High and low temperature universal water-based automobile finish paint and preparation method thereof
By adjusting the topcoat formula, using components such as water-based self-crosslinked modified acrylic emulsion, highly reactive amino resin and water-dispersed low-temperature curing and sealed isocyanate, a high and low-temperature universal water-based automotive topcoat coating was designed, which solved the problem of the current situation. In some technology, topcoat cannot adapt to the problem of high-temperature and low-temperature production lines at the same time, and realizes the coating of vehicle body and exterior parts on the same production line at the same time, reducing costs and improving production efficiency.
Patent Information
- Application Number
- CN202411683455.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-22
- Publication Date
- 2025-02-07
AI Technical Summary
In the prior art, automotive topcoats cannot adapt to high and low temperature production lines at the same time, resulting in the need for separate spraying, which increases cost and production complexity.
By adjusting the topcoat formula, using components such as water-based self-crosslinked modified acrylic emulsion, highly reactive amino resin and water-dispersed low-temperature curing and sealed isocyanate, a high and low-temperature universal water-based automotive topcoat coating can be designed in the same way The production line adapts to high and low temperature production needs.
It realizes the coating of the body and exterior parts on the same production line at the same time, reducing costs, improving production efficiency, avoiding the color difference between the two sets of paints with high temperature and low temperature, and is compatible with high temperature and low temperature products, with a wider product window.
Smart Images

Figure CN119391243A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and in particular relates to a high-low temperature universal water-based automobile topcoat coating applied in a 3C1B process production line and a preparation method thereof. Background Art
[0002] In recent years, the automobile industry has developed rapidly, domestic new energy passenger vehicles have developed rapidly, and the production pace of production lines has also become faster and faster. In the production process of the 3C1B process production line, the "three coatings and one baking" process needs to be adopted, and the topcoat needs to meet the comprehensive performance indicators of the paint film of the body and exterior parts at the same time. At present, the body material of the car is metal material, and the material of the exterior parts such as bumpers is plastic. For the metal material car shell topcoat, it is high-temperature baking, corresponding to the high-temperature topcoat, the process is: mid-coat-high-temperature color paint-high-temperature varnish; for the plastic bumper topcoat, it is low-temperature baking, corresponding to the low-temperature topcoat: conductive primer-low-temperature color paint-low-temperature varnish. Therefore, the body and exterior need to be sprayed separately, and two production lines corresponding to high temperature and low temperature are required.
[0003] In response to the current development trend of the automotive industry, the need to reduce costs has arisen, and the need to simultaneously paint the body and exterior parts on a single production line has emerged. In this process, it is very important for coatings, as key products, to adapt to the body and exterior parts in this new process and production line. Summary of the invention
[0004] In response to the above technical problems, the present invention provides a high- and low-temperature universal water-based automotive topcoat coating and a preparation method thereof. By adjusting the formula, the color paint can be adapted to the vehicle body and exterior parts, thereby reducing costs and overcoming the defect that the color paint in the prior art cannot support high and low temperature co-linearity.
[0005] To achieve the above object, the technical solution of the present invention is:
[0006] A high and low temperature general-purpose automobile topcoat coating, comprising the following components by mass fraction:
[0007] 10-20 parts of water-based self-crosslinking modified acrylic emulsion,
[0008] 3-20 parts of water-based hydroxy acrylic resin,
[0009] Acrylic polyurethane copolymer dispersion 0-15 parts,
[0010] 5-15 parts of water-based polyester secondary dispersion,
[0011] 1-5 parts of high-activity amino resin,
[0012] 0-5 parts of water-dispersible low-temperature curing blocked isocyanate;
[0013] The automobile topcoat coating also includes additives, functional additives, solvents and pigments.
[0014] Further preferably, the following components are included according to mass fraction:
[0015] Water-based self-crosslinking modified acrylic emulsion 13-16,
[0016] 4-10 parts of water-based hydroxy acrylic resin,
[0017] Acrylic polyurethane copolymer dispersion 0-9 parts,
[0018] 7 parts of water-based polyester secondary dispersion,
[0019] 3 parts of highly active amino resin,
[0020] 0-3 parts of water-dispersible low-temperature curing blocked isocyanate;
[0021] The automobile topcoat coating also includes additives, functional additives, solvents and pigments.
[0022] Preferably, the additive is selected from: any one of 0.5-2 parts of a wetting agent, 0.2-1 parts of a defoaming agent, 0-1.5 parts of a weathering agent, 0-0.5 parts of a leveling agent, and 1-3 parts of a dispersant, or a mixture thereof;
[0023] The functional additive is selected from: any one of 0-0.5 parts of adhesion promoter, 0-2 parts of pH regulator, 0-5 parts of rheological additive, 0-2 parts of pinhole additive or a mixture thereof;
[0024] The solvent comprises: 5-12 parts of alcohol ether solvent, 3-5 parts of alcohol solvent and 20-40 parts of pure water.
[0025] Preferably, the high-low temperature universal automobile topcoat coating further comprises 15-30 parts of pigment calculated by mass fraction.
[0026] Preferably, the water-based self-crosslinking modified acrylic emulsion is selected from any one or more of the water-based self-crosslinking modified acrylic emulsions of brand AC2742, brand XK14 or brand ROSHIELD 3311;
[0027] The water-based hydroxy acrylic resin is selected from any one or more of brand ROSHIELD 3275, brand Luhydran S938T or self-made hydroxy acrylic resin, and the self-made hydroxy acrylic resin refers to the hydroxy acrylic resin produced by Jinlitai Chemical;
[0028] The acrylic polyurethane copolymer dispersion is selected from any one or more of the acrylic polyurethane copolymer dispersions of the grades DAOTAN TW6466 / 36WA or NeoPac E-123;
[0029] The water-based polyester secondary dispersion is a resin produced by Jinlitai Chemical;
[0030] The highly active amino resin is selected from any one or more of the amino resins of brand MR-625, brand Resimene 717 or brand Cymel325;
[0031] The water-dispersible low-temperature curing blocked isocyanate is selected from brands WM44-L70G, Any one or more of water-dispersible low-temperature curing blocked isocyanate of brand BL-150 or brand BL-8124.
[0032] Preferably, the alcohol ether solvent is selected from any one of ethylene glycol butyl ether, ethylene glycol monohexyl ether, diethylene glycol butyl ether or dipropylene glycol butyl ether, or a mixture thereof; the alcohol solvent is selected from any one of isooctyl alcohol, isopropanol or industrial ethanol, or a mixture thereof; and the pigment is any one or more of Chemours Ti-Pur R706 titanium dioxide or Lomon R996 titanium dioxide.
[0033] Based on the same inventive concept, the present invention also provides a method for preparing a high-low temperature universal water-based automotive topcoat coating, comprising the following steps:
[0034] S1: Add water-based self-crosslinking modified acrylic emulsion, water-based hydroxy acrylate dispersion, acrylic polyurethane copolymer dispersion, water-based polyester secondary dispersion, high-activity amino resin and water-dispersible low-temperature curing blocked isocyanate into the first stirring container in sequence, stably disperse at a speed of 400-800 rpm, and add pH additive to adjust the pH value to 8-9. After stable dispersion, confirm that the fineness is qualified;
[0035] S2: During the stirring process, wetting agent, defoaming agent, weathering agent, leveling agent, adhesion promoter, alcohol ether solvent, alcohol solvent, rheological agent and deionized water are added to the first stirring container in sequence, and the mixture is stirred stably for 60-300 minutes at a speed of 500-1000 rpm, and the fineness is tested to be qualified;
[0036] S3: Add pigment, dispersant, defoamer, and alcohol ether solvent into a second stirring container, stir at a speed of 1500-2000 rpm, and grind until the fineness is qualified for the second time to obtain a slurry;
[0037] S4: adding the slurry obtained in step S3 into the first stirring container at a rotation speed of 500-1000 rpm, stirring stably for 60-300 min, and then checking and adjusting the pH, fineness and viscosity.
[0038] Preferably, the qualified fineness in the preparation method is less than 10 μm.
[0039] Due to the adoption of the above technical solution, the present invention has the following advantages and positive effects compared with the prior art:
[0040] By adjusting the topcoat formula, the present invention can achieve the use of a single paint on both the vehicle body and exterior, allowing co-production, improving the turnover efficiency of the vehicle body and exterior, improving the coating efficiency, saving coating costs, and making full use of production capacity; moreover, the use of the same paint for both the vehicle body and exterior can more easily achieve color stability, avoiding the color difference between the high-temperature and low-temperature paints; reducing product SKUs, facilitating efficient inventory management; and being compatible with both high-temperature and low-temperature products, with a wider product window, which is more conducive to customer construction. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 A (high temperature) vehicle body topcoat coating process provided by an embodiment of the present invention;
[0042] Figure 2 A (low temperature) exterior bumper painting process is provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0043] The present invention aims at the demand of coating the car body and exterior parts on the same production line at the same time, provides a high and low temperature universal water-based automobile topcoat coating, designs a ternary system of self-crosslinking modified acrylic emulsion, high-activity amino resin and low-temperature curing blocked isocyanate, and can coordinate the penetration reaction of the upper and lower coatings to ensure the chemical anchoring between the layers in the film-forming process. The water-based self-crosslinking modified acrylic emulsion itself contains more than two reactive functional groups (hydroxyl, carboxyl, amide, hydroxymethyl, etc.), and when heated to a certain temperature (or a catalyst is added at the same time), the functional groups react with each other to complete crosslinking; the high-activity amino resin (methyl etherified amino resin with high imino group) can be quickly cured without a strong acid catalyst, and can react with polymers containing hydroxyl, amide and carboxyl groups; the low-temperature curing blocked isocyanate is in the coating, uniformly and stably dispersed in the system, at 90-120°C, the blocking agent is opened, and the -NCO functional group begins to be exposed and begins to react with other functional groups.
[0044] Among water-based automotive topcoat resins, water-based self-crosslinking modified acrylic emulsions have the characteristics of rapid film-forming and stable performance. When used with water-based hydroxyl acrylic resins and water-based polyester secondary dispersions that can provide reactive functional groups, the resins are stacked and entangled with each other during flash drying and pre-baking and dehydration. After self-drying and film formation, micro-crosslinking with self-crosslinking resins can strengthen the entanglement between resins, and the exposed functional groups can react and crosslink with amino groups and isocyanates. While each functional group crosslinks with free -NCO and amino groups, it can also crosslink with the functional groups at the interface of the upper and lower layers to form a strong composite coating.
[0045] After the varnish is applied, the isocyanate in the varnish begins to seep down and the reaction starts. After entering the oven, the resin self-crosslinks, amino addition reacts and self-polymerizes, and the upper and lower layers react synergistically. The topcoat has good performance on the car body and bumper.
[0046] Therefore, the present invention provides a cross-linked structure of the coating film in multiple dimensions through water-based self-cross-linking modified acrylic emulsion, high-activity amino resin, water-based hydroxy acrylic resin, water-dispersible low-temperature curing blocked isocyanate, etc., so as to be compatible with high-temperature and low-temperature curing conditions at the same time, thereby meeting the purpose of high- and low-temperature spraying co-line production, thereby improving production efficiency, saving energy and reducing costs.
[0047] The following is a further detailed description of a high and low temperature universal water-based automotive topcoat coating and a preparation method thereof proposed by the present invention in conjunction with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become more apparent from the following description.
[0048] The high-low temperature universal water-based automobile topcoat coating provided by the present invention comprises, by mass fraction, 10-20 parts of water-based self-crosslinking modified acrylic emulsion, 3-20 parts of water-based hydroxy acrylic resin, 0-15 parts of acrylic polyurethane copolymer dispersion, 5-15 parts of water-based polyester secondary dispersion, 1-5 parts of high-activity amino resin, 0-5 parts of water-dispersible low-temperature curing blocked isocyanate, 15-30 parts of pigment, and additives and functional additives, etc.
[0049] The additives include: 0.5-2 parts of wetting agent, 0.2-1 parts of defoaming agent, 0-1.5 parts of weathering agent, 0-0.5 parts of leveling agent, 1-3 parts of dispersant, or any one of them or a mixture thereof;
[0050] Functional additives include: any one of 0-0.5 parts of adhesion promoter, 0-2 parts of pH adjuster, 0-5 parts of rheological additive, 0-2 parts of pinhole additive or a mixture thereof;
[0051] The solvent comprises: 5-12 parts of alcohol ether solvent, 3-5 parts of alcohol solvent and 20-40 parts of pure water.
[0052] The high and low temperature general purpose water-based automotive topcoat coating is prepared by the following preparation method, which specifically includes:
[0053] S1: Add water-based self-crosslinking modified acrylic emulsion, water-based hydroxy acrylate dispersion, acrylic polyurethane copolymer dispersion, water-based polyester secondary dispersion, amino resin and water-dispersible low-temperature curing blocked isocyanate into the first stirring container in sequence, stably disperse at a speed of 400-800 rpm, and add pH additive to adjust the pH value to 8-9. After stable dispersion, confirm that the fineness is less than 10 μm;
[0054] S2: During the stirring process, a wetting agent, a defoaming agent, a stabilizer, a weathering agent, a leveling agent, an adhesion promoter, an alcohol ether solvent, an alcohol solvent, a rheological agent and deionized water are sequentially added to the first stirring container, and the mixture is stirred stably for 60-300 minutes at a speed of 500-1000 rpm, and the fineness is checked to be less than 10 μm;
[0055] S3: Add pigment, dispersant, defoamer and alcohol ether solvent into the second stirring container, stir at a speed of 1500-2000 rpm and grind to obtain slurry after the fineness is qualified twice, and the qualified fineness is less than 10 μm;
[0056] S4: adding the slurry obtained in step S3 into the first stirring container at a rotation speed of 500-1000 rpm, stirring stably for 60-300 min, and then checking and adjusting the pH, fineness and viscosity.
[0057] Example 1
[0058] Table 1 High temperature water-based topcoat process implementation formula
[0059]
[0060]
[0061] Note: Competitor 1 is a high temperature paint standard
[0062] According to the formula in Table 1, topcoats were prepared according to the above preparation method to obtain competitor 1, topcoat 1, topcoat 2 and topcoat 3.
[0063] Table 2: Technical indicators of water-based topcoat original paint in Example 1
[0064]
[0065] use Figure 1 The high temperature coating process shown is to prepare a composite coating by coating the metal plate with a general topcoat prepared according to the formulation in Table 1.
[0066] Table 3: Technical indicators of high temperature water-based topcoat composite coating in Example 1
[0067]
[0068]
[0069]
[0070]
[0071] Example 2
[0072] Table 4 Low temperature water-based topcoat embodiment formula
[0073] Competitor 2 Synthesis example 4 Synthesis example 5 Synthesis example 6 Water-based self-crosslinking modified acrylic emulsion 20 16 13 13 Waterborne hydroxy acrylic resin / 10 4 4 Acrylic polyurethane copolymer dispersion 15 / 9 9 Waterborne polyester secondary dispersion / 7 7 7 Amino resin 1 3 3 3 Water-dispersible low temperature curing blocked isocyanate / / / 3 TEGO Wet 510 wetting agent 0.6 0.6 0.6 0.6 FoamStar ST 2400 Defoamer 0.2 0.2 0.2 0.2 TINUVIN 400 Weathering Agent 0.2 0.2 0.2 0.2 TINUVIN 123 Weathering Agent 0.1 0.1 0.1 0.1 YCK-1110 leveling agent 0.2 0.2 0.2 0.2 LUBRIZOL 2062 Adhesion Promoter / 0.5 0.5 0.5 DMEA dimethylethanolamine 0.4 0.4 0.4 0.4 AQUATIX 8421 rheological additive 0.3 0.3 0.3 0.3 N-5076 Catalyst / 0.01 0.01 0.01 DISPERBYK-190 Dispersant 2 2 2 2 BYKETOL AQ Pinhole Additive 1 1.5 1.5 1.5 Diethylene glycol butyl ether 2 2 2 2 Ethylene glycol monohexyl ether 1 1 1 1 Ethylene glycol butyl ether 5 5 5 2-Ethylhexyl alcohol / 1 1 1 Isopropyl alcohol 2 3 3 3 Dipropylene glycol methyl ether 6 / / / Propylene glycol methyl ether 3 / / / Pure water 25.7 26.69 26.69 23.69 Laponite RD Rheology Additive 0.3 0.3 0.3 0.3 Titanium dioxide 19 19 19 19
[0074] Note: Competitor 2 is a low-temperature topcoat standard
[0075] Using the above-mentioned preparation method, competitor 2 topcoat, topcoat 4, topcoat 5, and topcoat 6 were prepared according to the formula listed in Table 4.
[0076] Table 5 Technical indicators of water-based topcoat original paint in Example 2
[0077]
[0078] use Figure 2 The low temperature coating process shown is to coat the PP plate with a general purpose topcoat prepared according to the formulation in Table 4 to prepare a composite coating.
[0079] Table 6 Technical indicators of low temperature water-based topcoat composite coating of Example 2
[0080]
[0081]
[0082]
[0083]
[0084]
[0085] It can be seen from Tables 3 and 6 that the high and low temperature universal color paint coatings provided in the above embodiments 1 and 2 can well match the corresponding primer, varnish and process under both high temperature process and low temperature process conditions, and have obvious advantages in water resistance, moisture resistance, stone impact resistance and other properties.
[0086] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Even if various changes are made to the present invention, if these changes fall within the scope of the claims of the present invention and their equivalents, they still fall within the protection scope of the present invention.
Claims
1. A high and low temperature general purpose automotive topcoat coating, characterized in that: The components include the following in terms of mass fraction: 10-20 parts of water-based self-crosslinking modified acrylic emulsion, 3-20 parts of water-based hydroxy acrylic resin, Acrylic polyurethane copolymer dispersion 0-15 parts, 5-15 parts of water-based polyester secondary dispersion, 1-5 parts of high-activity amino resin, 0-5 parts of water-dispersible low-temperature curing blocked isocyanate; The automobile topcoat coating also includes additives, functional additives, solvents and pigments.
2. The high and low temperature general purpose automobile topcoat paint according to claim 1, characterized in that: The components include the following in terms of mass fraction: Water-based self-crosslinking modified acrylic emulsion 13-16, 4-10 parts of water-based hydroxy acrylic resin, Acrylic polyurethane copolymer dispersion 0-9 parts, 7 parts of water-based polyester secondary dispersion, 3 parts of high-activity amino resin, 0-3 parts of water-dispersible low-temperature curing blocked isocyanate; The automobile topcoat coating also includes additives, functional additives, solvents and pigments.
3. The high and low temperature general purpose automobile topcoat coating according to claim 1 or 2, characterized in that: The additive is selected from: any one of 0.5-2 parts of a wetting agent, 0.2-1 parts of a defoaming agent, 0-1.5 parts of a weathering agent, 0-0.5 parts of a leveling agent, and 1-3 parts of a dispersant, or a mixture thereof; The functional additive is selected from: any one of 0-0.5 parts of adhesion promoter, 0-2 parts of pH regulator, 0-5 parts of rheological additive, 0-2 parts of pinhole additive or a mixture thereof; The solvent comprises: 3-15 parts of alcohol ether solvent, 1-5 parts of alcohol solvent and 20-40 parts of pure water.
4. The high and low temperature general purpose automobile topcoat paint according to claim 1, characterized in that: The high-low temperature universal automobile topcoat coating also includes 15-30 parts of pigment calculated by mass fraction.
5. The high and low temperature universal automobile topcoat paint according to claim 1 or 2, characterized in that: The water-based self-crosslinking modified acrylic emulsion is selected from any one or more of the water-based self-crosslinking modified acrylic emulsions of brand AC2742, brand XK14 or brand ROSHIELD 3311; The water-based hydroxylated acrylic resin is selected from any one or more of brand ROSHIELD 3275, brand Luhydran S938T or homemade hydroxylated acrylic resin; The acrylic polyurethane copolymer dispersion is selected from any one or more of the acrylic polyurethane copolymer dispersions of the grades DAOTAN TW6466 / 36WA or NeoPac E-123; The water-based polyester secondary dispersion is a homemade resin; The highly active amino resin is selected from any one or more of the amino resins of brand MR-625, brand Resimene 717 or brand Cymel325; The water-dispersible low-temperature curing blocked isocyanate is selected from the brands WM44-L70G, Any one or more of the water-dispersible low-temperature curing blocked isocyanate of brand BL-150 or brand BL-8124.
6. The high and low temperature general purpose automobile topcoat paint according to claim 3, characterized in that: The alcohol ether solvent is selected from any one of ethylene glycol butyl ether, ethylene glycol monohexyl ether, diethylene glycol butyl ether or dipropylene glycol butyl ether, or a mixture thereof; the alcohol solvent is selected from any one of isooctyl alcohol, isopropanol or industrial ethanol, or a mixture thereof; the pigment is any one of Chemours Ti-Pur R706 titanium dioxide or Lomon R996 titanium dioxide.
7. A method for preparing a high-low temperature universal water-based automotive topcoat coating, characterized in that: The following steps are involved: S1: Add water-based self-crosslinking modified acrylic emulsion, water-based hydroxy acrylate dispersion, acrylic polyurethane copolymer dispersion, water-based polyester secondary dispersion, high-activity amino resin and water-dispersible low-temperature curing blocked isocyanate into the first stirring container in sequence, stably disperse at a speed of 400-800 rpm, and add pH additive to adjust the pH value to 8-9. After stable dispersion, confirm that the fineness is qualified; S2: During the stirring process, wetting agent, defoaming agent, weathering agent, leveling agent, adhesion promoter, alcohol ether solvent, alcohol solvent, rheological agent and deionized water are added to the first stirring container in sequence, and the mixture is stirred stably for 60-300 minutes at a speed of 500-1000 rpm, and the fineness is tested to be qualified; S3: Add pigment, dispersant, defoamer, and alcohol ether solvent into a second stirring container, stir at a speed of 1500-2000 rpm, and grind until the fineness is qualified for the second time to obtain a slurry; S4: adding the slurry obtained in step S3 into the first stirring container at a rotation speed of 500-1000 rpm, stirring stably for 60-300 min, and then checking and adjusting the pH, fineness and viscosity.
8. The method for preparing the high and low temperature universal water-based automobile topcoat coating according to claim 7, characterized in that: The qualified fineness in the preparation method is less than 10μm.
Citation Information
Patent Citations
Water-based automobile finish as well as preparation and usage methods thereof
CN104559718A
Glazing-free high-temperature baked finishing coat for sharing bicycle and preparation method thereof
CN107325661A
Water-based flash colored paint and preparation method thereof
CN110229574A
Primer surfacer for automobiles, preparation method and application thereof
CN110669416A
Aqueous coating composition and method for forming coating film
CN113286858A
Cited By
Preparation method and application of high-bird droppings-resistance coating varnish for automobiles
CN121736574A