Method for manufacturing semiconductor device
Through the three-layered body production process, including the superposition grinding of the resin layer and the substrate layer and the water reaction removal, the efficiency and accuracy problems of the back grinding process of the semiconductor wafer are solved, and the efficient removal of the resin layer is achieved. It is suitable for semiconductor chips monolithization and subsequent processes.
Patent Information
- Application Number
- CN202380036146.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-10-11
- Filing Date
- 2023-10-06
- Publication Date
- 2024-12-06
AI Technical Summary
The existing semiconductor wafer back grinding process has problems with efficiency and accuracy, and the removal of the resin layer is difficult, which affects the integrity of the process.
The three-layered body production process is adopted: first, a first laminate containing a low molecular weight resin layer is formed, and the back surface is grounded by superposition of the resin layer and the substrate layer, and then the substrate layer is removed to form the third laminate, and water is passed. Reaction degradation of the resin layer to achieve efficient removal of the resin layer.
The efficiency and accuracy of the back grinding process are improved, the resin layer removal process is simplified, and the back surface of the semiconductor wafer is smooth and residue-free, which is suitable for the monolithization and subsequent processes of semiconductor chips.
Smart Images

Figure CN119096331A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a semiconductor device. Background Art
[0002] In the manufacture of semiconductor devices, the following steps are usually performed: a pattern is formed on one side (surface) of a semiconductor wafer, and the other side (back side) of the semiconductor wafer is ground to a predetermined thickness using a back grinding machine or the like. In the back grinding step, for the purpose of protecting the semiconductor wafer, the following steps are usually performed: a back grinding tape is attached to the semiconductor wafer and the back side is ground (for example, Patent Document 1).
[0003] Previous technical literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-034379 Summary of the invention
[0006] Technical issues to be solved by the invention
[0007] An object of the present invention is to provide a novel method for manufacturing a semiconductor device including a step of grinding the back surface of a semiconductor wafer.
[0008] Means for solving technical problems
[0009] The present invention provides a method for manufacturing a semiconductor device according to [1] to [3].
[0010] [1] A method for manufacturing a semiconductor device, comprising:
[0011] A first stack production step is to produce a first stack comprising a semiconductor wafer, a resin layer containing a resin that has been de-molecularized by reaction with water, and a substrate layer; a second stack production step is to produce a second stack by back grinding the semiconductor wafer of the first stack; and a third stack production step is to remove the substrate layer of the second stack and produce a third stack comprising the semiconductor wafer and the resin layer that have been back ground.
[0012] [2] The method for manufacturing a semiconductor device according to [1], further comprising:
[0013] The step of manufacturing a semiconductor chip with a resin layer is to manufacture individual semiconductor chips with a resin layer by dicing the third stacked body.
[0014] [3] The method for manufacturing a semiconductor device according to [2], further comprising:
[0015] The resin layer sheet removing step causes the resin in the resin layer sheet of the semiconductor chip with the resin layer sheet to react with water, thereby removing the resin layer sheet from the semiconductor chip with the resin layer sheet.
[0016] Effects of the Invention
[0017] According to the present invention, there is provided a novel method for manufacturing a semiconductor device including a step of grinding the back surface of a semiconductor wafer. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 1 middle, Figure 1 (a) Figure 1 (b) Figure 1 (c) and Figure 1 (d) is a diagram showing each process.
[0019] Figure 2 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 2 middle, Figure 2 (a) Figure 2 (b) and Figure 2 (c) is a diagram showing each process.
[0020] Figure 3 is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device. Figure 3 middle, Figure 3 (a) Figure 3 (b) and Figure 3 (c) is a diagram showing each process. DETAILED DESCRIPTION
[0021] Hereinafter, the present embodiment will be described in detail with reference to the accompanying drawings. However, the present invention is not limited to the following embodiments. In the following embodiments, the constituent elements (including steps, etc.) are not necessary except for the cases specifically indicated. The same symbols are marked on the same or equivalent parts, and repeated descriptions are omitted. Regarding the positional relationship such as up, down, left, and right, unless otherwise specified, they are based on the positional relationship shown in the accompanying drawings. The sizes of the constituent elements in each figure are conceptual, and the relative relationship between the sizes of the constituent elements is not limited to those shown in the figures.
[0022] The same is true for the numerical value and its range in the present invention, and the present invention is not limited thereto. In this specification, the numerical range represented by "~" represents the range including the numerical values recorded before and after "~" as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit recorded in a numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In the numerical range recorded in this specification, the upper limit or lower limit of its numerical range can also be replaced by the value shown in the embodiment.
[0023] In this specification, the term "layer" includes not only a structure of a shape formed on the entire surface but also a structure of a shape formed on a part when viewed from a top view. In this specification, the term "process" includes not only an independent process but also a process that can achieve the desired effect of the process even if it cannot be clearly distinguished from other processes.
[0024] In this specification, "(meth)acryloyl" refers to at least one of acryloyl and methacryloyl. In this specification, "(poly)oxyalkylene" refers to at least one of oxyalkylene and polyoxyalkylene. Polyoxyalkylene is a group in which two or more alkylene groups are linked by an ether bond. The same applies to other similar expressions such as "(poly)oxyethylene".
[0025] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.
[0026] [Method for manufacturing semiconductor device]
[0027] A method for manufacturing a semiconductor device according to one embodiment of the present invention relates to a method for manufacturing a semiconductor device including a step of back grinding a semiconductor wafer. The method for manufacturing a semiconductor device includes a first stacked body manufacturing step, a second stacked body manufacturing step, and a third stacked body manufacturing step. The method for manufacturing a semiconductor device may further include a step of manufacturing a semiconductor chip with a resin layer, and may further include a step of removing the resin layer. Figure 1 , Figure 2 and Figure 3 This is a schematic cross-sectional view for explaining one embodiment of a method for manufacturing a semiconductor device.
[0028] <First laminate production step>
[0029] In this step, a first laminate 10 is prepared, which includes a semiconductor wafer 1, a resin layer 3 including a resin that is reduced in molecular weight by reacting with water (hereinafter also referred to as "resin A"), and a base material layer 5. Resin A is a resin that has the property of being reduced in molecular weight by reacting with water, thereby increasing its solubility in water.
[0030] In one embodiment, the resin A may be a resin containing an ester bond and a basic functional group. The resin containing an ester bond and a basic functional group is a resin that undergoes a hydrolysis reaction of the ester bond in the presence of a basic functional group by reacting with water to reduce the molecular weight. The resin layer 3 may be formed, for example, by curing the resin A or by reacting and curing a precursor of the resin A.
[0031] Examples of the basic functional group in the resin A include -NH- and -NH2.
[0032] Resin A can be formed using a resin layer forming material comprising the following compounds: compound A, which comprises two or more first groups and has an ester bond; and compound B, which comprises two or more second groups that can form a bond with the first group and can form a resin comprising an ester bond and a basic functional group by reacting with compound A.
[0033] Compound A may include an ester bond in the first group, and may include an ester bond as a functional group different from the first group. Examples of the first group in compound A include (meth)acryloyloxy; isocyanate; cyclic ether group (oxirane group (oxiranyl group, epoxy group), oxetanyl group (oxetanyl group), tetrahydrofuranyl group, tetrahydropyranyl group, etc.); ethylenically unsaturated group (C=C), etc. The number of the first group in the molecule of compound A1 is 2 or more, 3 or more, or 4 or more, and may be 10 or less, 8 or less, 6 or less, or 5 or less.
[0034] Compound A may be a compound comprising a linking group that links two or more first groups and these first groups. Regarding the linking group, for example, it may include a (poly)oxyalkylene group. As the (poly)oxyalkylene group, a (poly)oxyethylene group may be cited. The linking group may include at least one skeleton selected from the group consisting of a pentaerythritol skeleton, a trimethylolpropane skeleton, and an isocyanurate skeleton.
[0035] The molecular weight or number average molecular weight of compound A may be 150 or more, 500 or more, or 1000 or more, and may be 50000 or less, 10000 or less, or 2000 or less. In this specification, the "number average molecular weight" is a polystyrene conversion value obtained by gel permeation chromatography (GPC) using a calibration curve based on standard polystyrene.
[0036] Compound A may be a compound containing two first groups or a compound containing two (meth)acryloyloxy groups. When containing two first groups, the time required for resin A to dissolve in water tends to be longer than when containing two first groups.
[0037] The compound A including two (meth)acryloyloxy groups may include a structure represented by the following formula (a1).
[0038]
[0039] In formula (a1), R represents a hydrogen atom or a methyl group. 1 The number of carbon atoms in the alkylene group may be, for example, 2 or more, and may be 10 or less, 6 or less, 4 or less, or 3 or less. The alkylene group may be, for example, ethylene (-CH2-CH2-).
[0040] n represents an integer greater than or equal to 1. For example, n may be greater than or equal to 1, greater than or equal to 5, greater than or equal to 10, greater than or equal to 15, or greater than or equal to 20, and may be less than or equal to 50, less than or equal to 45, less than or equal to 40, less than or equal to 35, less than or equal to 30, or less than or equal to 25.
[0041] Examples of commercially available products of compound A containing two (meth)acryloyloxy groups include NK ester A-1000 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #1000 diacrylate), A-600 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #600 diacrylate), A-400 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #400 diacrylate), A-200 (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #200 diacrylate), 2G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: diethylene glycol dimethacrylate), 3G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: diethylene glycol dimethacrylate), Co., Ltd., chemical name: triethylene glycol dimethacrylate), 4G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #200 dimethacrylate), 9G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #400 dimethacrylate), 14G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #600 dimethacrylate), 23G (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: polyethylene glycol #1000 dimethacrylate), Light Acrylate 3EGA (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: triethylene glycol dimethacrylate), Light Acrylate 4EG-A (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #200 dimethacrylate), Light Acrylate 9EG-A (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #400 diacrylate), Light Acrylate 14EG-A (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #600 diacrylate), Light Acrylate EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: ethylene glycol dimethacrylate), Light Acrylate 2EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: ethylene glycol dimethacrylate),, chemical name: diethylene glycol dimethacrylate), light ester 3EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: triethylene glycol dimethacrylate), light ester 4EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #200 dimethacrylate), light ester 9EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #400 dimethacrylate), light ester 14EG (manufactured by Kyoeisha Chemical Co., Ltd., chemical name: polyethylene glycol #600 dimethacrylate), FANCRYL FA-222A (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol diacrylate), FANCRYL FA-232A (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol diacrylate), FANCRYL FA-220A, FA-230A, FA-240A, FA-260A, FA-2100A, FA-2200A (all manufactured by Showa Denko Materials Co., Ltd., chemical name: polyethylene glycol diacrylate), FANCRYL FA-222M (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol dimethacrylate), FANCRYL FA-232M (manufactured by Showa Denko Materials Co., Ltd., chemical name: diethylene glycol dimethacrylate), FANCRYL FA-220M, FA-230M, FA-240M, FA-260M, FA-2100M, FA-2200M (all manufactured by Showa Denko Materials Co., Ltd., chemical name: polyethylene glycol dimethacrylate). .
[0042] The compound A may be a compound containing three or more first groups, or may be a compound containing three or more (meth)acryloyloxy groups.
[0043] The compound A including three or more (meth)acryloyloxy groups may be, for example, a compound represented by the following formula (a2).
[0044]
[0045] In formula (a2), R represents a hydrogen atom or a methyl group, and X 2represents an alkylene group. a, b, c and d are each independent and represent an integer greater than or equal to 0 or 1. Multiple Rs may be the same or different. 2 The carbon number of the alkylene group represented by may be 2 or more, and may be 10 or less, 6 or less, or 3 or less. 2 The alkylene represented by X may be, for example, ethylene (-CH2-CH2-). 2 When there are multiple numbers, they may be the same or different. The total of a, b, c and d, a+b+c+d, may be, for example, 1 or more, 5 or more, 10 or more, 15 or more, 20 or more, 25 or more, or 30 or more, and may be 60 or less, 55 or less, 50 or less, 45 or less, or 40 or less.
[0046] Examples of commercially available products of compound A containing three or more (meth)acryloyloxy groups include NK ester ATM-35E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated pentaerythritol tetraacrylate), NK ester A-TMPT-9EO (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated trimethylolpropane triacrylate), NK ester AT-20E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated trimethylolpropane triacrylate), NK ester A-GLY-3E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated glycerol triacrylate), NK ester AGLY-9E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated glycerol triacrylate), NK ester A-GLY-20E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated trimethylolpropane triacrylate). Co., Ltd., chemical name: ethoxylated glycerol triacrylate) and A-DPH-12E (manufactured by Shin-Nakamura Chemical Co., Ltd., chemical name: ethoxylated dipentaerythritol polyacrylate).
[0047] Compound A may be a compound showing solubility in water. The solubility of compound A in 100 g of water at 25° C. may be 1 g or more, 5 g or more, or 10 g or more. The upper limit of the solubility is not particularly limited.
[0048] The content of compound A may be 80 parts by mass or more, 85 parts by mass or more, or 90 parts by mass or more, and may be 99 parts by mass or less, 95 parts by mass or less, or 90 parts by mass or less, based on 100 parts by mass of the total content of compound A and compound B.
[0049] The second group in compound B is appropriately selected according to the type of the first group. Regarding the combination of the first group and the second group, for example, it can be a combination of at least one first group selected from the group consisting of a (meth)acryloyloxy group, an isocyanate group, a cyclic ether group (oxirane group (oxiranyl group, epoxy group), oxetanyl group (oxetanyl group), tetrahydrofuranyl group, tetrahydropyranyl group, etc.) and an ethylenically unsaturated group (C=C) and at least one second group selected from the group consisting of an amino group (-NH-, -NH2) and a mercapto group (-SH), or it can be a combination of a (meth)acryloyloxy group and an amino group (-NH-, -NH2).
[0050] The number of the second groups in the compound B1 molecule is 2 or more, and may be 10 or less, 8 or less, 6 or less, 4 or less, or 3 or less, or 2. The number of the second groups in the compound B1 molecule may be the same as or different from the number of the first groups in the compound A1 molecule, or may be less than the number of the first groups in the compound A1 molecule.
[0051] Compound B may contain a functional group other than the second group. Examples of the functional group other than the second group include an alkylene group and -NH-(imino) group.
[0052] Compound B may be a compound containing two or more second groups and an alkylene group, a compound containing two or more second groups, an alkylene group, and -NH-, or a compound containing two or more amino groups, an alkylene group, and -NH-.
[0053] The compound B may be, for example, a compound represented by the following formula (b).
[0054] H2N-Y-NH2 (b)
[0055] Y represents a divalent group including an alkylene group. The divalent group including an alkylene group represented by Y may include -NH-. Compound B may be, for example, a compound represented by the following formula (b1).
[0056]
[0057] In formula (b), Z represents an alkylene group. The alkylene group may have 1 or more, 2 or more, or 3 or more carbon atoms, and may have 10 or less, 8 or less, 6 or less, or 4 or less carbon atoms.
[0058] Examples of compound B include bis(3-aminopropyl)amine, norbornanediamine, ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, polyetheramine, 4,4′-diaminodiphenyl sulfone, 3,3′-diaminodiphenyl sulfone, 4,4′-diaminodiphenyl ether, 1,3-bis(3-aminophenoxy)benzene, dianiline, aminobenzylamine, and polyoxypropylenediamine.
[0059] Compound B may be a compound showing solubility in water. The solubility of compound B in 100 g of water at 25° C. may be 1 g or more, 5 g or more, or 10 g or more. The upper limit of the solubility is not particularly limited.
[0060] The ratio of the number of moles of compound B to the number of moles of compound A (the number of moles of compound B / the number of moles of compound A) may be 0.20 or more, 0.40 or more, 0.60 or more, 0.80 or more, or 1.00 or more. The ratio of the number of moles of compound B to the number of moles of compound A (the number of moles of compound B / the number of moles of compound A) may be, for example, 10.00 or less, 8.00 or less, 6.00 or less, 4.00 or less, 3.00 or less, 2.50 or less, or 2.20 or less.
[0061] The content of compound B may be 1 part by mass or more, 5 parts by mass or more, 8 parts by mass or more, or 10 parts by mass or more relative to 100 parts by mass of the total content of compound A and compound B. The content of compound B may be 20 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, or 8 parts by mass or less relative to 100 parts by mass of the total content of compound A and compound B.
[0062] The resin A, which is a reaction product of compound A and compound B, can be obtained by mixing or kneading these compounds. Mixing and kneading can be performed by appropriately combining a common disperser such as a stirrer, a pestle, a three-roll mill, a ball mill, or a bead mill.
[0063] The reaction may be carried out while heating as required. The reaction temperature when reacting compound A and compound B may be, for example, 0°C or more, 10°C or more, or 20°C or more, and may be 100°C or less, 85°C or less, or 70°C or less. The time for maintaining the reaction temperature may be, for example, 1.0 minute or more, and may be 60 minutes or less, 30 minutes or less, 10 minutes or less, 5 minutes or less, or 3 minutes or less.
[0064] The resin layer 3 may further include components (other components) other than the resin A. As other components, for example, plasticizers; adhesiveness imparting agents such as tackifiers; antioxidants; leuco dyes; sensitizers; adhesion improvers such as coupling agents; polymerization inhibitors; light stabilizers; defoamers; fillers; chain transfer agents; thixotropy imparting agents; flame retardants; mold release agents; surfactants; lubricants; antistatic agents and other additives can be used for these additives. Known additives can be used. When the resin layer 3 contains other components, the total amount of the content of the other components is based on the total amount of the resin layer 3, and can be 0 to 95% by mass, 0.01 to 50% by mass, or 0.1 to 10% by mass.
[0065] Resin A can be diluted with an organic solvent and used as a varnish. Examples of the organic solvent include aromatic hydrocarbons such as toluene, xylene, mesitylene, cumene, and p-cymene; aliphatic hydrocarbons such as hexane and heptane; cycloalkanes such as methylcyclohexane; cyclic ethers such as tetrahydrofuran and 1,4-dioxane; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and 4-hydroxy-4-methyl-2-pentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, methyl lactate, ethyl lactate, and γ-butyrolactone; carbonates such as ethylene carbonate and propylene carbonate; amides such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone (NMP). The solid content in the varnish, that is, the content other than the organic solvent in the varnish, can be 10 to 95% by mass, 15 to 70% by mass, or 20 to 50% by mass based on the total amount of the varnish.
[0066] The first stacked body manufacturing process may include, for example, a process of preparing a semiconductor wafer 1; a process of forming a resin layer 3 containing a resin A on the semiconductor wafer 1 (see Figure 1 and configuring the base material layer 5 on the resin layer 3, and preparing the first stacked body 10 step (reference Figure 1 (b)).
[0067] The first stacked body manufacturing process is not limited to the above method, and may include, for example, a process of forming a resin layer 3 containing resin A on a base layer 5; a process of arranging a stacked body including a base layer 5 and a resin layer 3 on a semiconductor wafer 1 in such a manner that the resin layer 3 is in contact with the semiconductor wafer 1, thereby manufacturing the first stacked body 10 (see Figure 1 (b)) As a method for arranging the laminated body including the base material layer 5 and the resin layer 3 on the semiconductor wafer 1, there can be mentioned a method of laminating or stacking in a heating process or at room temperature.
[0068] Examples of the semiconductor wafer 1 include single crystal silicon, polycrystalline silicon, various ceramics, and compound semiconductors such as gallium arsenide. The semiconductor wafer 1 may have a circuit formation surface.
[0069] The thickness d1 of the semiconductor wafer 1 may be, for example, 10 to 1000 μm, 20 to 900 μm, or 30 to 800 μm.
[0070] As a method for forming a resin layer on a semiconductor wafer, for example, a method including the following steps can be used: applying a resin on a semiconductor wafer by a spin coating method, a slit coating method, etc.; and forming a resin layer by curing the applied resin. The resin layer can be arranged on a circuit formation surface on a semiconductor wafer, for example. The resin can be cured at room temperature.
[0071] The thickness of the resin layer 3 may be, for example, 1 to 1000 μm, 3 to 500 μm, or 5 to 200 μm.
[0072] In the third laminate production step, the substrate layer 5 can be made of a material that can be removed from the resin layer 3. Examples of the substrate layer 5 include polyolefin films such as polyethylene (PE) and polypropylene (PP); polyester films such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate; polyvinyl chloride (PVC) films; polyimide (PI) films; polyphenylene sulfide (PPS) films; ethylene vinyl acetate (EVA) films; and polytetrafluoroethylene (PTFE) films.
[0073] The thickness of the base material layer 5 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 200 μm.
[0074] In this manner, the first laminate 10 including the semiconductor wafer 1 , the resin layer 3 including the resin A, and the base material layer 5 in this order can be manufactured.
[0075] <Second laminate production step>
[0076] In this step, the semiconductor wafer 1 of the first stack 10 is back-ground to produce the second stack 20 (see Figure 1 (c)). The base layer 5 and the resin layer 3 of the first stack 10 can be regarded as a back grinding tape 7 having the base layer 5 and the resin layer 3 provided on the base layer 5. The first stack 10 can attach the back grinding tape 7 to the semiconductor wafer 1, and the first stack 10 can be directly used in the back grinding (back grinding) process.
[0077] The back grinding of the semiconductor wafer 1 can be performed using a conventional back grinding machine. Figure 1As shown in (d), the semiconductor wafer 1 is thinned using, for example, a grinder 9 on the surface of the semiconductor wafer 1 opposite to the surface to which the back grinding tape 7 is attached.
[0078] The thickness d1A of the back-ground semiconductor wafer (semiconductor wafer 1A) is thinner than the thickness d1 of the semiconductor wafer 1 , and may be, for example, 10 to 1000 μm, 20 to 900 μm, or 30 to 800 μm.
[0079] In this manner, the second laminated body 20 including the semiconductor wafer 1A, the resin layer 3 including the resin A, and the base material layer 5 in this order can be manufactured.
[0080] <Third laminate production step>
[0081] In this step, the base material layer 5 of the second stacked body 20 is removed to produce a third stacked body 30 including the semiconductor wafer 1A and the resin layer 3 (see FIG. Figure 2 (a)).
[0082] There is no particular limitation on the method for removing the substrate layer 5 from the second laminate 20, and a common method can be used. For example, as the substrate layer 5, a material having adhesiveness is used on the surface in contact with the resin layer 3, and the degree of adhesiveness thereof is adjusted, thereby enabling the substrate layer 5 to be removed from the second laminate 20.
[0083] The resin layer 3 of the third stacked body 30 can be used as a protective layer for the semiconductor wafer 1A in the next process. The resin layer 3 is reduced in molecular weight by reacting with water, and as a result, contains a resin having improved solubility in water. Therefore, it can be easily removed using an aqueous solvent in the process after being used as a protective layer.
[0084] <Process for manufacturing semiconductor chips with resin layers>
[0085] In this step, the third stacked body 30 is diced to produce individual semiconductor chips 15 with resin layers.
[0086] The process of manufacturing a semiconductor chip with a resin layer sheet may include, for example, a process of preparing a stacked body 40 having a dicing tape 11, a semiconductor wafer 1A, and a resin layer 3 in this order (see Figure 2 and in the laminate 40, at least by cutting the semiconductor wafer 1A and the resin layer 3, and obtaining a single-piece semiconductor chip 15 with a resin layer (reference Figure 2 (c)).
[0087] As the dicing tape 11, for example, plastic films such as polytetrafluoroethylene film, polyethylene terephthalate film, polyethylene film, polypropylene film, polymethylpentene film, polyimide film, etc. can be cited. The dicing tape 11 can also be subjected to surface treatments such as primer coating, UV treatment, corona discharge treatment, grinding treatment, etching treatment, etc. as needed. The dicing tape 11 can have adhesiveness. Such a dicing tape 11 can impart adhesiveness to the above-mentioned plastic film, or it can be a dicing tape having a pressure-sensitive adhesive layer on one side of the above-mentioned plastic film. The pressure-sensitive adhesive layer can be formed by a UV-curable or UV-non-curable pressure-sensitive pressure-sensitive adhesive, and there is no particular limitation as long as it has sufficient adhesive force to prevent the semiconductor elements from flying apart during dicing, and a previously known pressure-sensitive adhesive layer can be used.
[0088] The thickness of the dicing tape 11 may be, for example, 10 to 1000 μm, 30 to 500 μm, or 50 to 300 μm.
[0089] The stacked body 40 can be obtained by attaching the dicing tape 11 to the semiconductor wafer 1A of the third stacked body 30 .
[0090] Next, in the stacked body 40, at least the semiconductor wafer 1A and the resin layer 3 (and a portion of the dicing tape 11) are cut and singulated. The cutting may be, for example, cutting by a dicing blade 13. The cutting by the dicing blade 13 may be performed using a commercially available device. The cutting by the dicing blade 13 may be performed, for example, in a grid-shaped cutting pattern in a plan view with respect to the semiconductor wafer 1A and the resin layer 3.
[0091] From the viewpoint of suppressing a temperature rise in a contact portion between the semiconductor wafer 1A or the resin layer 3 and the dicing blade 13 , dicing by the dicing blade 13 may be performed while spraying cooling water (cutting water) to these contact portions.
[0092] The resin layer 3 can function as a protective layer that prevents cut materials (chips) from adhering to the circuit formation surface of the semiconductor wafer.
[0093] As for the cutting instead of the blade cutting, for example, it may be plasma cutting, stealth cutting, or laser cutting.
[0094] In this manner, the semiconductor wafer 1A and the resin layer 3 can be singulated separately to obtain the semiconductor chip 15 with the resin layer sheet including the semiconductor chip 1Aa and the resin layer sheet 3a.
[0095] The shape of the semiconductor chip 1Aa in plan view may be, for example, a square or a rectangle. The area of the semiconductor chip 1a may be, for example, 1 to 250 mm. 2 , 4~200mm 2 , or 9~150mm 2 The length of one side of the semiconductor chip 1a may be greater than 1 mm, greater than 2 mm, or greater than 3 mm, and may be less than 20 mm, less than 18 mm, or less than 15 mm. The thickness of the semiconductor chip 1Aa may be the same as the thickness of the semiconductor wafer 1A.
[0096] <Resin layer removal process>
[0097] In this step, the resin in the resin layer sheet 3a of the semiconductor chip with a resin layer sheet 15 is reacted with water, and the resin layer sheet 3a is removed from the semiconductor chip with a resin layer sheet 15. From the viewpoint of reducing the molecular weight by reacting with water and thus improving the solubility in water, the resin A contained in the resin layer sheet 3a can be easily removed from the semiconductor chip with a resin layer sheet 15 by using water.
[0098] Examples of the aqueous solvent include water, a mixed solvent of water and a hydrophilic organic solvent, etc. In the mixed solvent of water and a hydrophilic organic solvent, the proportion of water can be, for example, 80% by mass or more. For example, a pH adjuster can be added to the aqueous solvent.
[0099] The aqueous solvent can be water. As water, for example, tap water, natural water, purified water, distilled water, ion exchanged water, pure water and ultrapure water (Milli-Q water, etc.) can be cited. Milli-Q water refers to ultrapure water obtained by the Milli-Q water manufacturing device of Merck Millipore (Merck KGaA). From the viewpoint of impurity reduction, water can be purified water, distilled water, ion exchanged water, pure water, or ultrapure water.
[0100] Examples of the hydrophilic organic solvent include alcohols such as methanol, ethanol, 2-propanol, and 1,2-propylene glycol; and glycol ethers such as ethylene glycol monomethyl ether, propylene glycol monomethyl ether, ethyl cellosolve, propylene glycol monopropyl ether, propylene glycol monoisopropyl ether, butyl cellosolve, ethylene glycol monoisobutyl ether, propylene glycol monobutyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, and dipropylene glycol monomethyl ether.
[0101] As the pH adjusting agent, inorganic acids, inorganic bases, organic acids, organic bases, etc. can be mentioned. As inorganic acids, nitric acid, sulfuric acid, hydrochloric acid, phosphoric acid, boric acid, etc. can be mentioned. As inorganic bases, sodium hydroxide, potassium hydroxide, calcium hydroxide, etc. can be mentioned. As organic acids, formic acid, acetic acid, propionic acid, butyric acid, acrylic acid, benzoic acid, picolinic acid, etc. can be mentioned. As organic bases, primary amines, secondary amines, tertiary amines, tetramethylammonium hydroxide, tetraethylammonium hydroxide, imidazole compounds, etc. can be mentioned.
[0102] The temperature of the water used to react the resin with water may be, for example, 5°C or higher, 10°C or higher, 15°C or higher, 20°C or higher, 25°C or higher, 35°C or higher, 45°C or higher, or 55°C or higher, and may be 80°C or lower, or 70°C or lower. By adjusting the temperature of the water used to react the resin with water, etc., the time required for the resin layer to dissolve in the water can be adjusted. By increasing the temperature of the water used to react the resin with water, the resin layer tends to dissolve in the water in a shorter time.
[0103] The time for reacting the resin with water may be, for example, 5 minutes or more, 10 minutes or more, 30 minutes or more, 60 minutes or more, 90 minutes or more, or 120 minutes or more, and may be 150 minutes or less, 120 minutes or less, 90 minutes or less, 60 minutes or less, 45 minutes or less, or 30 minutes or less.
[0104] In one embodiment, the resin layer removal step may be a step of immersing the resin layer 3a in the aqueous solvent 17 from the semiconductor chip 15 with the resin layer (see Figure 3 (a)) From the viewpoint of reducing the molecular weight by reacting with water and thereby improving the solubility in water, the resin A contained in the resin layer 3a flows out in the aqueous solvent 17 by being immersed in the aqueous solvent 17, and the resin layer 3a can be removed efficiently.
[0105] In this manner, a plurality of semiconductor chips 1Aa (see FIG. 1A ) in which adhesion of cut materials (chips) is sufficiently suppressed can be obtained from the semiconductor wafer 1A. Figure 3 (b)).
[0106] The manufacturing method of the semiconductor device of the present embodiment may further include: an ultraviolet irradiation process of irradiating ultraviolet rays to the pressure-sensitive adhesive layer of the dicing tape 11; a picking up process of picking up the semiconductor chip 1Aa; a semiconductor chip bonding process of bonding the picked up semiconductor chip 1Aa and the supporting component 19 by thermal compression bonding via an adhesive layer 21 (grain bonding film, etc.); and a thermal curing process of thermally curing the adhesive layer 21, etc.
[0107] <Ultraviolet irradiation process>
[0108] When the pressure-sensitive adhesive layer of the dicing tape 11 is composed of a UV-curable pressure-sensitive adhesive, the method for manufacturing a semiconductor device may include an ultraviolet irradiation step. In this step, the pressure-sensitive adhesive layer is irradiated with ultraviolet rays. In the ultraviolet irradiation, the wavelength of the ultraviolet rays may be 200 to 400 nm. In the ultraviolet irradiation conditions, the illumination and the irradiation amount may be 30 to 240 mW / cm 2 The range is 50~500mJ / cm 2 range.
[0109] <Pick-up process>
[0110] In this step, the individualized semiconductor chips 1Aa are separated from each other, and the semiconductor chips 1Aa pushed up from the dicing tape 11 side by the needles are sucked by a suction chuck and picked up from the dicing tape 11 .
[0111] The ultraviolet irradiation step and the pickup step may be performed after the resin layer sheet removal step or may be performed before the resin layer sheet removal step.
[0112] <Semiconductor chip bonding process>
[0113] In this step, the picked-up semiconductor chip 1Aa and the support member 19 are bonded by thermocompression via an adhesive layer 21 (die bonding film, etc.). The die bonding film can be a die bonding film used in this field. A plurality of semiconductor chips 1Aa can be bonded to the support member 19.
[0114] The heating temperature during the thermocompression bonding may be, for example, 80 to 160° C. The load during the thermocompression bonding may be, for example, 5 to 15 N. The heating time during the thermocompression bonding may be, for example, 0.5 to 20 seconds.
[0115] <Thermosetting process>
[0116] In this step, the adhesive layer 21 is thermally cured. The heating temperature can be appropriately changed according to the constituent components of the die bonding film. The heating temperature can be, for example, 60 to 200° C., 90 to 190° C., or 120 to 180° C. The heating time can be 30 minutes to 5 hours, 1 to 3 hours, or 2 to 3 hours. The temperature or pressure can be changed in stages.
[0117] In this manner, a semiconductor device 50 including a semiconductor chip 1Aa, a support member 19 on which the semiconductor chip 1Aa is mounted, and an adhesive layer 21 provided between the semiconductor chip 1Aa and the support member 19 to bond the semiconductor chip 1Aa and the support member 19 can be manufactured (see Figure 3 (c)).
[0118] Explanation of symbols
[0119] 1. 1A-semiconductor wafer, 1Aa-semiconductor chip, 3-resin layer, 3a-resin layer sheet, 5-base layer, 7-back grinding tape, 9-grinder, 10-first stack, 11-dicing tape, 13-dicing blade, 15-semiconductor chip with resin layer sheet, 17-aqueous solvent, 19-support component, 20-second stack, 21-adhesive layer, 30-third stack, 40-stack, 50-semiconductor device.
Claims
1. A method for manufacturing a semiconductor device, comprising: A first laminate production step of producing a first laminate including a semiconductor wafer, a resin layer including a resin that is reduced in molecular weight by reaction with water, and a base material layer; a second stacked body manufacturing step of performing back grinding on the semiconductor wafer of the first stacked body to manufacture a second stacked body; and The third stacked body manufacturing step is to remove the base layer of the second stacked body and manufacture a third stacked body including the semiconductor wafer and the resin layer that have been back-ground.
2. The method for manufacturing a semiconductor device according to claim 1, further comprising: The step of manufacturing a semiconductor chip with a resin layer is to manufacture individual semiconductor chips with a resin layer by dicing the third stacked body.
3. The method for manufacturing a semiconductor device according to claim 2, further comprising: The resin layer sheet removing step causes the resin in the resin layer sheet of the semiconductor chip with the resin layer sheet to react with water, thereby removing the resin layer sheet from the semiconductor chip with the resin layer sheet.
Citation Information
Patent Citations
Back grinding tape
JP2010034379A