Flexible micro-beam myocardial tissue contractility sensor based on light curing process and preparation method thereof
A flexible microbeam myocardial tissue contractile force sensor was prepared by photopolymerization process. By combining the flexible microbeam and fiber scaffold, the problems of real-time detection and stiffness mismatch of traditional sensors were solved. This enabled real-time and quantitative detection of myocardial tissue and simulation of the growth environment, improving detection sensitivity and preparation efficiency.
Patent Information
- Application Number
- CN202411588999.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-08
- Publication Date
- 2025-11-18
- Estimated Expiration
- 2044-11-08
AI Technical Summary
Existing myocardial contractility sensing technologies are difficult to achieve real-time, quantitative detection, and the sensor is not compatible with the stiffness of myocardial tissue, affecting myocardial tissue growth and functional assessment.
A flexible microbeam myocardial tissue contractile force sensor was prepared using a photocuring process. The flexible microbeam and fiber scaffold were combined, and a photocurable conductive hydrogel material was used as the sensitive layer. The resistance change was detected by the deformation of the flexible microbeam. The growth environment of myocardial cells was constructed by combining roller electrospinning technology.
It enables real-time and quantitative detection of myocardial contractility. The flexible microbeams are modulated to match myocardial tissue, promoting orderly growth and functional maturation of myocardial tissue. It simplifies the preparation process and improves detection sensitivity.
Smart Images

Figure CN119506082B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cell detection technology, specifically relating to a flexible microbeam myocardial tissue contractility sensor based on photocuring technology and its preparation method. Background Technology
[0002] As a vital organ, the heart supplies blood, nutrients, and oxygen to the entire body through circulatory contractions and relaxations, ensuring normal bodily functions. Myocardial contraction plays a crucial role in maintaining normal cardiac function; its magnitude and frequency are the most direct indicators of myocardial maturity and physiological state, and are also important indicators for assessing whether myocardial function is normal. Therefore, real-time quantitative measurement of parameters such as the magnitude, frequency, and synchronicity of myocardial tissue contractility is of great significance for evaluating the efficacy of drug treatments and establishing models of myocardial disease.
[0003] To rapidly, efficiently, and accurately sense the mechanical behavior of cardiomyocytes and tissues, researchers have developed various physical sensing mechanisms targeting the contractile force of cardiomyocytes. In the field of optical sensing, traditional methods use optical microscopes to observe myocardial tissue contraction, but these methods are inefficient, have low resolution, and cannot quantitatively detect contractile force in real time. In recent years, atomic force microscopy, traction force microscopy, calcium transient, and structural color sensing methods have developed rapidly, showing outstanding performance in terms of spatial resolution and sensitivity. However, they suffer from drawbacks such as high equipment costs, inability to meet high-throughput, long-term detection requirements, and some methods can even cause invasive damage to cells.
[0004] To achieve quantitative, real-time detection of contractile force, researchers have extensively studied electrical sensing methods (such as resistive, piezoelectric, and magnetic sensing). Compared to optical sensing, electrical sensing can monitor changes in the mechanical properties of myocardial tissue in real time by detecting changes in electrical signals. However, its sensitive materials have high modulus and stiffness, which are mismatched with the mechanical properties of myocardial tissue. Furthermore, existing optical and electrical sensors generally use planar cell models, whose structural environment differs significantly from the natural tissue growth environment. These two technical limitations are detrimental to the growth, maturation, and contraction of myocardial tissue, restricting the widespread application of electrical sensing in myocardial chips. Summary of the Invention
[0005] The purpose of this invention is to provide a flexible microbeam myocardial tissue contractile force sensor based on photocuring technology and its preparation method. This invention overcomes the shortcomings of existing sensing methods, such as difficulty in real-time monitoring and stiffness mismatch. The preparation process is simple and fast, and it can realize in-situ real-time detection of the ordered induced growth and contractile performance of myocardial tissue.
[0006] The technical solution of the present invention is as follows:
[0007] A flexible microbeam myocardial tissue contractile force sensor based on photocuring process, wherein the main body of the device is provided with a cell culture chamber, a flexible microbeam and a fiber scaffold;
[0008] The cell culture cavity mentioned above is a hollow structure on the main body of the device;
[0009] The two ends of the aforementioned flexible microbeam are respectively connected to two opposite sidewalls of the aforementioned cell culture chamber. The aforementioned flexible microbeam includes an encapsulation layer and a sensitive layer. The encapsulation layer covers the aforementioned sensitive layer, and the two ends of the aforementioned sensitive layer are exposed outside the encapsulation layer. The encapsulation layer is made of a flexible photocurable resin material, and the aforementioned sensitive layer is made of a photocurable conductive hydrogel material. The Young's modulus of the aforementioned flexible microbeam is 70-250 kPa.
[0010] The fiber scaffold comprises several oriented fibers, one end of which is connected to the sidewall of the cell culture chamber, and the other end of which is perpendicularly connected to the flexible microbeam.
[0011] In the above technical solution, cardiomyocytes are cultured on a fiber scaffold. When the cardiomyocytes beat, they cause the fiber scaffold to deform, thereby causing a change in resistance in the sensitive layer of the flexible microbeam. The change in electrical signal can be measured in real time by an external testing device.
[0012] Preferably, the main body of the device includes a flexible layer and a PCB substrate, wherein the flexible layer is disposed on the PCB substrate;
[0013] The flexible layer is provided with an opening that extends through the thickness direction, and the PCB substrate is provided with a slot that communicates with and is adapted to the opening. The opening and the slot form the cell culture chamber.
[0014] The aforementioned flexible microbeams are formed on the aforementioned flexible layer, which is the aforementioned encapsulation layer, and the aforementioned sensitive layer is electrically connected to the aforementioned PCB substrate.
[0015] In the above technical solution, the PCB substrate is used to bring out the electrical signals of the flexible microbeam.
[0016] More preferably, the flexible microbeam is connected to the middle of the opening and divides the opening into two regions;
[0017] The aforementioned fiber scaffold is disposed on the aforementioned flexible layer, and a plurality of the aforementioned fiber filaments are located in the same aforementioned region and are perpendicular to the length direction of the aforementioned flexible microbeam.
[0018] More preferably, the thickness of the flexible microbeam myocardial tissue contractility sensor is 1.5-3 mm; the cross-sectional length of the flexible microbeam is 0.2-1 mm; the cross-sectional width of the flexible microbeam is 0.3-1 mm; and the length of the flexible microbeam is 5-15 mm.
[0019] More preferably, the above-mentioned flexible photocurable resin material comprises polyurethane acrylate, isodecanyl acrylate, isobornyl acrylate and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 75:55:20:1.
[0020] More preferably, the above-mentioned photocurable conductive hydrogel material comprises acrylamide, polyethylene glycol diacrylate, silver nanowires, and lithium phenyl-2,4,6-trimethylbenzoyl phosphite in a mass ratio of 150:3:5:5.
[0021] More preferably, the raw material of the fiber scaffold includes a biocompatible polymer material, such as at least one of polycaprolactone, polylactic acid and polyimide.
[0022] A method for preparing the above-mentioned flexible microbeam myocardial tissue contractility sensor includes the following steps:
[0023] (1) The above-mentioned flexible layer and the flexible microbeam formed on the above-mentioned flexible layer are printed by photopolymerization process to obtain a flexible layer with flexible microbeams formed thereon.
[0024] (2) A fiber scaffold is prepared by roller electrospinning on the surface of the flexible layer on which the flexible microbeams are formed, to obtain a flexible layer with a flexible microbeam-fiber scaffold composite.
[0025] (3) The flexible layer with the flexible microbeam-fiber support composite is bonded to the PCB substrate, and then the flexible microbeam and the PCB substrate are electrically connected.
[0026] Preferably, the flexible layer includes a flexible substrate layer and a flexible encapsulation layer, wherein the raw materials of the flexible substrate layer and the flexible encapsulation layer are both the flexible photocurable resin material, and the sensitive layer of the flexible microbeam is disposed between the flexible substrate layer and the flexible encapsulation layer.
[0027] The specific operations of step (1) above include the following steps:
[0028] ① The above-mentioned flexible substrate layer was prepared using a photopolymerization printing process;
[0029] ② The above-mentioned sensitive layer is prepared by printing on the above-mentioned flexible substrate using a photopolymerization printing process;
[0030] ③ The above-mentioned flexible encapsulation layer is prepared by printing on the above-mentioned sensitive layer using a photopolymerization printing process;
[0031] ④ Remove the residual flexible photocurable resin material with ethanol to obtain the flexible layer with flexible microbeams. Preferably, the method for removing the residual flexible photocurable resin material with ethanol is to soak for 4-5 hours.
[0032] Preferably, the specific operation of step (2) above includes the following steps:
[0033] ① Dissolve the biocompatible polymer material in an organic solvent and stir until clear to obtain a fiber solution;
[0034] ② The flexible layer with flexible microbeams is attached to the roller, and then the fiber solution is sprayed by electrospinning to obtain a device integrated with a fiber support.
[0035] ③ Remove the device with integrated fiber support from the roller, remove excess fiber filaments, and obtain the flexible layer with flexible microbeam-fiber support composite.
[0036] The extension direction of the aforementioned flexible microbeam is the axial direction of the roller.
[0037] More preferably, the fiber solution is a 20 wt% polycaprolactone acetic acid solution. In other possible implementations, the biocompatible polymer can also be polylactic acid and polyimide, etc., and the organic solvent can be chloroform, hexafluoroisopropanol, methanol, etc.
[0038] More preferably, the flexible layer and the PCB substrate are bonded together with kraft adhesive, and the sensitive layer and the PCB substrate are electrically connected with conductive silver paste.
[0039] The present invention has at least the following beneficial effects:
[0040] 1. This invention uses a photocurable conductive hydrogel material as the sensitive layer material and a flexible photocurable resin material as the encapsulation layer material. The modulus of the printed flexible microbeam is 70-250 kPa, which can achieve modulus matching with myocardial tissue. The deformation of the flexible microbeam adapts to the contraction deformation of myocardial tissue. When the tissue contracts, the deformation of the sensitive layer in the flexible microbeam causes a change in resistance, realizing real-time detection of myocardial tissue contraction force. This overcomes the limitations of traditional electrical sensing methods, such as the mismatch between the stiffness of the microbeam and myocardial tissue and the inability to detect in real time.
[0041] 2. This invention utilizes roller electrospinning technology to integrate an ordered nanofiber membrane onto a flexible layer, serving as a scaffold for culturing cardiomyocytes. This induces anisotropic growth of myocardial tissue, promoting its morphological and functional maturation. The resulting flexible microbeam myocardial tissue contractility sensor more closely resembles the state of real human myocardial tissue, overcoming the limitations of traditional methods that struggle to simulate the natural growth environment of myocardial tissue. This flexible microbeam myocardial tissue contractility sensor achieves integrated culture and sensing functions, showing broad application prospects in drug evaluation and the establishment of cardiac disease models.
[0042] 3. This invention uses photopolymerization 3D printing technology to prepare flexible microbeam layers. The preparation process is simple and enables the rapid preparation of flexible microbeam myocardial tissue contractile force sensors. By adjusting the material composition of the sensitive layer and the encapsulation layer, the preparation efficiency and structural accuracy of the flexible microbeam layers can be further improved. Customized printing of flexible microbeam structures can be achieved, which helps to improve the sensitivity of flexible microbeams and reduce hysteresis, overcoming the limitations of traditional methods such as complex preparation processes, long cycles, and low flexibility. Attached Figure Description
[0043] Figure 1 This is a schematic diagram of the structure of a flexible microbeam myocardial tissue contractile force sensor;
[0044] Figure 2 This is an exploded view of a flexible microbeam myocardial tissue contractile force sensor;
[0045] Figure 3 This is an exploded view of the flexible layer;
[0046] Figure 4 This is a schematic diagram of the fabrication process of a flexible microbeam myocardial tissue contractile force sensor;
[0047] Figure 5 This is a performance test diagram of a flexible microbeam myocardial tissue contractile force sensor.
[0048] Reference numerals: 1-flexible layer, 11-flexible microbeam, 111-sensitive layer, 12-fiber scaffold, 13-opening, 14-flexible substrate layer, 15-flexible encapsulation layer, 2-PCB substrate, 21-PCB board, 211-second opening, 22-glass slide, 23-PCB pad electrode, 24-PCB lead connection hole, 3-cell culture chamber. Detailed Implementation
[0049] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. The following embodiments and drawings are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0050] In this invention, the terms "first," "second," and "third," etc., are used only to distinguish similar objects and are not necessarily used to describe a specific order or sequence, nor should they be construed as indicating or implying relative importance. The use of terms such as "upper," "lower," "left," "right," "front," and "rear" to indicate orientation or positional relationships is based on the orientation or positional relationships shown in the accompanying drawings and is only for the convenience of describing the invention, not to indicate or imply that the device referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, it should not be construed as a limitation on the scope of protection of this invention. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.
[0051] In the following embodiments, the water used can be one or more of distilled water, purified water, and drinking water; unless otherwise specified, the detection methods in the following embodiments are conventional detection methods; unless otherwise specified, the reagents in the following embodiments are all purchased from commercial channels.
[0052] Example 1
[0053] This embodiment provides a flexible microbeam myocardial tissue contractile force sensor (or sensor), the structure of which is as follows: Figures 1-3 As shown.
[0054] like Figure 1 and Figure 2 As shown, the sensor's main body includes a PCB substrate 2 and a flexible layer 1 bonded to the PCB substrate 2. The main body of the sensor includes a cell culture chamber 3, a flexible microbeam 11, and a fiber scaffold 12. The two ends of the flexible microbeam 11 are connected to the two sidewalls of the cell culture chamber 3, respectively. The fiber scaffold 12 includes several oriented fibers, one end of which is connected to the flexible microbeam 11, and the other end is connected to one sidewall of the cell culture chamber 3. The length direction of the fibers is perpendicular to the length direction of the flexible microbeam 11.
[0055] Specifically, the flexible layer 1 has an opening 13 that extends through the thickness direction, and the PCB substrate 2 has a slot that is connected to and adapted to the opening 13. The opening 13 and the slot together constitute the cell culture chamber 3.
[0056] Please see Figure 3 A flexible microbeam 11 is formed at the opening 13 of the flexible layer 1, dividing the opening 13 into two regions. The flexible microbeam 11 has a sensitive layer 111 and an encapsulation layer. The sensitive layer 111 is encapsulated within the encapsulation layer, and both ends of the sensitive layer 111 are exposed from the encapsulation layer to extract signals. In this embodiment, since the flexible microbeam 11 is formed directly on the flexible layer 1, the flexible layer 1 is also the encapsulation layer of the flexible microbeam 11. Further, the sensor thickness is 2 mm, the cross-sectional length of the flexible microbeam 11 is 0.4 mm, the cross-sectional width of the flexible microbeam 11 is 0.5 mm, the length of the flexible microbeam 11 is 6 mm, the length of the flexible layer 1 is 15 mm, the width of the flexible layer 1 is 10 mm, and the width of one region of the opening 13 (i.e., the approximate length of the fiber) is 3.5 mm. In addition, for ease of printing, the flexible layer 1 includes a flexible base layer 14 and a flexible encapsulation layer 15 that are bonded together, and the sensitive layer 111 of the flexible microbeam 11 is disposed between the flexible base layer 14 and the flexible encapsulation layer 15.
[0057] The fiber scaffold 12 is disposed in one of the regions of the opening 13 and is perpendicularly connected to the flexible microbeam 11.
[0058] Back Figure 2The PCB substrate 2 includes a PCB board 21 and a glass slide 22. The lower surface of the PCB board 21 is bonded to the upper surface of the glass slide 22. The PCB board 21 has a second opening 211 that communicates with and is adapted to the opening 13 of the flexible layer 1. The second opening 211 is the sidewall of the slot. The upper surface of the glass slide 22 is partially exposed at the second opening 211, forming the bottom surface of the slot.
[0059] The PCB board 21 is provided with PCB pad electrodes 23 and PCB lead connection holes 24. The sensitive layer 111 of the flexible microbeam 11 is connected to the PCB pad electrodes 23 by conductive silver paste coating, so that the PCB board 21 and the flexible microbeam 11 are electrically connected. The PCB lead connection holes 24 are used to connect external testing equipment such as digital source meters.
[0060] In this embodiment, the flexible layer 1 is obtained by photocuring acrylamide, polyethylene glycol diacrylate, silver nanowires, and lithium phenyl-2,4,6-trimethylbenzoyl phosphite in a mass ratio of 150:3:5:5. The sensitive layer 111 is obtained by photocuring polyurethane acrylate, isodecanyl acrylate, isobornyl acrylate, and 2,4,6-trimethylbenzoyl-diphenylphosphine oxide in a mass ratio of 75:55:20:1. The flexible microbeam 11 obtained by combining the two has a Young's modulus of 164 kPa. In other possible implementations, the flexible layer 1 (or encapsulation layer) can also be prepared using other photocurable conductive hydrogel materials, and the sensitive layer 111 can also be prepared using other flexible photocurable resin materials, as long as the Young's modulus of the flexible microbeam 11 obtained by combining the two is between 70 and 250 kPa.
[0061] The fiber scaffold 12 is prepared by electrospinning using a 20 wt% polycaprolactone acetic acid solution as the fiber filament solution. The flexible layer 1 and the PCB substrate 2 are bonded together using Kaft adhesive.
[0062] The fabrication method of the above sensor is described below, such as... Figure 4 As shown, it includes the following steps:
[0063] (1) The above-mentioned flexible layer and the flexible microbeam formed on the above-mentioned flexible layer are printed by photopolymerization process to obtain a flexible layer with flexible microbeams formed thereon.
[0064] (2) A fiber scaffold is prepared by roller electrospinning on the surface of the flexible layer on which the flexible microbeams are formed, to obtain a flexible layer with a flexible microbeam-fiber scaffold composite.
[0065] (3) The flexible layer with the flexible microbeam-fiber support composite is bonded to the PCB substrate, and then the flexible microbeam and the PCB substrate are electrically connected.
[0066] Step (1) specifically includes the following steps:
[0067] ① The above-mentioned flexible substrate layer is prepared by photopolymerization printing process. The flexible microbeam cross-section length in the substrate layer is 0.4 mm, the cross-section width is 0.2 mm, the total printing layer thickness is 0.2 mm, the slice layer thickness is 0.05 mm, the number of printing layers is 4, and the exposure time is 2.1 s / layer.
[0068] ② The above-mentioned sensitive layer is prepared by printing on the above-mentioned flexible substrate using a photopolymerization printing process. The sensitive layer has a flexible microbeam cross-sectional length of 0.3 mm, a cross-sectional width of 0.2 mm, a total printed layer thickness of 0.2 mm, a slice layer thickness of 0.05 mm, a total of 4 printed layers, and an exposure time of 1.1 s / layer.
[0069] ③ The above-mentioned flexible encapsulation layer is prepared by printing on the above-mentioned sensitive layer using a photopolymerization printing process. The flexible microbeam in the encapsulation layer has a cross-sectional length of 0.4 mm, a cross-sectional width of 0.1 mm, a total printed layer thickness of 0.1 mm, a slice layer thickness of 0.05 mm, a printing layer number of 2 layers, and an exposure time of 2.9 s / layer.
[0070] ④ Soak in ethanol for 4.5 hours to remove residual flexible photocurable resin material, and obtain the flexible layer with flexible microbeams formed.
[0071] Step (2) specifically includes the following steps:
[0072] ① Dissolve the biocompatible polymer material in an organic solvent and stir until clear to obtain a fiber solution;
[0073] ② The flexible layer with flexible microbeams is attached to the roller, and then the fiber solution is sprayed by electrospinning to obtain a device integrated with a fiber support.
[0074] ③ Remove the device with integrated fiber support from the roller, remove excess fiber filaments, and obtain the flexible layer with flexible microbeam-fiber support composite.
[0075] The flexible microbeam extends in the axial direction of the roller, the spinneret is subjected to a voltage of 8kV, the roller is grounded, the relative distance between the roller and the spinneret is 10cm, the fiber solution propulsion speed is 350μL / h, the roller rotation speed is 1800rpm, and the electrospinning time is 8min.
[0076] The working principle of the sensor is explained below:
[0077] In this embodiment, cardiomyocytes are seeded onto a fibrous scaffold. The scaffold can induce anisotropic spreading of the cardiomyocytes, which helps promote their growth and maturation. During cell contraction, the fibrous strands cause deformation of the flexible microbeams, resulting in deformation of the sensitive layer of the microbeams and thus a change in electrical resistance. Subsequently, by measuring the changes in electrical signal using an external device, real-time detection of the contractile force of the myocardial tissue can be achieved. Figure 5 The electrical signal response of the flexible microbeam myocardial tissue contractile force sensor provided in Example 1 under a small strain of 1%-6% is shown, indicating that this sensor has high sensitivity and can meet the testing requirements of myocardial tissue contractile force.
[0078] The above description is merely a preferred embodiment of the present invention, and therefore should not be construed as limiting the scope of the present invention. All equivalent changes and modifications made in accordance with the scope of the patent and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A flexible microbeam myocardial tissue contractility sensor based on a photocuring process, characterized by, The device body is provided with a cell culture cavity, a flexible micro-beam and a fiber scaffold; The cell culture cavity is a cavity structure on the device body; The two ends of the flexible micro-beam are respectively connected with two opposite side walls of the cell culture cavity, the flexible micro-beam comprises an encapsulation layer and a sensitive layer, the encapsulation layer wraps the sensitive layer and the two end portions of the sensitive layer are exposed outside the encapsulation layer, the encapsulation layer is made of a flexible photocurable resin material, the sensitive layer is made of a photocurable conductive hydrogel material, and the Young's modulus of the flexible micro-beam is 70-250 kPa; The fiber scaffold comprises a plurality of directionally arranged fiber filaments, one end of the fiber filaments is connected to the side wall of the cell culture cavity, and the other end of the fiber filaments is connected to the flexible micro-beam perpendicularly; The flexible photocurable resin material comprises polyurethane acrylate, isodecyl acrylate, isobornyl acrylate and 2,4,6-trimethylbenzoyl-diphenyl phosphine oxide in a mass ratio of 75:55:20:1; The photocurable conductive hydrogel material comprises acrylamide, polyethylene glycol diacrylate, silver nanowire and phenyl-2,4,6-trimethylbenzoyl lithium phosphite in a mass ratio of 150:3:5:
5.
2. The flexible micro-ribbon myocardial tissue contractive force sensor of claim 1, wherein, The device body comprises a flexible layer and a PCB substrate, and the flexible layer is arranged on the PCB substrate; The flexible layer is provided with an opening penetrating through in the thickness direction, the PCB substrate is provided with a matching air slot in communication with the opening, and the opening and the air slot form the cell culture cavity; The flexible layer is the encapsulation layer, the flexible layer comprises a flexible base layer and a flexible encapsulation layer, the raw materials of the flexible base layer and the flexible encapsulation layer are the flexible photocurable resin material, the sensitive layer of the flexible micro-beam is arranged between the flexible base layer and the flexible encapsulation layer, and the sensitive layer is electrically connected with the PCB substrate.
3. The flexible micro-ribbon myocardial tissue contractive force sensor of claim 2, wherein, The flexible micro-beam is connected to the middle portion of the opening and divides the opening into two regions; The fiber scaffold is arranged on the flexible layer, and a plurality of fiber filaments are located in the same region and are perpendicular to the length direction of the flexible micro-beam.
4. The flexible micro-ribbon myocardial tissue contractive force sensor of any one of claims 1-3, wherein, The thickness of the flexible micro-beam myocardial tissue contraction force sensor is 1.5-3 mm, the cross-sectional length of the flexible micro-beam is 0.2-1 mm, the cross-sectional width of the flexible micro-beam is 0.3-1 mm, and the length of the flexible micro-beam is 5-15 mm.
5. The flexible micro-ribbon myocardial tissue contractive force sensor of any one of claims 1-3, wherein, The raw material of the fiber scaffold comprises a biocompatible polymer material.
6. A method of manufacturing the flexible micro-rib cardiac muscle tissue contractility sensor according to any one of claims 2-5, characterized in that, The method comprises the following steps: (1) printing the flexible layer and the flexible micro-beam formed on the flexible layer by using a photocuring process to obtain a flexible layer formed with a flexible micro-beam; (2) preparing a fiber scaffold on the surface of the flexible layer formed with a flexible micro-beam by roller electrospinning to obtain a flexible layer with a flexible micro-beam-fiber scaffold composite; (3) bonding the flexible layer with a flexible micro-beam-fiber scaffold composite and a PCB substrate, and then electrically connecting the flexible micro-beam and the PCB substrate.
7. The preparation method of claim 6, wherein The specific operation of step (1) comprises the following steps: ① The flexible substrate layer is prepared using a photopolymerization printing process; ② The sensitive layer is prepared by printing on the flexible substrate using a photopolymerization printing process; ③ The flexible encapsulation layer is prepared by printing on the sensitive layer using a photopolymerization printing process; ④ Remove the residual flexible photocurable resin material with ethanol to obtain the flexible layer with flexible microbeams.
8. The production method according to claim 6 or 7, characterized by, The specific operation of step (2) includes the following steps: ① Dissolve the biocompatible polymer material in an organic solvent and stir until clear to obtain a fiber solution; ② A flexible layer with flexible microbeams is attached to a roller, and then the fiber solution is sprayed by electrospinning to obtain a device integrated with a fiber scaffold. ③ Remove the device with integrated fiber support from the roller, remove excess fiber filaments, and obtain the flexible layer with flexible microbeam-fiber support composite; The flexible microbeam extends in the axial direction of the roller.
Citation Information
Patent Citations
Gelatin hydrogel myocardium bionic scaffold and preparation method thereof
CN104800886A
Myocardial tissue flexible micro-beam force sensor based on liquid metal and array and preparation method thereof