Device for utilizing solar energy to drive photo-thermal catalytic oxidation of VOCs and application of device

By using defective 3DOM LaMn1.2O3 material in the photothermal catalytic oxidation VOCs device, using Fresnel lens to focus the sunlight, the problem of low solar light utilization efficiency is solved, and efficient catalyzing of VOCs at low light intensity is achieved, which significantly improves the Catalytic activity and water resistance stability.

CN119139859AActive Publication Date: 2024-12-17INST OF URBAN ENVIRONMENT CHINESE ACAD OF SCI

Patent Information

Application Number
CN202310719267.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-16
Publication Date
2024-12-17
Estimated Expiration
2043-06-16

AI Technical Summary

Technical Problem

In the prior art, when using solar energy to catalyze the oxidation of volatile organic compounds (VOCs), the solar light utilization efficiency is low, high-intensity light is required, and it is susceptible to intermediate product deposition, and lacks efficient, low-cost, and large-scale utilization methods.

Method used

A solar-driven photothermal catalytic oxidation VOCs device is designed, including a miniature photothermal reactor, a light source that simulates sunlight and a Fresnel lens. The defective 3DOM LaMn1.2O3 is used as the photothermal material and uses polymethyl methacrylic acid Ester (PMMA) prepares LaMn1.2O3 in three-dimensional ordered macroporous structures, increasing oxygen defects to enhance light absorption and catalytic activity.

Benefits of technology

It has achieved effective catalyzed VOCs at lower light intensity, especially under 60mW/cm² sunlight irradiation, which can achieve 100% toluene conversion and 90% mineralization in a short time, expanding the solar light utilization range. Improves catalytic activity and water resistance stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119139859A_ABST
    Figure CN119139859A_ABST
Patent Text Reader

Abstract

The invention discloses a device for carrying out photo-thermal catalytic oxidation on VOCs (Volatile Organic Compounds) by utilizing daily solar energy and application of the device. The photo-thermal device comprises a miniature photo-thermal reactor, a light source simulating sunlight, a Fresnel lens and a photo-thermal material. The device is applied to solar-driven photo-thermal catalytic oxidation of VOCs (Volatile Organic Compounds). According to the invention, daily sunlight (the light intensity is 50-70mW / cm < 2 >) is converged through the Fresnel lens, and the light intensity can be increased by dozens of times. Focused sunlight is absorbed by providing defect type three-dimensional macroporous lanthanum manganate, and light energy is converted into heat energy and chemical energy. The invention has the following beneficial effects: under the irradiation of daily sunlight, the toluene degradation rate is up to 100% and the mineralization efficiency can reach more than 90% through a condensation catalysis system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of photocatalysis technology, and specifically relates to a device and application thereof for photocatalytically oxidizing VOCs using daily solar energy. Background Art

[0002] Volatile organic compounds (VOCs) are important precursors of PM2.5 and ozone pollution, and some of them are toxic and malodorous substances. Long-term exposure can be harmful to human health.

[0003] Thermal catalytic oxidation has been commercialized for various industrial VOCs treatment, which requires fossil fuel combustion to provide thermal energy as a driving force. However, high-temperature operation caused by fossil fuel combustion will increase energy consumption and bring new pollution. Using clean, pollution-free, renewable solar energy to drive VOCs to undergo oxidation reactions is an ideal way to achieve VOCs purification. For full-spectrum sunlight, semiconductor photocatalysts can usually only absorb ultraviolet light, or part of the visible light, while the energy in the infrared region is not enough to excite VOCs to react. Part of the visible and all of the infrared in the solar spectrum have not been effectively utilized.

[0004] Photothermal conversion is a new type of solar energy utilization solution. Some metal oxide catalysts have wide spectrum high absorption, good thermal stability, structural modifiability and redox ability, and are therefore favored. Wang Wenzhong et al. reported the catalytic performance of two-dimensional porous Co3O4 materials for propylene and propane under sunlight. Li Yuanzhi's team studied a series of bimetallic oxide photothermal catalysts CeO2 / TiO2, Co3O4 / TiO2, MnO x / TiO2、CeMn x O y / TiO2, etc. Although the research on metal oxide photothermal catalysts in VOCs treatment has achieved certain results, there are still many problems that need to be solved. For example, high-intensity light (500mW / cm 2 above), are susceptible to the deposition of intermediate products.

[0005] At present, the efficiency of solar energy conversion is low. One important reason is that the solar energy density is low, the dispersion is strong, and it is discontinuous, so we still lack effective means to utilize it efficiently, at low cost, and on a large scale. Therefore, how to use the advantages of the structural diversity, controllability, and designability of metal oxides to rationally design and prepare efficient, stable, and economical photothermal catalysts, and how to use concentrating equipment to achieve excellent VOCs purification capabilities under daily sunlight requires more innovative research work. Summary of the invention

[0006] The purpose of the present invention is to provide a device for utilizing daily sunlight, which can make full use of the diffused daily sunlight and the ultraviolet, visible and infrared spectrum parts of the full solar spectrum and focus the diffused sunlight, thereby solving the problem of insufficient utilization of sunlight in the prior art.

[0007] The present invention is achieved through the following technical solutions:

[0008] A solar-powered photothermal catalytic oxidation device for VOCs comprises a micro photothermal reactor, a light source for simulating sunlight, a Fresnel lens, and photothermal materials.

[0009] The photothermal reactor is a microreactor, the light source is located just above the light window of the microreactor, the Fresnel lens is between the two, the lens diameter is adjustable, the focused light spot size is adjustable, and the light intensity can be increased by dozens of times.

[0010] The photothermal material is defective 3DOM LaMn 1.2 O3, 3DOM LaMn prepared by using polymethyl methacrylate (PMMA) as a hard template 1.2 O3. Among them, manganese metal oxide MnO x In-situ precipitation on the three-dimensional ordered framework of LaMnO3 can achieve a highly dispersed and uniform distribution of metal oxides. Its multiple scattering and reflection can enhance light absorption and maximize the use of sunlight. Reduction of 3DOM LaMn by sodium borohydride, hydrogen, aluminum, etc. 1.2 O3 creates surface oxygen defects and increases active sites.

[0011] According to an embodiment of the present invention, the defective LaMn 1.2 O3 materials have three-dimensional ordered macroporous structures and oxygen defects.

[0012] According to an embodiment of the present invention, the defective LaMn 1.2 O3 materials have a photothermal synergistic enhancement effect.

[0013] The present invention also provides the above three-dimensional ordered macroporous material LaMn 1.2 The application of O3 as a catalyst. Preferably, the application in the photothermal synergistic catalytic purification of VOCs. More preferably, the application of the catalyst driven by sunlight as an energy source (instead of traditional fossil fuels) in the photothermal synergistic catalytic purification of VOCs.

[0014] Exemplarily, the application in the photothermal synergistic catalytic oxidation of toluene.

[0015] Beneficial Effects

[0016] (1) The full solar spectrum sunlight utilization device provided by the present invention can maximize the use of daily sunlight, and use the line focusing Fresnel lens to focus daily sunlight into a circular spot, and the spot size is adjustable, and the light intensity can be focused and enhanced by dozens of times, which can be used in catalytic reaction systems. (2) The defective 3DOM LaMn 1.2 O3 can make the most of the full-band solar spectrum. Ultraviolet-a small part of visible light provides high-energy photons and excites the catalyst to produce electron-hole pairs for photocatalytic reaction. Most of the visible-infrared light is absorbed and converted into heat energy, which synergistically strengthens the catalytic reaction and effectively expands the scope of sunlight utilization. The device of the present invention is simple and economical, and realizes the efficient utilization of sunlight. Compared with pure 3DOMLaMn 1.2 O3, defective 3DOM LaMn of the present invention 1.2 O3 has a photothermal synergistic enhancement effect and can be used under low-intensity sunlight (60mW·cm -2 , about 0.6 sun) and a relatively short time, effectively achieving the degradation of volatile organic compounds. Among them, the gas composition: 21vol% O2+79vol% N2, defective 3DOM LaMn 1.2 O3 dosage: 30 mg, mass space velocity: 25600 mL·h -1 ·g -1 Under the above conditions, the toluene conversion rate was 100% and the mineralization rate was 90%. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic structural diagram of an embodiment of the present invention.

[0018] Figure 2 The defective 3DOM LaMn prepared in Example 1 1.2 Scanning electron microscope image of O3 (scales from left to right are 5μm, 1μm, and 500nm).

[0019] Figure 3 The electron paramagnetic resonance images of the catalysts prepared in Example 1 and Comparative Example 1 are shown.

[0020] Figure 4 The X-ray powder diffraction patterns of the catalysts prepared in Example 1 and Comparative Example 1.

[0021] Figure 5 The catalysts prepared in Example 1 and Comparative Example 1 were heated to 60 mW·cm -2 The conversion rate and mineralization rate of toluene change with time under concentrated light irradiation.

[0022] Figure 6 The defective 3DOM LaMn prepared in Example 1 1.2When O3 is used as a catalyst, the sunlight intensity is 60mW·cm -2 Graph showing water resistance under concentrated light irradiation.

[0023] Figure 7 The catalysts prepared in Example 1 and Comparative Example 1 and the commercially available catalyst in Comparative Example 2 were heated to 60 mW·cm -2 A graph showing the change of catalyst surface temperature with time during concentrated photooxidation of toluene under conditions of . DETAILED DESCRIPTION

[0024] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0025] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0026] Example 1

[0027] Defective 3DOM LaMn 1.2 The preparation method of O3 comprises the following steps:

[0028] (1) Preparation of 3DOM LaMn using PMMA colloidal crystal template method 1.2 O3. The specific steps are as follows: at room temperature, measure 10mL of deionized water into a beaker, add 3.976g of La(NO3)3·6H2O, 2.535mL of 50wt% Mn(NO3)2 aqueous solution, and 3.84g of citric acid into the beaker in turn, stir magnetically for 1h, and obtain a transparent precursor solution. Subsequently, 2.0g of PMMA template is completely immersed in the precursor solution for 4.0h, and the excess solution is removed by suction. The obtained solid sample is placed in a vacuum drying oven at 60°C and vacuum dried overnight, and then the sample is transferred to a small porcelain boat, and then placed in a tube furnace for calcination. First, in a nitrogen atmosphere (flow rate of 350 mL / min), the temperature was raised from room temperature to 300 °C at a rate of 1 °C / min, maintained at this temperature for 3 h, and then cooled to room temperature; switched to an air atmosphere (flow rate of 350 mL / min), the temperature was raised from room temperature to 300 °C at a rate of 1 °C / min, maintained at this temperature for 1 h, and then continued to rise from 300 °C to 750 °C at a rate of 1 °C / min, maintained at this temperature for 5 h, and then cooled to room temperature to obtain 3DOM LaMn 1.2 O3.

[0029] (2) The above 3DOM LaMn 1.2O3 undergoes a certain reduction treatment to obtain defective 3DOM LaMn 1.2 O3.

[0030] Comparative Example 1

[0031] Compared with Example 1, the difference is that the catalyst 3DOM LaMn obtained in Example 1 1.2 O3 was used directly as Comparative Example 1 without any treatment.

[0032] Comparative Example 2

[0033] Commercially available Desay P25 was used directly as Comparative Example 2.

[0034] Figure 1 The schematic diagram of the structure of the embodiment of the present invention is mainly composed of three parts: a light source module, a focusing module and a catalytic module.

[0035] Figure 2 (a), (b), and (c) are defective 3DOM LaMn prepared in Example 1 1.2 SEM image of O3. It can be seen from the image that defective 3DOM LaMn 1.2 The three-dimensional macroporous structure of O3 is very regular and orderly, with a pore diameter of about 150nm.

[0036] Figure 3 The electron paramagnetic diagrams of the catalysts prepared in Example 1 and Comparative Example 1 are shown in FIG. As can be seen from the figure, the defective 3DOM LaMn prepared in Example 1 1.2 O3 has a large oxygen defect peak at 2.01, while the comparative example does not have any oxygen defect peak.

[0037] Figure 4 The X-ray powder diffraction patterns of the catalysts prepared in Example 1 and Comparative Example 1 are shown in FIG. 1.2 O3 and the crystal phase is LaMnO 3.08 No MnO was detected. x Related components. 3DOM LaMn prepared in comparative example 1.2 The crystal phase of O3 is LaMnO3, and no MnO is detected. x Related components.

[0038] Test Example 1

[0039] Defective 3DOM LaMn prepared in Example 1 1.2 O3, 3DOM LaMn prepared in Comparative Example 1 1.2O3 and the commercially available P25 of Comparative Example 2 were used as catalysts to catalytically oxidize toluene under daily sunlight. The specific implementation steps are as follows: a certain amount of catalyst is weighed, loaded into a quartz reactor, and a small amount of quartz wool is plugged into the inlet and outlet of the reactor. Gas-phase toluene is introduced into the reactor through a self-built gas path, with an initial toluene reaction concentration of 230ppm and a flow rate of 12.8mL / min. The light source used during the reaction is a PLS-SXE300 xenon lamp (Beijing Bofeilai), and the concentrations of toluene and CO2 during the reaction are detected online by a gas chromatograph.

[0040] Toluene conversion % = 100% × ([toluene] 进口浓度 –[Toluene] 出口浓度 ) / [Toluene] 进口浓度

[0041] Mineralization rate of toluene % = 100% × [CO2] 产生浓度 / [CO2] 理论浓度 =100%×[CO2] 产生浓度 / ([Toluene] 进口浓度 ×7).

[0042] The catalytic activity of different catalysts under sunlight irradiation is shown in Figure 2. Figure 5 As shown in the figure, it can be seen that: 3DOMLaMn 1.2 The O3 catalyst was exposed to sunlight with an intensity of (60 mW·cm -2 ) under the conditions of concentrated light, the conversion rate of toluene was 100% and the mineralization rate was 50%. 1.2 After the introduction of certain defects in O3, the catalytic activity was significantly improved. Specifically, the conversion rate of toluene was 100% and the mineralization rate was 90%. This shows that the defective 3DOM LaMn 1.2 O3 has excellent catalytic activity when used as a catalyst because defects provide reactive sites, which ultimately enhance the catalytic activity.

[0043] Furthermore, the present invention also studies the effect of water vapor on defective 3DOM LaMn 1.2The influence of O3 catalyst on catalytic activity. The experimental method is as follows: the toluene concentration is 230ppm, the reaction space velocity is 25600mL / (gh), the total air flow rate is 12.8mL / min, of which the toluene purge gas is 0.2mL / min, the balance gas is 12.6mL / min, and the balance gas is passed through a steam generator containing water. The relative volume content of water in the reaction gas is ensured by adjusting the temperature of the water in the generator. When the water temperature is 25°C, the corresponding saturated vapor pressure is 3619Pa. According to the formula: relative humidity = actual air water vapor pressure / saturated water vapor pressure at the same temperature. It is calculated that when the water is at 4°C, 16°C and 28°C, the relative humidity of water in the total airflow is 25%, 50% and 100% respectively.

[0044] Figure 6 The defective 3DOM LaMn prepared in Example 1 1.2 O3 is used as a catalyst when the sunlight intensity is 60mW·cm -2 The water resistance stability diagram under concentrated light irradiation. It can be seen from the figure that when the sunlight intensity is 60mW·cm -2 When the relative humidity is zero (i.e., dry air), the conversion rate of toluene is 100% and the yield of CO2 is 88%. When the relative humidity is 50%, the conversion rate of toluene is still 100%, and there is no change within 25 hours, but the yield of CO2 gradually decreases from 88% to 72%. When the relative humidity increases to 100%, the yield of CO2 further decreases from 72% to 68%, and can be maintained for 25 hours. When the relative humidity drops to zero (i.e., dry air), the yield of CO2 can be restored to 88% within 20 hours. The above experimental results show that: although to a certain extent, water vapor and toluene molecules will form competitive adsorption on the catalyst surface and inhibit the catalytic activity of toluene, after switching the water vapor to dry air, the defective 3DOM LaMn 1.2 The catalytic performance of O3 can still be restored. This shows that the defective 3DOM LaMn 1.2 When O3 is used as a catalyst, it has good tolerance to water vapor.

[0045] Test Example 2

[0046] Defective 3DOM LaMn prepared in Test Example 1 1.2 O3, 3DOM LaMn prepared in Comparative Example 1 1.2 O3 and the P25 commercial catalyst of comparative example 2 were subjected to a solar light intensity of 60 mW·cm -2 The change of catalyst surface temperature over time during concentrated photocatalytic oxidation of toluene under the conditions of Figure 7 As shown. Figure 7It can be seen that in the presence of the commercial P25 catalyst (which only absorbs ultraviolet light and does not contribute to light-to-heat conversion) of Comparative Example 2, the solar light intensity is 60 mW·cm -2 Under the conditions of concentrated light irradiation, the temperature of the reaction layer bed only reached 138°C; and when the defective 3DOM LaMn prepared in Example 1 and Comparative Example 1 was used 1.2 O3 and 3DOMLaMn 1.2 When O3 is used as a catalyst, the solar intensity is 60mW·cm -2 Under the concentrated light irradiation, the temperature of the reaction layer bed increased to 218°C. This shows that the defective 3DOM LaMn prepared by the present invention 1.2 O3 and 3DOM LaMn 1.2 As a catalyst, O3 can quickly and efficiently convert absorbed sunlight into thermal energy to provide the temperature required for the reaction system.

Claims

1. A device for photocatalytically oxidizing VOCs using daily solar energy and its application, The method is characterized by comprising the following steps: (1) in the photothermal device, the light source is located above the light window, and the focusing device is a Fresnel lens located between the light source and the light window, which can focus light with an intensity of 50-70 mW / cm 2 Everyday sunlight is concentrated into a circular spot, the size of the spot is adjustable, and the light intensity is focused by more than ten times; (2) In the photothermal device, the photothermal material is a defective three-dimensional macroporous LaMn 1.2 O3 can make sunlight refract and scatter multiple times in perovskite, achieving efficient capture, absorption, and energy conversion of full-spectrum sunlight from ultraviolet to visible to infrared, and providing more active sites; (3) In the photothermal device, the reactor is a microreactor, and a thermocouple is arranged in the reaction chamber.

Citation Information

Patent Citations

  • Attapulgite supported LaMnO3 catalyst for degrading VOCs

    CN109999795A

  • Thermotropic phase-change thermal-control skin based on near-field thermal radiation and application thereof in spacecraft

    CN110079774A

  • Light absorber based on aluminum oxide / lanthanum manganate film-based structure and preparation method thereof

    CN115991610A

  • Thermally enhanced compact reformer

    CN1222256A

  • Manganese oxide-lanthanum manganate perovskite-PGM composites for three-way catalysis

    EP3718627A1

Cited By

  • Method for constructing defect interface in metal oxide by utilizing photo-thermal synergistic strategy and product thereof

    CN121695860A