Method for manufacturing semiconductor device
By forming a low-molecular light-mobilized resin film on the semiconductor wafer, and removing the resin film by using light irradiation or an aqueous solvent, the resin film dissolution problem is solved, and the manufacturing efficiency and quality of the semiconductor chip are improved.
Patent Information
- Application Number
- CN202380036436.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-11
- Filing Date
- 2023-10-06
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art has difficulty in removing the protective film due to dissolution of the resin film during the semiconductor wafer cutting process, which affects the manufacturing efficiency and quality of the semiconductor device.
The low-molecule photomelting resin film is used to form and remove the resin film by irradiating light, and efficient removal of the resin film is achieved by using aqueous solvents or light irradiation.
The dissolution of the cooling water on the resin film is effectively suppressed, and the resin film is simply removed, thereby improving the manufacturing efficiency and quality of semiconductor chips.
Smart Images

Figure CN119096327A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art
[0002] Semiconductor devices are usually manufactured through the following steps. First, a semiconductor wafer is attached to a dicing tape and the semiconductor wafer is singulated into semiconductor chips in this state (dicing step). After that, a pickup step of picking up the semiconductor chip and a semiconductor chip bonding step of bonding the picked-up semiconductor chip and supporting components by thermal compression bonding with an adhesive (die bonding film) are performed to manufacture a semiconductor device.
[0003] In the dicing process, sometimes fine cuttings (chips) generated by cutting the semiconductor wafer adhere to the circuit formation surface of the semiconductor wafer, causing poor connection in the subsequent process. Therefore, the following process is being studied: the dicing process is performed after a resin film (protective film) is provided on the semiconductor wafer, and the resin film (protective film) is removed after dicing (for example, Patent Documents 1 and 2).
[0004] Previous technical literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2014-172932
[0007] Patent Document 2: Japanese Patent Application Publication No. 2018-129365 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] An object of the present invention is to provide a novel method for manufacturing a semiconductor device including a step of forming a resin film on a semiconductor wafer.
[0010] Means for solving technical problems
[0011] The present invention provides a method for manufacturing a semiconductor device according to [1] to [3].
[0012] [1] A method for manufacturing a semiconductor device, comprising:
[0013] A resin film forming step, forming a resin film including a resin that is reduced in molecular weight by irradiating light on a semiconductor wafer; a semiconductor chip manufacturing step with a resin film sheet, manufacturing a single-piece semiconductor chip with a resin film sheet by cutting the semiconductor wafer with the resin film formed thereon with a cutting blade; and a resin film sheet removing step, irradiating light to the resin film sheet of the semiconductor chip with the resin film sheet and removing the resin film sheet from the semiconductor chip with the resin film sheet.
[0014] [2] The method for manufacturing a semiconductor device according to [1], wherein:
[0015] The resin film sheet removal step is a step of removing the resin film sheet from the semiconductor chip with the resin film sheet using an aqueous solvent.
[0016] [3] The method for manufacturing a semiconductor device according to [1], wherein:
[0017] The resin film removal step is a step of irradiating the resin film of the semiconductor chip with the resin film with light in an aqueous solvent.
[0018] Effects of the Invention
[0019] According to the present invention, a novel method for manufacturing a semiconductor device having a step of forming a resin film on a semiconductor wafer is provided. According to the method for manufacturing a semiconductor device of the present invention, the dissolution of the resin film (protective film) caused by cooling water (cutting water) can be sufficiently suppressed, and the resin film (protective film) can be easily removed. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 1 middle, Figure 1 (a) Figure 1 (b) Figure 1 (c) and Figure 1 (d) is a diagram showing each process.
[0021] Figure 2 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 2 middle, Figure 2 (a) Figure 2 (b) Figure 2 (c) and Figure 2 (d) is a diagram showing each process.
[0022] Figure 3 These are photographic data showing the results of the optical melting test (2) of the examples. DETAILED DESCRIPTION
[0023] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In the following embodiments, the constituent elements (including steps, etc.) are not necessary except for the cases specifically indicated. The same symbols are marked on the same or equivalent parts, and repeated descriptions are omitted. In addition, regarding the positional relationship such as up, down, left, and right, unless otherwise specified, they are all based on the positional relationship shown in the accompanying drawings. The sizes of the constituent elements in each figure are conceptual, and the relative relationship between the sizes of the constituent elements is not limited to those shown in the figures.
[0024] The same is true for the numerical values and their ranges in the present invention, and the present invention is not limited thereto. In this specification, the numerical range represented by "~" represents the range containing the numerical values recorded before and after "~" as the minimum and maximum values, respectively. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. Moreover, in the numerical ranges recorded in this specification, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiments.
[0025] In this specification, the term "layer" includes not only a structure of a shape formed on the entire surface but also a structure of a shape formed on a part when viewed from a top view. In this specification, the term "process" includes not only an independent process but also a process that can achieve the desired effect of the process even if it cannot be clearly distinguished from other processes.
[0026] In the present specification, (meth)acrylate refers to acrylate or its corresponding methacrylate. The same applies to other similar expressions such as (meth)acrylic copolymers.
[0027] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.
[0028] [Method for manufacturing semiconductor device]
[0029] A method for manufacturing a semiconductor device according to one embodiment of the present invention relates to a method for manufacturing a semiconductor device including a step of forming a resin film (protective film) on a semiconductor wafer. The method for manufacturing a semiconductor device includes a resin film (protective film) forming step, a semiconductor chip manufacturing step with a resin film (protective film), and a resin film (protective film) sheet removing step. Figure 1 and Figure 2 This is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device.
[0030] <Resin film forming step>
[0031] In this process, a resin film 3 including a resin that is reduced in molecular weight by irradiation with light (hereinafter sometimes referred to as a "photofusible resin") is formed on the semiconductor wafer 1. The photofusible resin may be a resin having properties such as reduced in molecular weight by irradiation with light, reduced elastic modulus, increased loss tangent (tanδ), etc. In addition, the photofusible resin is a water-insoluble resin, and may be a gel-like or liquid-like resin that is reduced in molecular weight by irradiation with light and thus imparts water solubility. The resin film 3 can function as a protective film that prevents fine cuttings (chips) generated by cutting the semiconductor wafer from adhering to the circuit formation surface of the semiconductor wafer.
[0032] In one embodiment, the photofusible resin may be a reaction product of a compound A having a disulfide bond and having two or more thiol groups and a compound B having two or more functional groups capable of reacting with a thiol group. In addition to the photofusible resin, the resin film 3 may further include a photoradical generator. Regarding the resin film 3, for example, it can be formed by: a curing composition comprising compound A, compound B, a photoradical generator, and a curing accelerator that promotes the reaction of compound A and compound B as needed is arranged at a predetermined position, and the curing composition is cured by heating or light irradiation (compound A and compound B react). At this time, the resin film 3 may include the following cured product: a cured product of a curing composition comprising compound A, compound B, a photoradical generator, and a curing accelerator that promotes the reaction of compound A and compound B as needed. The cured product of the curing composition may include a reaction product of compound A and compound B and a photoradical generator. The curing composition may be a thermosetting composition cured by heating, or a photocurable composition cured by light irradiation, but in one embodiment, it may be a thermosetting composition.
[0033] In one embodiment, the curable composition may contain compound A, compound B, a photoradical generator, and a curing accelerator that accelerates the reaction of compound A and compound B as needed.
[0034] (Compound A)
[0035] Compound A is a compound having a disulfide bond (-SS-) and having two or more thiol groups (-SH). The upper limit of the number of thiol groups of compound A may be, for example, 10 or less, 8 or less, 6 or less, or 4 or less. Regarding component (A), for example, it may be a dithiol compound of a compound having two thiol groups (-SH). Component (A) may be a high molecular weight component of a polymer or oligomer. A compound having two thiol groups (-SH) may be considered to be a compound comprising two thiol groups and a disulfide bond, and formed by a group (the first linking group) linked to the two thiol groups.
[0036] The molecular weight or number average molecular weight of compound A may be, for example, 100 to 10,000,000, 200 to 3,000,000, 300 to 1,000,000, 400 to 10,000, or 500 to 5,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.
[0037] Compound A has one or more (two or more) disulfide bonds in the molecule. The number of disulfide bonds in Compound A may be, for example, 1 to 1000 or 4 to 50.
[0038] Compound A may be a compound (e.g., a polymer or oligomer) having a linear or branched molecular chain and an end group, and having a disulfide bond in the molecular chain. In this case, the end group in compound A may be a thiol group. By including such a compound as compound A in the curable composition, the optical meltability of the optical meltable resin (the reaction product of compound A and compound B) tends to be further improved. The molecular chain in compound A may include a disulfide bond and a polyether chain, or may be formed by a disulfide bond and a polyether chain.
[0039] Compound A may be, for example, a compound represented by formula (1): HS-(XSS) n1 -X-SH (compound (1)). In the formula, X represents a polyether chain. A plurality of Xs may be the same or different. n1 represents an integer greater than 1. For example, n1 may be 1 or more or 4 or more, and may be 1000 or less. When the component (A) is a compound represented by the formula (1), -(XSS) n1 The group represented by -X- is the first linking group. The compound for chain-extending the compound (1) may be, for example, a Michael adduct of the compound (1) or a thiocarbamate of the compound (1).
[0040] The polyether chain as X may be, for example, a polyoxyalkylene chain. The polyether chain as X may be, for example, a 1 -OX2 -OX 3 - represents a group. 1 ~X 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 2 carbon atoms (for example, methylene group, ethylene group). As for the polyether chain as X, for example, -CH2CH2-O-CH2-O-CH2CH2- and the like can be mentioned.
[0041] As commercially available products of compound A, for example, polysulfide rubber LP series (dithiol with disulfide bond, manufactured by TORAY FINE CHEMICALS CO., LTD.) etc. can be cited. Compound A can be obtained by converting the reactive functional group of a compound having a reactive functional group (e.g., carboxyl group, hydroxyl group) and a disulfide bond at the terminal into a thiol group. As compounds having a reactive functional group and a disulfide bond at the terminal, 3,3'-dithiodipropionic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), dithiodiethanol, cystamine etc. can be cited.
[0042] The content of compound A may be 15 mass % or more, 25 mass % or more, or 35 mass % or more, and may be 80 mass % or less, 70 mass % or less, or 60 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0043] (Compound B)
[0044] Compound B is a compound having two or more functional groups capable of reacting with a thiol group. As a functional group capable of reacting with a thiol group, for example, a cyclic ether group (oxirane group (oxiranyl group, epoxy group), oxetane group (oxetanyl group), tetrahydrofuranyl group, tetrahydropyranyl group, etc.); an isocyanate group; an ethylenically unsaturated group (C=C), etc. Regarding the upper limit of the number of functional groups of compound B, for example, it can be 10 or less, 8 or less, 6 or less, or 4 or less.
[0045] In one embodiment, compound B may be compound B1 having a polyether chain and having two or more cyclic ether groups. Since the curable composition includes compound B1 as compound B, the low molecular weight component generated by irradiating the photo-fusible resin with light has a large number of polyether chains or hydroxyl groups and tends to be water-soluble, and the low molecular weight component can be removed in an aqueous solvent.
[0046] From the viewpoint of reactivity and easy availability, cyclic ether group can be oxirane group. That is, compound B1 is an oxirane compound (epoxy compound) with a polyether chain and with more than 2 oxirane groups (oxiranyl, epoxy group). In addition, in this specification, in the cyclic ether group, a group with a cyclic ether structure (structure comprising a cyclic ether group) is included. For example, in the oxirane group, a group with an oxirane structure (structure comprising an oxirane group (oxiranyl, epoxy group)) such as a glycidyl group, a glycidyl ether group, an epoxycyclohexyl group is included.
[0047] The molecular weight or number average molecular weight of compound B1 may be, for example, 100 to 1,000,000, 100 to 500,000, 100 to 10,000, 150 to 5,000, or 200 to 2,000. The number average molecular weight is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.
[0048] When the cyclic ether group of compound B1 is an oxirane group (oxiranyl group, epoxy group), the epoxy equivalent of component (B) may be 50 to 2000 g / eq, 80 to 1500 g / eq, or 100 to 1000 g / eq.
[0049] Compound B1 may be a compound B1a having two cyclic ether groups, or a compound B1b having three or more cyclic ether groups. Compound B1a may be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. At this time, the end group in compound B1a may be a cyclic ether group. Compound B1a can be regarded as a compound comprising two cyclic ether groups and a polyether chain, and formed by a group (the second linking group) linked to the two cyclic ether groups. Compound B1b may be a compound having one or more cyclic ether groups as a side chain or substituent of the second linking group in compound B1a. From the viewpoint of being able to further shorten the curing time and being able to further improve the optical solubility and water solubility, compound B1 may include both compound B1a and compound B1b.
[0050] Compound B1a can be a compound (e.g., a polymer or oligomer) having a linear molecular chain and an end group, and having a polyether chain in the molecular chain. At this time, the end group in compound B1a can be a cyclic ether group. When compound B is compound B1a, it has a tendency to become easy to remove low molecular components generated by irradiating light to the photofusible resin in an aqueous solvent. The polyether chain as a molecular chain can have a hydroxyl group and a substituent such as an alkyl group that can have a hydroxyl group. The molecular chain in compound B1a can include a polyether chain or can be composed of a polyether chain.
[0051] Compound B1a may be, for example, a compound represented by the formula (2): Z-(Y) n2 -Z represents a compound (compound (2)). In the formula, Y represents a polyether chain, and Z represents a cyclic ether group. Multiple Zs may be the same or different. n2 represents an integer greater than 1. For example, n2 may be greater than 1 or greater than 2, and may be less than 1000. When compound B1a is compound (2), -(Y) n2 The group represented by - is the second linking group.
[0052] The polyether chain as Y may be, for example, a polyoxyalkylene chain. 1 -OY 2 -OY 3 -represented by a group. 1 ~Y 3 Each of them independently may be an alkylene group, or may be an alkylene group having 1 to 3 carbon atoms (for example, methylene, ethylene, propylene). As for the polyether chain as Y, for example, -CH2CH2-O-CH2-CH2-O-CH2CH2- and the like can be mentioned.
[0053] Examples of commercially available products of compound B1a include DENACOL EX series (EX-850, EX-851, EX-821, EX-830, EX-832, EX-841, EX-861, and EX-920, manufactured by Nagase ChemteX Corporation).
[0054] Compound B1b may be a compound having one or more cyclic ether groups as side chains of the second linking group (polyether chain as Y) in compound B1a.
[0055] Examples of commercially available products of compound B1b include DENACOL EX series (EX-614B, EX-313, EX-512, and EX-521, manufactured by Nagase ChemteX Corporation).
[0056] The mass ratio of the content of compound B1b to the total content of compound B1a and compound B1b (content (mass) of compound B1b / total content (mass) of compound B1a and compound B1b) may be 0.01 to 0.40. If the mass ratio is 0.01 or more, there is a tendency that the curing time of the curable composition can be further shortened, and if the mass ratio is 0.40 or less, there is a tendency that the optical melting property and water solubility can be further improved. The mass ratio may be 0.02 or more or 0.03 or more, and may be 0.35 or less, 0.30 or less, 0.25 or less, 0.20 or less, 0.15 or less, or 0.10 or less.
[0057] The content of compound B may be 10 mass % or more, 20 mass % or more, or 30 mass % or more, and 60 mass % or less, 50 mass % or less, or 40 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0058] The ratio of the total number of moles of thiol groups in compound A to the total number of moles of functional groups in compound B may be, for example, 0.90 or more or 0.95 or more and 1.10 or less or 1.05 or less.
[0059] (Photoradical Generator)
[0060] The photoradical generator is a component that generates free radicals by light irradiation. As the photoradical generator, for example, a component used as a photopolymerization initiator can be used. As the photoradical generator, there can be mentioned an intramolecular cleavage type photoradical polymerization initiator in which the substance itself is photo-cleaved by light irradiation to generate two free radicals.
[0061] Examples of the intramolecular cleavage type photoradical generator include benzyl ketal photoradical generators, α-aminoalkylphenone photoradical generators, α-hydroxyalkylphenone photoradical generators, α-hydroxyacetophenone photoradical generators, and acylphosphine oxide photoradical generators.
[0062] Examples of the benzyl ketal-based photoradical generator include 2,2-dimethoxy-1,2-diphenylethane-1-one (Omnirad 651) and the like.
[0063] Examples of α-aminoalkylphenone-based photoradical generators include 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1 (Omnirad369), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one (Omnirad907), and 2-dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholino-4-yl-phenyl)-butane-1-one (Omnirad379EG).
[0064] Examples of the α-hydroxyalkylphenone-based photoradical generator include 1-hydroxy-cyclohexyl-phenyl-ketone (Omnirad 184) and the like.
[0065] Examples of the α-hydroxyacetophenone-based photoradical generator include 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]-phenyl}-2-methyl-propane-1-one (Omnirad127) and 2-hydroxy-2-methyl-1-phenyl-propane-1-one (Omnirad1173).
[0066] Examples of the acylphosphine oxide-based photoradical generator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (Omnirad TPO H) and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Omnirad 819).
[0067] The content of the photoradical generator may be 1 mass % or more, 3 mass % or more, or 5 mass % or more, and may be 30 mass % or less, 20 mass % or less, or 15 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0068] From the viewpoint of further improving the photosensitivity, the ratio of the mole number of the photoradical generator to the mole number of the compound A (mole number of the photoradical generator / mole number of the compound A) may be 0.1 or more, 0.2 or more, or 0.3 or more.
[0069] (Curing accelerator)
[0070] The curing accelerator is a component for accelerating the reaction between compound A and compound B, and includes a component that functions as a catalyst for the curing reaction (catalyst-type curing agent). Examples of the curing accelerator include amine compounds, imidazole derivatives, quaternary ammonium salts, organic metal salts, phosphorus compounds, and the like.
[0071] Examples of the amine compound include dicyandiamide, trimethylamine, triethylamine, tripropylamine, tributylamine, tri-n-octylamine, dimethylethylamine, dimethylpropylamine, dimethylbutylamine, dimethyl-n-octylamine, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene, benzyldimethylamine, 4-methyl-N,N-dimethylbenzylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 4-dimethylaminopyridine.
[0072] Examples of the imidazole derivatives include 1-(1-cyanomethyl)-2-ethyl-4-methyl-1H-imidazole, 2-ethyl-4-methylimidazole, 2-methylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,4,5-triphenylimidazole, 1-benzyl-2-imidazole, 1,2-dimethylimidazole, and 1-benzyl-2-phenylimidazole.
[0073] Examples of the quaternary ammonium salt include tetramethylammonium chloride, tetraethylammonium chloride, tetrabutylammonium chloride, benzyltrimethylammonium chloride, benzyltriethylammonium chloride, benzyltributylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrabutylammonium bromide, benzyltrimethylammonium bromide, benzyltriethylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, tetrabutylammonium iodide, and benzyltributylammonium iodide.
[0074] Examples of the organic metal salt include organic metal salts such as bis(2,4-pentanedione)zinc(II), zinc octylate, zinc naphthenate, cobalt naphthenate, copper naphthenate, iron acetylacetonate, nickel octylate, and manganese octylate.
[0075] Examples of the phosphorus compound include sodium tetraphenylphosphonium tetra-p-tolylborate, tetraphenylphosphonium tetraphenylborate, triphenylphosphine, tri-p-tolylphosphine, tri(4-chlorophenyl)phosphine, tri(4-methoxyphenyl)phosphine, tri(2,6-dimethoxyphenyl)phosphine, triphenylphosphine triphenylborane, tetraphenylphosphonium dicyanimide, and tetraphenylphosphonium tetra(4-methylphenyl)borate.
[0076] The content of the curing accelerator may be 0.01 mass % or more, 0.1 mass % or more, or 0.5 mass % or more, and may be 10 mass % or less, 5 mass % or less, or 2 mass % or less, based on the total amount of the curable composition (solid content excluding the solvent).
[0077] The curable composition may further include compound A, compound B, a photoradical generator, and components (other components) that do not conform to the curing accelerator. As other components, for example, plasticizers, adhesiveness imparting agents such as tackifiers, antioxidants, leuco dyes, sensitizers, adhesion improvers such as coupling agents, polymerization inhibitors, light stabilizers, defoamers, fillers, chain transfer agents, thixotropy imparting agents, flame retardants, release agents, surfactants, lubricants, antistatic agents and other additives can be used for these additives. Known additives can be used. When the curable composition includes other components, the total amount of the content of the other components is based on the total amount of the curable composition, and can be 0 to 95% by mass, 0.01 to 50% by mass, or 0.1 to 10% by mass.
[0078] The curable composition can be used as a varnish of the curable composition diluted with a solvent. As the solvent, for example, aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-cymene; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amides (NMP) such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. The content of the solid content in the varnish, that is, the content other than the solvent in the varnish, can be 10 to 95% by mass, 15 to 70% by mass, or 20 to 50% by mass based on the total amount of the varnish.
[0079] The resin film forming step may include, for example, a step of preparing the semiconductor wafer 1 (see Figure 1 (a)); a step of disposing a curable composition comprising compound A, compound B, a photoradical generator and, if necessary, a curing accelerator for promoting the reaction of compound A and compound B on a semiconductor wafer 1; and a step of curing the curable composition to form a resin film 3 comprising a cured product of the curable composition (reference Figure 1 (b)) The resin film 3 may also contain a reaction product of the compound A and the compound B (photofusible resin) and a photoradical generator.
[0080] Examples of the semiconductor wafer 1 include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide. The semiconductor wafer 1 may have a circuit formation surface.
[0081] The thickness of the semiconductor wafer 1 may be, for example, 10 to 1000 μm, 20 to 900 μm, or 30 to 800 μm.
[0082] The curable composition can be prepared, for example, by a method including the step of mixing or kneading the above-mentioned components. The mixing and kneading can be performed by appropriately combining a common disperser such as a stirrer, a pestle, a three-roll mill, a ball mill, or a bead mill.
[0083] There is no particular limitation on the method of configuring the curable composition on the semiconductor wafer, but for example, there can be cited a method of applying the curable composition on the semiconductor wafer 1 using a spin coater, a rod coater, etc., a method of forming the curable composition into a film and attaching the formed curable composition film to the semiconductor wafer 1 (transfer), etc. The curable composition film can be in a semi-cured state (B stage state) before the curable composition film is bonded to the semiconductor wafer 1. Regarding the curable composition, for example, it can be configured on the circuit formation surface of the semiconductor wafer 1.
[0084] About curable composition, for example, can form the solidified material of curable composition by heating.By heating curable composition, compound A and compound B are reacted.At this time, curing accelerator can promote reaction.About the reaction product (light-melting resin) of compound A and compound B, for example, can be the compound (polymer) of the structure represented by the following formula.On the other hand, the participation of light free radical generator in the reaction is small, and the solidified material of curable composition can include the reaction product (light-melting resin) of compound A and compound B and light free radical generator.
[0085]
[0086] In the formula, X represents the first linking group, and Y represents the second linking group. m represents an integer greater than 1. For example, m may be greater than 50, greater than 100, greater than 500, or greater than 1000. * represents an atomic bonding.
[0087] The heating temperature of the curable composition may be, for example, 0 to 200° C., 30 to 150° C., or 60 to 100° C. The heating time of the curable composition may be, for example, 0.1 to 168 hours, or 72 hours or less, 48 hours or less, or 24 hours or less.
[0088] The resin film 3 may be in a (completely) cured state (C-stage state). The thickness of the resin film 3 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 200 μm.
[0089] In this manner, the resin film 3 including the photofusible resin can be formed on the semiconductor wafer 1 .
[0090] <Process for manufacturing semiconductor chips with resin films>
[0091] In this step, the semiconductor wafer 1 on which the resin film 3 is formed is diced by a dicing blade 9 to produce individual semiconductor chips 7 with resin film sheets.
[0092] The process of manufacturing a semiconductor chip with a resin film sheet may include, for example, a step of preparing a laminate 10 having a dicing tape 5, a semiconductor wafer 1, and a resin film 3 in this order (see Figure 1 and in the laminate 10, at least the semiconductor wafer 1 and the resin film 3 are cut by a dicing blade 9 to obtain a single-piece semiconductor chip 7 with a resin film (reference Figure 1 (d)).
[0093] As the dicing tape 5, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. In addition, the dicing tape can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, etching treatment, etc. as needed. The dicing tape can have adhesiveness. This dicing tape can impart adhesiveness to the above-mentioned plastic film, or it can be a dicing tape with a pressure-sensitive adhesive layer provided on one side of the above-mentioned plastic film. The pressure-sensitive adhesive layer can be formed by a UV-curable or UV-non-curable pressure-sensitive pressure-sensitive adhesive, and there is no particular limitation as long as it has sufficient adhesive force to prevent the semiconductor elements from flying apart during dicing, and a previously known pressure-sensitive adhesive layer can be used.
[0094] The thickness of the dicing tape 5 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 300 μm.
[0095] The laminated body 10 can be obtained by attaching the dicing tape 5 to the semiconductor wafer 1 on which the resin film 3 is formed.
[0096] Next, in the stacked body 10, at least the semiconductor wafer 1 and the resin film 3 (and a portion of the dicing tape 5) are cut by a dicing blade 9 and are separated into individual pieces. The dicing by the dicing blade 9 can be performed using a commercially available device. The dicing by the dicing blade 9 is performed, for example, in a grating-shaped dicing pattern in a plan view on the semiconductor wafer 1 and the resin film 3.
[0097] From the viewpoint of suppressing the temperature rise of the contact portion between the semiconductor wafer 1 or the resin film 3 and the dicing blade 9, the dicing by the dicing blade 9 is usually performed while spraying cooling water (cutting water) on these contact portions. From the viewpoint that the photofusible resin is a water-insoluble resin, the resin film 3 can fully suppress the dissolution of the resin film caused by the cooling water (cutting water), and can fully prevent the cuttings (chips) from adhering to the circuit formation surface of the semiconductor wafer.
[0098] In this manner, the semiconductor wafer 1 and the resin film 3 can be singulated separately to obtain the semiconductor chip 7 with the resin film sheet including the semiconductor chip 1 a and the resin film sheet 3 a .
[0099] The shape of the semiconductor chip 1a in plan view may be, for example, a square or a rectangle. The area of the semiconductor chip 1a may be, for example, 1 to 250 mm. 2 , 4~200mm 2 , or 9~150mm 2 The length of one side of the semiconductor chip 1 a may be greater than 1 mm, greater than 2 mm, or greater than 3 mm, and may be less than 20 mm, less than 18 mm, or less than 15 mm. The thickness of the semiconductor chip 1 a may be the same as the thickness of the semiconductor wafer 1 .
[0100] <Resin film removal process>
[0101] In this step, the resin film 3a of the semiconductor chip 7 with a resin film is irradiated with light A, and the resin film 3a is removed from the semiconductor chip 7 with a resin film (see Figure 2 (a)) The light-melting resin contained in the resin film sheet 3a can easily remove the resin film sheet 3a from the semiconductor chip 7 with the resin film sheet, from the viewpoint of being reduced in molecular weight by irradiation with the light A and thus providing a gel or liquid substance.
[0102] The mechanism of low molecular weight (melting) of photofusible resin is not always obvious, but for example, the following mechanism can be considered. However, it is not limited to these mechanisms. The photofusible resin contains a compound having a disulfide bond (the reaction product of compound A and compound B). The disulfide bonds in the photofusible resin are decomposed (cracked) by irradiating the photofusible resin contained in the resin film with light, and thiol radicals are generated. At this time, if there is a photoradical generator (intramolecular cleavage type photoradical generator), the thiol radical reacts with the photoradical generator, and the thiol radical is capped by the photoradical generator. Thus, it can be considered that the compound with a disulfide bond is low molecular weight and the cured product is photo-softened (photo-melted). As another mechanism, it can also be considered that the photoinduced radical caused by the photoradical generator (intramolecular cleavage type photoradical generator) directly reacts with the disulfide bond, causing the formation of a photoinduced radical-thioether bond and the generation of thiol radicals, and the thiol radical reacts with another photoinduced radical, and the compound with a disulfide bond itself is low molecular weight and softens the photocured material. The disulfide bond cleavage reaction can be said to be an irreversible reaction.
[0103] The light A irradiated to the resin film 3a may be, for example, ultraviolet light or visible light. The wavelength of the light A may be appropriately selected, for example, according to the type of the photo-radical generator used. The wavelength of the light A may be, for example, 150 to 830 nm. The light A may include, for example, light having a wavelength of 405 nm or a wavelength of 365 nm.
[0104] Regarding the irradiation of light A, for example, a light irradiation device can be used and the irradiation amount can be set to 1000 mJ / cm 2 The irradiation dose can be appropriately set according to the wavelength of light A, for example. The irradiation dose can be, for example, 3000 mJ / cm 2 Above, 5000mJ / cm 2 Above or 10000mJ / cm 2 Above, and can be 100000mJ / cm 2 Below, 80000mJ / cm 2 Below, or 60000mJ / cm 2 the following.
[0105] The irradiation amount is the product of the illuminance and the irradiation time (seconds). Examples of the light source for irradiation with ultraviolet light or visible light include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, metal halide lamps, and LED lamps.
[0106] In one embodiment, the resin film sheet removal step may be a step of removing the resin film sheet 3a from the semiconductor chip 7 with the resin film sheet using an aqueous solvent. From the viewpoint of reducing the molecular weight by irradiating light and thereby providing a gel or liquid substance, the photofusible resin contained in the resin film sheet 3a can be fully removed by washing with an aqueous solvent.
[0107] Examples of the aqueous solvent include water, a mixed solvent of water and a hydrophilic organic solvent, etc. In the mixed solvent of water and a hydrophilic organic solvent, the proportion of water can be, for example, 80% by mass or more. For example, a pH adjuster can be added to the aqueous solvent.
[0108] The aqueous solvent can be water. As water, for example, tap water, natural water, purified water, distilled water, ion exchanged water, pure water, ultrapure water (Milli-Q water, etc.) can be cited. In addition, Milli-Q water refers to ultrapure water obtained by the Milli-Q water manufacturing device of Merck Millipore (Merck KGaA). From the viewpoint of impurity reduction, water can be purified water, distilled water, ion exchanged water, pure water, or ultrapure water.
[0109] Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethyl cellosolve, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, butyl cellosolve, ethylene glycol monoisobutyl ether, propylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and dipropylene glycol monomethyl ether.
[0110] As the pH adjusting agent, inorganic acids, inorganic bases, organic acids, organic bases, etc. can be mentioned. As inorganic acids, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, boric acid, etc. can be mentioned. As inorganic bases, sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. can be mentioned. As organic acids, formic acid, acetic acid, propionic acid, butyric acid, acrylic acid, benzoic acid, picolinic acid, etc. can be mentioned. As organic bases, primary amines, secondary amines, tertiary amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, imidazole compounds, etc. can be mentioned.
[0111] In one embodiment, the resin film removal step may be a step of irradiating the resin film 3a of the semiconductor chip 7 with the resin film in the aqueous solvent 11 with light A (see Figure 2 (b)). The photofusible resin contained in the resin film 3a is reduced in molecular weight by irradiation with light, thereby giving a gel or liquid substance. Therefore, by irradiating the resin film 3a with light A in the aqueous solvent 11, the gel or liquid substance flows out in the aqueous solvent 11, and the resin film 3a can be removed efficiently.
[0112] In this manner, a plurality of semiconductor chips 1a (see FIG. 1 ) in which adhesion of cut materials (chips) is sufficiently suppressed can be obtained from the semiconductor wafer 1. Figure 2 (c)).
[0113] The manufacturing method of the semiconductor device of the present embodiment may further include: an ultraviolet irradiation process of irradiating ultraviolet rays to the pressure-sensitive adhesive layer of the dicing tape 5; a picking up process of picking up the semiconductor chip 1a; a semiconductor chip bonding process of bonding the picked up semiconductor chip 1a and the supporting component 13 by thermal compression bonding via an adhesive layer 15 (grain bonding film, etc.); and a thermal curing process of thermally curing the adhesive layer 15, etc.
[0114] <Ultraviolet irradiation process>
[0115] When the pressure-sensitive adhesive layer of the dicing tape 5 is composed of a UV-curable pressure-sensitive adhesive, the method for manufacturing the semiconductor device may include an ultraviolet irradiation step. In this step, the pressure-sensitive adhesive layer is irradiated with ultraviolet rays. In the ultraviolet irradiation, the wavelength of the ultraviolet rays may be 200 to 400 nm. In the ultraviolet irradiation conditions, the illumination and the irradiation amount may be 30 to 240 mW / cm 2 The range is 50~500mJ / cm 2 range.
[0116] <Pick-up process>
[0117] In this step, the individualized semiconductor chips 1 a are separated from each other, and the semiconductor chips 1 a pushed up from the dicing tape 5 side by the needles are sucked by a suction chuck and picked up from the dicing tape 5 .
[0118] The ultraviolet irradiation step and the pickup step may be performed after the resin film sheet removal step or may be performed before the resin film sheet removal step.
[0119] <Semiconductor chip bonding process>
[0120] In this step, the picked-up semiconductor chip 1a and the support member 13 are bonded by thermocompression via an adhesive layer 15 (die bonding film, etc.). The die bonding film can be a die bonding film used in this field. A plurality of semiconductor chips 1a can be bonded to the support member 13.
[0121] The heating temperature during the thermocompression bonding may be, for example, 80 to 160° C. The load during the thermocompression bonding may be, for example, 5 to 15 N. The heating time during the thermocompression bonding may be, for example, 0.5 to 20 seconds.
[0122] <Thermosetting process>
[0123] In this step, the adhesive layer 15 is thermally cured. The heating temperature can be appropriately changed according to the constituent components of the die bonding film. The heating temperature can be, for example, 60 to 200° C., 90 to 190° C., or 120 to 180° C. The heating time can be 30 minutes to 5 hours, 1 to 3 hours, or 2 to 3 hours. In addition, the temperature or pressure can be changed in stages.
[0124] In this manner, a semiconductor device 20 including a semiconductor chip 1a, a support member 13 on which the semiconductor chip 1a is mounted, and an adhesive layer 15 provided between the semiconductor chip 1a and the support member 13 to bond the semiconductor chip 1a to the support member 13 can be manufactured (see Figure 2 (d)).
[0125] Example
[0126] Hereinafter, the present invention will be specifically described by way of Examples, but the present invention is not limited to these Examples.
[0127] [Preparation of Compounds]
[0128] The compounds shown below were prepared.
[0129] Compound A:
[0130] (A-1) Polysulfide rubber LP-3 (dithiol compound, manufactured by TORAY FINE CHEMICALS CO., LTD.)
[0131] Compound B:
[0132] (B1a-1) DENACOL EX-841 (oxirane compound, number of oxirane groups: 2, manufactured by Nagase ChemteX Corporation, epoxy equivalent: 372 g / eq)
[0133] (B1b-1) DENACOL EX-512 (oxirane compound, number of oxirane groups: 4, manufactured by Nagase ChemteX Corporation, epoxy equivalent: 168 g / eq)
[0134] Photo free radical generators:
[0135] (C-1) Omnirad 651 (2,2-dimethoxy-1,2-diphenylethane-1-one (manufactured by IGM Resins BV)
[0136] Curing accelerator:
[0137] (D-1) DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol)
[0138] [Preparation of curable composition]
[0139] Compound A and a curing accelerator having the components and amounts (unit: parts by mass) described in Table 1 were added to a 125 mL ointment jar, mixed at 2000 rpm for 90 seconds using an autorotational stirrer (manufactured by THINKY CORPORATION, trade name: Awatori RentaroARE-310), and then heated at 90° C. for 15 minutes. After cooling, compound B and a curing accelerator were added, and the mixture was stirred at 2000 rpm for 90 seconds using an autorotational stirrer to obtain curable compositions of Preparation Examples 1 and 2.
[0140] [Table 1]
[0141]
[0142] [Preparation of laminated body]
[0143] A resin film was formed on a silicon wafer using the curable composition of Manufacturing Examples 1 and 2. The curable composition was applied with a bar coater, and spin-coated on an 8-inch silicon wafer (thickness: 200 μm) at 25°C at 500 rpm for 5 seconds and then at 2000 rpm for 30 seconds, and heated for 24 hours in a nitrogen atmosphere in a dryer set at 100°C to form a resin film with a thickness of 70 μm on the silicon wafer. Next, a dicing tape was attached to the surface opposite to the resin film of the silicon wafer, and a laminate of Examples 1 and 2 was prepared, which had a dicing tape, a silicon wafer, and a resin film in this order.
[0144] [Cut resistance test]
[0145] The cutting resistance test was conducted using a dicing saw (DISCO Corporation, trade name: DFD6361) and a dicing blade (DISCO Corporation, trade name: Z1: ZH05-SD2000-N1-110FF, Z2: ZH05-SD2000-N1-110EE). The cutting method adopted the step cutting method. In Z1 (the first cutting), the spindle speed was set to 40,000 rpm, the feed speed was set to 50 mm / sec, and the blade height was set to 200 μm. In Z2 (the second cutting), the spindle speed was set to 40,000 rpm, the feed speed was set to 50 mm / sec, and the blade height was set to 80 μm. In addition, the amount of cooling water was set to 1.0 L / min. Under these conditions, the chip size was 5 mm in length and 5 mm in width, and the silicon wafer with a protective layer was cut, and the semiconductor chips with resin film sheets of Examples 1 and 2 were made on the dicing tape. In the semiconductor chips with resin film sheets of Examples 1 and 2, the vicinity of the intersection of the dicing pattern of the resin film was observed under a microscope, and the case where the resin film was not peeled off was evaluated as good "A", and the case where the resin film was peeled off was evaluated as "B". The results are shown in Table 2.
[0146] [Photofusibility test (1)]
[0147] The semiconductor chips with resin film sheets of Examples 1 and 2 obtained in the cutting resistance test were picked up from the dicing tape, and the optical melting test was carried out using the semiconductor chips with resin film sheets. The semiconductor chip with resin film sheet was immersed in a water tank added with pure water, and the resin film sheet of the semiconductor chip with resin film sheet was irradiated with light (LED light with a wavelength of 365nm). For the light irradiation, a UV irradiation device (manufactured by Panasonic Industrial Devices SUNX Co., Ltd., power supply: Aicure UJ30, 365nm LED head: ANUJ6186) was used. Regarding the irradiation conditions, a light receiver for 365nm was used using an illuminance meter UIT-250 (manufactured by USHIO INC.). Regarding the light irradiation, the illuminance was 1000mW / cm 2 Irradiate for 60 seconds with an exposure dose of 60000 mJ / cm 2 After the light was irradiated and the semiconductor chip was placed in a water tank for 15 minutes, the semiconductor chip was observed, and the case where the resin film did not remain on the silicon wafer was evaluated as good and "A", and the case where the resin film remained on the silicon wafer was evaluated as "B". The results are shown in Table 2.
[0148] [Photofusibility test (2)]
[0149] The photofusibility test was conducted in the same manner as the photofusibility test (1) except that a sample in which half of the surface of the semiconductor chip with the resin film was shielded with aluminum foil was used. The exposure dose was set to 10000 mJ / cm 2 、30000mJ / cm 2 and 60000mJ / cm 2 3 conditions.
[0150] Figure 3 This is photographic data showing the results of the optical melting test (2) of the embodiment. The resin film of the semiconductor chip with the resin film of the embodiment 1 and 2 was irradiated with light, and the resin film remained in the part where the light was not irradiated (the part shielded by the aluminum foil). In contrast, the resin film melted in the part where the light was irradiated (the part not shielded by the aluminum foil), and no resin film remained on the silicon wafer.
[0151] [Table 2]
[0152] Example 1 Example 2 Types of curable compositions Production Example 1 Production Example 2 Cut resistance test A A Optical melting test (1) A A
[0153] According to the method for manufacturing a semiconductor device of the present invention, dissolution of a resin film (protective film) by cooling water (cutting water) can be sufficiently suppressed, and the resin film (protective film) can be easily removed.
[0154] Explanation of symbols
[0155] 1-semiconductor wafer, 1a-semiconductor chip, 3-resin film, 3a-resin film sheet, 5-dicing tape, 7-semiconductor chip with resin film sheet, 9-dicing blade, 10-laminated body, 11-aqueous solvent, 13-support member, 15-adhesive layer, 20-semiconductor device.
Claims
1. A method for manufacturing a semiconductor device, comprising: a resin film forming step of forming a resin film including a resin reduced in molecular weight by irradiation with light on the semiconductor wafer; a step of manufacturing a semiconductor chip with a resin film, wherein the semiconductor wafer with the resin film formed thereon is diced with a dicing blade to thereby manufacture individual semiconductor chips with a resin film; and The resin film sheet removing step is to irradiate the resin film sheet of the semiconductor chip with the resin film sheet with light and remove the resin film sheet from the semiconductor chip with the resin film sheet.
2. The method for manufacturing a semiconductor device according to claim 1, in, The resin film sheet removal step is a step of removing the resin film sheet from the semiconductor chip with the resin film sheet using an aqueous solvent.
3. The method for manufacturing a semiconductor device according to claim 1, in, The resin film removal step is a step of irradiating the resin film of the semiconductor chip with the resin film with light in an aqueous solvent.