contact with the support film 10 of the photosensitive layer 20. As the protective film 30, for example, a polymer film such as polyethylene or polypropylene may be used.
[0138] [Printed circuit board]
[0139] The printed wiring board according to the present embodiment includes a permanent resist containing a cured product of the photosensitive resin composition according to the present embodiment.
[0140] The method for manufacturing a printed wiring board according to the present embodiment includes: forming a photosensitive layer on a substrate using the photosensitive resin composition or the photosensitive element, exposing and developing the photosensitive layer to form a resist pattern, and curing the resist pattern to form a permanent resist. An example of each step is described below.
[0141] First, a substrate such as a copper-clad laminate is prepared, and a photosensitive layer is formed on the substrate. The photosensitive layer can also be formed by coating a photosensitive resin composition on the substrate and drying it. As a method for coating the photosensitive resin composition, for example, screen printing, spraying, roller coating, curtain coating, and electrostatic coating can be cited. The drying temperature can be 60 to 120° C., 70 to 110° C., or 80 to 100° C. The drying time can also be 1 to 7 minutes, 1 to 6 minutes, or 2 to 5 minutes.
[0142] The photosensitive layer can also be formed by peeling the protective film from the photosensitive element on the substrate and laminating the photosensitive layer. As a method for laminating the photosensitive layer, for example, a method of heat lamination using a laminator can be mentioned.
[0143] Next, the negative film is brought into direct contact with the photosensitive layer or through a support film, and exposed to active light. Examples of active light include electron beams, ultraviolet rays, and X-rays, preferably ultraviolet rays. The exposure dose may also be 10 to 2000 mJ / cm 2 100~1500mJ / cm 2 , or 300~1000mJ / cm 2 .
[0144] As the light source of active light, as long as it is a commonly used known light source, there is no particular limitation, for example, a carbon arc lamp, a mercury vapor arc lamp, an ultra-high pressure mercury lamp, a high pressure mercury lamp, a xenon lamp, a gas laser such as an argon laser, a solid laser such as a YAG laser, a semiconductor laser such as a gallium nitride blue-violet laser, etc. can be used. Light sources that effectively emit ultraviolet light. Among these, from the viewpoint of improving resolution and alignment with good balance, a light source capable of emitting i-ray monochromatic light with an exposure wavelength of 365nm, a light source capable of emitting h-ray monochromatic light with an exposure wavelength of 405nm, or a light source capable of emitting active light with an exposure wavelength of ih mixed rays can also be used, preferably a light source capable of emitting i-ray monochromatic light with an exposure wavelength of 365nm or h-ray monochromatic light with an exposure wavelength of 405nm. As a light source capable of emitting i-ray monochromatic light with an exposure wavelength of 365nm, for example, an ultra-high pressure mercury lamp can be cited. As a light source capable of emitting h-ray monochromatic light with an exposure wavelength of 405nm, for example, a blue-violet laser diode with a wavelength of 405nm can be cited. Since the photosensitive layer is formed using the photosensitive resin composition according to the present embodiment, a through hole opening having a good shape can be formed even at any of the above-mentioned exposure wavelengths.
[0145] After exposure, the unexposed portion is removed by using a developer to form a resist pattern. As a developing method, for example, an immersion method and a spray method can be cited. As a developer, for example, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, and tetramethylammonium hydroxide can be used.
[0146] By performing at least one of post-exposure and post-heating on the resist pattern, a pattern cured film (permanent resist) can be formed. The exposure dose of the post-exposure may be 100 to 5000 mJ / cm 2 , 500~2000mJ / cm 2 , or 700~1500J / cm 2 The heating temperature of the post-heating may be 100 to 200° C., 120 to 180° C., or 135 to 165° C. The heating time of the post-heating may be 5 minutes to 12 hours, 10 minutes to 6 hours, or 30 minutes to 2 hours.
[0147] The permanent resist involved in this embodiment can be used as an interlayer insulating layer or surface protective layer of a semiconductor element. A semiconductor element or an electronic device including the semiconductor element can be produced, and the semiconductor element has an interlayer insulating layer or a surface protective layer formed by a cured film of the above-mentioned photosensitive resin composition. The semiconductor element can be, for example, a memory, a package, etc. having a multi-layer circuit structure, a re-circuit structure, etc. As an electronic device, for example, a mobile phone, a smart phone, a touch-type terminal, a personal computer, and a hard disk suspension can be cited. By having a patterned cured film formed by the photosensitive resin composition involved in this embodiment, a semiconductor element and an electronic device with excellent reliability can be provided.
[0148] Example
[0149] Hereinafter, the present invention will be described in further detail with reference to Examples, but the present invention is not limited to these Examples.
[0150] <(A) Synthesis of acid-modified vinyl-containing resin>
[0151] (Synthesis example 1)
[0152] 350 parts by mass of dicyclopentadiene epoxy resin (manufactured by Nippon Kayaku Co., Ltd., product name "XD-1000", epoxy equivalent: 252 g / eq, softening point: 74.2°C, number of ring-forming carbon atoms of alicyclic skeleton: 10), 70 parts by mass of acrylic acid, 0.5 parts by mass of methylhydroquinone, and 120 parts by mass of carbitol acetate were added, and the mixture was heated to 90°C and stirred to react and dissolve the mixture. Next, the obtained solution was cooled to 60°C, and 2 parts by mass of triphenylphosphine was added, and the mixture was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. 98 parts by mass of tetrahydrophthalic anhydride and 85 parts by mass of carbitol acetate were added to the solution after the reaction, and the mixture was heated to 80°C and reacted for 6 hours. Thereafter, the solution was cooled to room temperature to obtain a solution of an acid-modified dicyclopentadiene epoxy acrylate (A-1) having a solid content concentration of 73% by mass.
[0153] (Synthesis example 2)
[0154] 350 parts by mass of a dicyclopentadiene epoxy resin (manufactured by DIC Corporation, product name "EPICLON (registered trademark) HP-7200", epoxy equivalent: 254-264 g / eq, softening point: 56-66°C, number of ring-forming carbon atoms of alicyclic skeleton: 10), 70 parts by mass of acrylic acid, 0.5 parts by mass of methylhydroquinone, and 120 parts by mass of carbitol acetate were added, and the mixture was heated to 90°C and stirred to react and dissolve the mixture. Next, the obtained solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the mixture was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. 98 parts by mass of tetrahydrophthalic anhydride and 85 parts by mass of carbitol acetate were added to the solution after the reaction, and the mixture was heated to 80°C and reacted for 6 hours. Thereafter, the solution was cooled to room temperature to obtain a solution of an acid-modified dicyclopentadiene epoxy acrylate (A-2) having a solid content concentration of 74% by mass.
[0155] (Synthesis example 3)
[0156] 350 parts by mass of bisphenol F novolac epoxy resin (manufactured by DIC Corporation, product name "EXA-7376"), 70 parts by mass of acrylic acid, 0.5 parts by mass of methyl hydroquinone, and 120 parts by mass of carbitol acetate were added, and heated to 90°C and stirred, thereby reacting to dissolve the mixture. Next, the obtained solution was cooled to 60°C, and 2 parts by mass of triphenylphosphine was added, and heated to 100°C, and reacted until the acid value of the solution reached 1 mgKOH / g. In the reacted solution, 98 parts by mass of tetrahydrophthalic anhydride and 85 parts by mass of carbitol acetate were added, and heated to 80°C, and reacted for 6 hours. Thereafter, the solution was cooled to room temperature, thereby obtaining a solution of acid-modified bisphenol F epoxy acrylate (A-3) having a solid content concentration of 73% by mass.
[0157] <Preparation of ingredients (B) to (H)>
[0158] The following materials were prepared as components (B) to (H).
[0159] (B) Photopolymerization initiator
[0160] (B1) Alkylphenone-based photopolymerization initiator
[0161] B1-1: 2-Benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (manufactured by IGM Resins BV, product name "Omnirad 369")
[0162] B1-2: 2-Hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone (manufactured by IGM Resins BV, product name "Omnirad 2959")
[0163] B1-3: 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone (manufactured by IGM Resins BV, product name "Omnirad 907")
[0164] (B2) Oxime ester photopolymerization initiator
[0165] B2-1: Ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyl oxime) (manufactured by BASF, product name "Irgacure OXE02")
[0166] B2-2: 1-[4-(Phenylthio)phenyl]octane-1,2-dione=2-(O-benzoyl oxime) (manufactured by BASF, product name "Irgacure OXE01")
[0167] (B3) Benzophenone-based photopolymerization initiator
[0168] B3-1: 4,4'-bis(diethylamino)benzophenone (manufactured by Tokyo Aniline Dye Manufacturing Co., Ltd., product name "EAB")
[0169] (B4) Other photopolymerization initiators
[0170] B4-1: 2,4-diethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., trade name "DETX-S")
[0171] (C) Photopolymerizable compound
[0172] C-1: Dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku CO., Ltd., product name "DPHA")
[0173] (D) Polymerization inhibitor
[0174] D-1: 4,4'-butylene-bis(6-tert-butyl-m-cresol) (manufactured by Kawaguchi Chemical Industry Company, Limited, product name "ANTAGE W-300")
[0175] (F) Pigment
[0176] F-1: Phthalocyanine pigment (manufactured by Sanyo Color Works, Ltd.)
[0177] (G) Inorganic filler
[0178] G-1: Silica particles (manufactured by Denka Company Limited, product name "SFP-20M", average particle size: 0.3 μm)
[0179] (H) Thermosetting resin
[0180] H-1: biphenyl type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name "YX4000")
[0181] [Examples 1 to 19 and Comparative Examples 1 to 6]
[0182] <Preparation of photosensitive resin composition>
[0183] The components were prepared according to the formulation compositions shown in Tables 1 to 3 (the units of the values in the tables are parts by mass, and in the case of solutions, the amounts are calculated based on the solid content) and kneaded using a three-roll mill. Methyl ethyl ketone was then added so that the solid content concentration became 60% by mass, thereby obtaining a photosensitive resin composition.
[0184] <Production of photosensitive elements>
[0185] As a support film, a polyethylene terephthalate film (manufactured by TEIJIN LIMITED, product name "G2-16") with a thickness of 16 μm was prepared. The photosensitive resin composition was applied to the support film so that the thickness after drying was 20 μm, and dried at 75° C. for 30 minutes using a hot air convection dryer to form a photosensitive layer. Next, a polyethylene film (manufactured by TAMAPOLY CO., Ltd., product name "NF-15") was attached to the surface of the photosensitive layer on the opposite side of the side in contact with the support film as a protective film to obtain a photosensitive element.
[0186] [1. Evaluation of through-hole resolution (i-ray)]
[0187] (1-1) Preparation of evaluation laminate
[0188] The copper foil surface of a printed circuit board substrate (MCL-E-679, manufactured by Resonac Corporation.) in which a 12 μm thick copper foil was laminated on a glass epoxy substrate was treated with a roughening treatment liquid (manufactured by MEC COMPANY Ltd., product name "CZ-8100"), and then washed and dried to obtain a roughened printed circuit board substrate. Next, the protective film was peeled off from the photosensitive element prepared in each embodiment and comparative example, and the exposed photosensitive layer was placed in contact with the copper foil of the roughened printed circuit board substrate, and then laminated using a pressure vacuum laminator (manufactured by MEIKI CO., Ltd., product name "MVLP-500"). In addition, the lamination conditions were set to a hot plate temperature of 70°C, an evacuation time of 20 seconds, a lamination pressing time of 30 seconds, an air pressure of 4 kPa or less, and a crimping pressure of 0.4 MPa. After the lamination treatment, the laminate was left to stand at room temperature for 1 hour or more, thereby obtaining a laminate for evaluation in which a photosensitive layer and a support film were laminated in this order on the copper foil surface of the printed wiring board substrate.
[0189] (1-2) Sensitivity measurement of photosensitive layer
[0190] After peeling off the support film of the evaluation laminate obtained in (1-1), a 41-stage ladder plate (manufactured by Resonac Corporation) was placed and exposed using an i-ray exposure device (manufactured by Ushio Co., Ltd., product name "UX-2240SM-XJ-01"). The exposure pattern used was a pattern including After exposure, the photosensitive resin composition in the unexposed part was spray-developed for 60 seconds using a 1% by mass sodium carbonate aqueous solution at 30°C. 2 The exposure energy is set to 25 mJ / cm 2 The above test was repeated once, and the exposure energy at which the number of residual steps of the 41-step ladder plate after development became 10.0 was set as the sensitivity of the photosensitive layer (unit: mJ / cm 2 ). The pattern exposed at this sensitivity was used and the resolution of the through-holes provided in the photosensitive layer was evaluated by the following method. In addition, the sensitivity was evaluated according to the following criteria.
[0191] <Evaluation Criteria>
[0192] A: Sensitivity is 150mJ / cm 2 the following.
[0193] B: Sensitivity is more than 150mJ / cm2 And 200mJ / cm 2 the following.
[0194] C: Sensitivity is more than 200mJ / cm 2 And 300mJ / cm 2 the following.
[0195] D: Sensitivity exceeds 300mJ / cm 2 .
[0196] (1-3) Evaluation of through-hole resolution
[0197] Regarding the evaluation of the resolution of the through-holes, the photosensitive layer was exposed to an exposure energy at which the residual order became 10.0, which was the sensitivity of the photosensitive layer measured in (1-2) above, and then spray-developed. The through-hole pattern of the obtained cured film (permanent resist) was observed using an optical microscope and evaluated according to the following criteria. Here, the through-hole is in an "open" state, which means that when the through-hole opening is observed from directly above using an optical microscope, the state of the copper foil of the substrate for the printed wiring board can be visually identified. And, as Figure 2 As shown in FIG. 1 , the “cone angle” refers to the angle θ formed between the permanent resist 60 and the printed wiring board substrate 50 when the cross section of the through hole opening 70 of the permanent resist 60 formed on the printed wiring board substrate 50 is observed using an optical microscope. It can be said that the closer the cone angle θ is to 90 degrees, the better the shape of the through hole opening. In the case where the evaluation result is A evaluation or B evaluation, it is judged that a through hole opening with a good shape can be formed. In addition, in the case of the sensitivity evaluation of D, the resolution of the through hole is not evaluated.
[0198] <Evaluation Criteria>
[0199] A: The through hole opening has a taper angle of more than 80 degrees and less than 90 degrees.
[0200] B: The through hole opening has a taper angle of more than 70 degrees and less than 80 degrees.
[0201] C: The through hole opening has a taper angle of more than 60 degrees and less than 70 degrees.
[0202] D: Through hole opening, taper angle is less than 60 degrees.
[0203] E: The through hole is not opened.
[0204] [2. Evaluation of through-hole resolution (mixed rays)]
[0205] (2-1) Preparation of evaluation laminate
[0206] A laminate for evaluation was prepared in the same manner as in the above (1-1).
[0207] (2-2) Sensitivity measurement of photosensitive layer
[0208] After peeling off the support film of the evaluation laminate obtained in (2-1) above, a 41-stage ladder plate (manufactured by Resonac Corporation.) was arranged and exposed using a direct imaging exposure device (manufactured by ORCMANUFACTURING CO., Ltd., product name "EDi-5308", 355-420 filter, mixed rays of i-rays and h-rays) using an ultra-high pressure mercury lamp as a light source. The exposure pattern used a pattern in which dots were arranged in a grid (dot diameter: distance between the centers of dots = 1:2). The diameter of the dot After exposure, the photosensitive resin composition was left at room temperature for 30 minutes, and then spray-developed for 60 seconds using a 1 mass % sodium carbonate aqueous solution at 30°C. 2 The exposure energy is set to 10 mJ / cm 2 The above test was repeated once, and the exposure energy at which the number of residual steps of the 41-step ladder plate after development became 10.0 was set as the sensitivity of the photosensitive layer (unit: mJ / cm 2 ). The pattern exposed at this sensitivity was used and the resolution of the through-holes provided in the photosensitive layer was evaluated by the following method. In addition, the sensitivity was evaluated according to the following criteria.
[0209] <Evaluation Criteria>
[0210] A: Sensitivity is 80mJ / cm 2 the following.
[0211] B: Sensitivity is more than 80mJ / cm 2 And 100mJ / cm 2 the following.
[0212] C: Sensitivity is more than 100mJ / cm 2 and 150mJ / cm 2 the following.
[0213] D: Sensitivity exceeds 150mJ / cm 2 .
[0214] (2-3) Evaluation of through-hole resolution
[0215] The resolution of the through hole was evaluated in the same manner as in (1-3) above. The evaluation criteria are as follows. When the evaluation result is A or B, it is judged that a through hole opening with a good shape can be formed. In addition, when the sensitivity is D, the resolution of the through hole is not evaluated.
[0216] <Evaluation Criteria>
[0217] A: The through hole opening has a taper angle of more than 80 degrees and less than 90 degrees.
[0218] B: The through hole opening has a taper angle of more than 70 degrees and less than 80 degrees.
[0219] C: The through hole opening has a taper angle of more than 60 degrees and less than 70 degrees.
[0220] D: Through hole opening, taper angle is less than 60 degrees.
[0221] E: The through hole is not opened.
[0222] [Table 1]
[0223]
[0224] [Table 2]
[0225]
[0226] [Table 3]
[0227]
[0228] Explanation of symbols
[0229] 1- photosensitive element, 10- supporting film, 20- photosensitive layer, 30- protective film, 50- printed wiring board substrate, 60- permanent resist, 70- through hole opening.
Claims
1. A photosensitive resin composition comprising (A) an acid-modified vinyl-containing resin, (B) a photopolymerization initiator, (C) a photopolymerizable compound, and (D) a polymerization inhibitor, The (B) photopolymerization initiator includes (B1) an alkylphenone-based photopolymerization initiator, (B2) an oxime ester-based photopolymerization initiator, and (B3) a benzophenone-based photopolymerization initiator.
2. The photosensitive resin composition according to claim 1, wherein The content of the (B1) alkylphenone-based photopolymerization initiator is 30% by mass or more based on the total amount of the (B1) alkylphenone-based photopolymerization initiator, the (B2) oxime ester-based photopolymerization initiator, and the (B3) benzophenone-based photopolymerization initiator.
3. The photosensitive resin composition according to claim 1, wherein The content of the (B2) oxime ester photopolymerization initiator is 0.5 to 30% by mass based on the total amount of the (B1) alkylphenone photopolymerization initiator, the (B2) oxime ester photopolymerization initiator, and the (B3) benzophenone photopolymerization initiator.
4. The photosensitive resin composition according to claim 1, wherein The content of the benzophenone-based photopolymerization initiator (B3) is 0.2 to 50% by mass based on the total amount of the alkylphenone-based photopolymerization initiator (B1), the oxime ester-based photopolymerization initiator (B2), and the benzophenone-based photopolymerization initiator (B3). The photosensitive resin composition according to claim 1 , further comprising (E) a sensitizer. The photosensitive resin composition according to claim 1 , further comprising (F) a pigment. 7 . The photosensitive resin composition according to claim 1 , further comprising (G) an inorganic filler.
8. The photosensitive resin composition according to claim 1, wherein The (B) photopolymerization initiator further includes (B4) a thioxanthone compound.
9. The photosensitive resin composition according to claim 8, wherein The content of the (B4) thioxanthone compound is 0.1 to 50 parts by mass based on 100 parts by mass of the total amount of the (B1) alkylphenone photopolymerization initiator, the (B2) oxime ester photopolymerization initiator, and the (B3) benzophenone photopolymerization initiator.
10. A photosensitive element comprising a support film and a photosensitive layer formed on the support film, The photosensitive layer comprises the photosensitive resin composition according to any one of claims 1 to 9. 11 . A printed wiring board comprising a permanent resist comprising a cured product of the photosensitive resin composition according to claim 1 .
12. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive resin composition according to any one of claims 1 to 9; A step of exposing and developing the photosensitive layer to form a resist pattern; and The process of curing the resist pattern to form a permanent resist.
13. A method for manufacturing a printed circuit board, comprising: A step of forming a photosensitive layer on a substrate using the photosensitive element according to claim 10; A step of exposing and developing the photosensitive layer to form a resist pattern; and The process of curing the resist pattern to form a permanent resist.