An austenitic stainless steel welded pipe for high-temperature molten salt conveying of a photo-thermal power generation and a manufacturing process thereof

By employing a specific processing technique for TP347H stainless steel plates, the problems of high-temperature tensile strength and grain size requirements for welded pipes used in high-temperature molten salt transportation were solved, thus meeting the operational requirements for high-temperature molten salt transportation in solar thermal power generation and improving the level of domestic production.

CN119525926BActive Publication Date: 2026-11-10JIANGSU WUJIN STAINLESS STEEL PIPE GRP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411625716.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-11-14
Publication Date
2026-11-10
Estimated Expiration
2044-11-14

AI Technical Summary

Technical Problem

Existing technologies cannot meet the requirements for high-temperature tensile testing, base material grain size, and weld ferrite in austenitic stainless steel welded pipes used for high-temperature molten salt transportation at 575℃, resulting in insufficient import quantities and long import cycles, which restricts the development of solar thermal power generation technology.

Method used

Using TP347H stainless steel plates with a specific grain size, the welding heat input and interpass temperature are controlled through processes such as ultrasonic inspection, edge planing, forming, spot welding, welding, solution heat treatment and rotary furnace heat treatment to ensure that the grain size of the base material is between 4 and 7 and the yield strength of the tensile test at 575℃ is not less than 131MPa.

Benefits of technology

The prepared stainless steel welded pipe meets the operating requirements of high-temperature molten salt transportation in solar thermal power generation, and achieves optimization of high-temperature tensile testing and base material grain size, thus improving the level of domestic production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application belongs to the field of stainless steel welded pipe production, and particularly discloses an austenitic stainless steel welded pipe for high-temperature molten salt conveying in a photo-thermal power generation and a manufacturing process. The grain size of the raw material is required, and the heat treatment temperature and holding time are controlled, so that the grain size of the finished product meets the requirement of 4-7 levels. Higher requirements are proposed for the control of the welding heat input and the interlayer temperature. The final normal temperature tensile test (tensile strength ≥515MPa, yield strength ≥205MPa, and elongation after fracture ≥40%), the bending test (no cracks and other defects after bending, and the bending test is qualified), the hardness test (hardness value ≤92HRB), the 575℃ high-temperature tensile test (yield strength ≥131MPa), and the ferrite content FN of the weld before post-weld heat treatment (3-10) are all met. The stainless steel welded pipe for high-temperature molten salt conveying in the photo-thermal power generation meets the working condition requirement of the high-temperature molten salt pipeline in the photo-thermal power generation, and is also applicable to different specifications of stainless steel welded pipes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of stainless steel welded pipes, and specifically to a manufacturing process for austenitic stainless steel welded pipes used for high-temperature molten salt transportation in solar thermal power generation. Background Technology

[0002] With the introduction of the "dual carbon" target, my country's power generation capacity structure is facing tremendous changes, making the construction of a new power system based on new energy sources an urgent priority. In recent years, with the completion and grid connection of the first batch of solar thermal power generation demonstration projects, my country's solar thermal power generation technology has matured. With the development of solar thermal technology and the rapid growth of installed capacity in my country, the market demand for welded pipes for high-temperature molten salt transportation will also grow rapidly, reaching a very large volume. In addition to the conventional performance requirements such as room temperature tensile testing, bending testing, hardness testing, and radiographic inspection, austenitic stainless steel welded pipes for high-temperature molten salt transportation must also meet the requirements for 575℃ high-temperature tensile testing, base metal grain size, and weld ferrite (before post-weld heat treatment). Compared to traditional austenitic stainless steel welded pipe production processes, such as the manufacturing method of CN202110771391.7 austenitic stainless steel pipes for LNG transportation;

[0003] CN202110771392.1 Method for manufacturing composite welded austenitic stainless steel pipe for fluid transportation;

[0004] CN202010919711.4 The manufacturing process of stainless steel welded pipes for marine oil and gas transportation. These processes are applicable to the manufacturing of products under different working conditions. The above three are respectively applicable to the transportation of liquefied natural gas, ordinary fluids and marine oil and gas under low temperature conditions. They cannot meet the transportation requirements of high temperature molten salt under high temperature conditions. Stainless steel welded pipes for high temperature molten salt need to meet the requirements of high temperature tensile strength, base material grain size and weld ferrite (before post-weld heat treatment). The welding process and solution heat treatment have a greater impact on performance.

[0005] Given the numerous uncertainties in the international environment, the insufficient import quantity and long import cycle of welded pipes for high-temperature molten salt transportation have become key factors restricting the development of concentrated solar power (CSP) technology. As a crucial component of CSP generator sets, the "welded pipe for high-temperature molten salt transportation in CSP" urgently needs to be completely domestically produced. This invention has the following characteristics compared to traditional processes: ① Traditional processes do not have grain size requirements, while this process specifies grain size requirements for raw materials and controls the temperature and holding time during heat treatment to ensure that the grain size of the finished welded pipe base material meets the requirements of grade 4-7. ② To meet the testing requirements of molten salt conditions, the welding process of the pipe weld seam differs from that of traditional pipe welding processes in terms of welding heat input and interpass temperature control. ③ A different heat treatment method is selected than that of traditional pipes, reducing or avoiding deformation such as pipe collapse due to its own gravity. Rotary furnace heat treatment is preferred, meaning the pipe rotates forward, keeping its center constantly changing. ④ The pipe finally prepared by this invention is used in high-temperature molten salt conditions, meeting the 575℃ high-temperature tensile test requirement that traditional processes cannot meet. Summary of the Invention

[0006] To address the aforementioned issues, this invention provides a manufacturing process for austenitic stainless steel welded pipes used in high-temperature molten salt transportation for solar thermal power generation, meeting the requirements for use in high-temperature molten salt conditions.

[0007] The technical solution adopted in this invention includes the following steps:

[0008] a. Raw material requirements: Plate grain size 6-8.5; TP347H is selected for austenitic stainless steel welded pipes used for molten salt transportation in solar thermal power generation.

[0009] b. Ultrasonic testing of the boards: After the boards pass the ultrasonic testing, they should be labeled and stacked in the designated location;

[0010] c. Sheet metal edge planing: The cutting speed is 5-8 m / min, and the cutting amount is controlled to not exceed 0.5 mm per pass. When the sheet metal thickness is not greater than 9 mm, the sheets can be stacked and pressed, but the total thickness after stacking should not exceed 9 mm. Different types of beveling are processed according to different sheet metal thicknesses: I-type beveling for sheet metal thickness ≤ 9 mm; Y-type beveling for sheet metal thickness ≤ 28 mm with a blunt edge of 4-6 mm and a beveling angle of 65-70°; X-type beveling for sheet metal thickness > 28 mm with a blunt edge of 3-5 mm and a beveling angle of 60-65°. The surface roughness of the planed edge should not exceed Ra 6.3 μm.

[0011] d. Sheet forming: The bending forming process is adopted. The bent tubes are not allowed to have obvious creases after visual inspection. The distance between the openings is controlled within 50-100mm.

[0012] e. Shaping and spot welding: The formed open pipe is spot welded in a seam closing machine. The spot welding adopts manual argon arc welding process, the welding current is 100-160A, the weld length is 5-10mm, and the distance between each weld is 195-205mm.

[0013] f. Pipe welding: For pipe thicknesses between 2mm and 12mm, use plasma welding + argon arc welding; for pipe thicknesses between 12mm and 28mm, use plasma welding + submerged arc welding + argon arc welding; for pipe thicknesses greater than 28mm, use plasma welding + submerged arc welding.

[0014] The heat input for plasma welding shall not exceed 1.5 KJ / mm, the heat input for argon arc welding shall not exceed 1.4 KJ / mm, and the heat input for submerged arc welding shall not exceed 2.4 KJ / mm. Heat input (KJ / mm) = welding current (A) * welding voltage (V) / welding speed (mm / min) * 0.06. The interpass temperature shall not exceed 120℃.

[0015] g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner, which reduces or avoids deformation such as tube collapse caused by its own weight in thin-walled tubes. The heat treatment temperature is 1080℃~1130℃, and the holding time is min: tube wall thickness * (1~2), where tube wall thickness is in mm; weld ferrite (before post-weld heat treatment) FN: 3~10.

[0016] For plasma welding of the root pass, a back shielding gas is required, ensuring the oxygen content on the back side does not exceed 500 ppm. An argon-hydrogen mixture is used as the ionizing gas in plasma welding to increase welding speed. In plasma welding, the ionizing gas is 93% Ar + 7% H2, with a flow rate of 3–8 L / min; the gun shielding gas is 99.99% Ar, with a flow rate of 10–25 L / min; the tail shielding gas is 99.99% Ar, with a flow rate of 15–22 L / min; and the back shielding gas is 99.99% Ar, with a flow rate of 20–30 L / min. In argon arc welding, the gun shielding gas is 93% Ar + 7% H2, with a flow rate of 10–25 L / min; and the tail shielding gas is 99.99% Ar, with a flow rate of 15–22 L / min.

[0017] h. Straightening: During the straightening process, pay close attention to the surface quality of the pipe to prevent dents. After straightening, the straightness should not exceed 1mm / m.

[0018] i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray.

[0019] j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm;

[0020] k. Pickling and passivation: Immerse the pipe in a tank containing a mixed solution of nitric acid, hydrofluoric acid, and water for pickling and passivation. The volume ratio of nitric acid to hydrofluoric acid is 10%–13% and 5%–7%, respectively. Rinse thoroughly after removal from the tank. l. Finished product inspection: Tensile test at room temperature (tensile strength ≥ 515 MPa, yield strength ≥ 205 MPa, elongation after fracture ≥ 40%), bending test (if there are no cracks or other defects after bending, the bending test is qualified), hardness test (hardness value ≤ 92 HRB), base material grain size grade 4–7, and yield strength of not less than 131 MPa in the 575℃ high temperature tensile test.

[0021] Compared with existing technologies, the advantages of this invention are as follows: By setting the welding process for the pipe weld, especially controlling the welding heat input and interpass temperature, the resulting product has a base material grain size within the range of 4 to 7, a yield strength of not less than 131 MPa in a 575℃ high-temperature tensile test, and meets the requirements for room temperature tensile tests and bending tests. Therefore, the prepared stainless steel welded pipe for high-temperature molten salt transportation in solar thermal power generation meets the high-temperature operating requirements of molten salt pipelines in solar thermal power generation. Detailed Implementation

[0022] Example 1

[0023] Welded pipe material TP347H, product specifications Its manufacturing method includes the following steps:

[0024] a. Raw material requirements: Plate grain size grade 6-7;

[0025] b. Ultrasonic testing of the boards: After the boards pass the ultrasonic testing, they should be labeled and stacked in the designated location;

[0026] c. Sheet metal edge planing: Cutting speed is 7.5 m / min, and the cutting depth is controlled at 0.5 mm per pass. Type I bevel is machined; the surface roughness of the planed edge is Ra 3.2 μm.

[0027] d. Sheet forming: The bending forming process is adopted. The bent tubes are not allowed to have obvious creases after visual inspection. The distance between the openings is controlled between 60 and 100 mm.

[0028] e. Shaping and spot welding: The formed open pipe is spot welded in a seam closing machine. The spot welding adopts manual argon arc welding process, the welding current is 100-120A, the weld length is 5-10mm, and the distance between each weld is 195-205mm.

[0029] f. Pipe Welding: ① Plasma welding + TIG welding process is adopted. ② For the root pass plasma welding, a back shielding gas is required, and the oxygen content on the back side must not exceed 500 ppm. ③ In plasma welding, the plasma gas is 93% Ar + 7% H2, with a gas flow rate of 5 L / min; the gun shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; and the back shielding gas is 99.99% Ar, with a gas flow rate of 25 L / min. In TIG welding, the gun shielding gas is 93% Ar + 7% H2, with a gas flow rate of 16 L / min; and the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min. ④ The heat input for plasma welding is 1.2 KJ / mm, and the heat input for TIG welding is 1.1 KJ / mm. Heat input (KJ / mm) = welding current (A) * welding voltage (V) / welding speed (mm / min) * 0.06. ⑤ The interpass temperature during welding should not exceed 70℃;

[0030] g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner, which reduces or avoids deformation such as tube collapse caused by its own weight. The heat treatment temperature is 1100℃ and the holding time is 9min; h. Straightening: During the straightening process, the surface quality of the tube is constantly monitored to prevent pitting. The straightness after straightening is 0.9mm / m.

[0031] i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray.

[0032] j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm;

[0033] k. Pickling and passivation: Immerse the tube in a tank containing a mixed solution of nitric acid, hydrofluoric acid and water for pickling and passivation. The volume percentages of nitric acid and hydrofluoric acid are 10%–13% and 5%–7%, respectively. Rinse thoroughly after removing from the tank.

[0034] 1. Finished Product Inspection: The product passed the room temperature tensile test (tensile strength 669 MPa, yield strength 351 MPa, elongation after fracture 51%), the bending test (no cracks or other defects after bending), and the hardness test (hardness values: base metal 79 HRB, heat-affected zone 82 HRB, weld 80 HRB). The base metal grain size was 4.5–6. The yield strength in the 575℃ high-temperature tensile test was 149 MPa. The weld ferrite (before post-weld heat treatment) FN was 5.3, meeting the performance requirements. The room temperature tensile test, bending test, and hardness test were conducted according to ASTM A370; the base metal grain size according to ASTM E112; the high-temperature tensile test according to ASTM E21; and the weld ferrite according to ISO 8249.

[0035] Example 2

[0036] Welded pipe material TP347H, product specifications Its manufacturing method includes the following steps:

[0037] a. Raw material requirements: Grain size of the board material must be 6-7.5.

[0038] b. Ultrasonic testing of the boards: After the boards pass the ultrasonic testing, they should be labeled and stacked in the designated location;

[0039] c. Plate edge planing: Cutting speed is 6.5 m / min, and the cutting amount is controlled at 0.5 mm per pass. Type I bevel is machined; the surface roughness of the planed edge is Ra 3.2 μm.

[0040] d. Sheet forming: The bending forming process is adopted. The bent tubes are not allowed to have obvious creases after visual inspection. The distance between the openings is controlled between 50 and 90 mm.

[0041] e. Shaping and spot welding: The formed open pipe is spot welded in a seam closing machine. The spot welding adopts manual argon arc welding process, the welding current is 100-120A, the weld length is 5-10mm, and the distance between each weld is 195-205mm.

[0042] f. Pipe Welding: ① The process uses plasma welding + submerged arc welding + argon arc welding. ② For the root pass plasma welding, a back shielding gas is required, and the oxygen content on the back side must not exceed 500 ppm. ③ In plasma welding, the plasma gas is 93% Ar + 7% H2, with a gas flow rate of 6.5 L / min; the gun shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; and the back shielding gas is 99.99% Ar, with a gas flow rate of 25 L / min. In argon arc welding, the gun shielding gas is 93% Ar + 7% H2, with a gas flow rate of 18 L / min; and the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min. ④ The heat input for plasma welding is 1.4 KJ / mm, for submerged arc welding it is 2.1 KJ / mm, and for argon arc welding it is 1.0 KJ / mm. Heat input (KJ / mm) = welding current (A) * welding voltage (V) / welding speed (mm / min) * 0.06. ⑤ The interpass temperature should not exceed 100℃.

[0043] g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner, which reduces or avoids deformation such as tube collapse caused by its own weight. The heat treatment temperature is 1100℃ and the holding time is 14min; h. Straightening: During the straightening process, the surface quality of the tube should be monitored at all times to prevent pitting. The straightness after straightening is 1.0mm / m.

[0044] i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray.

[0045] j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm;

[0046] k. Pickling and passivation: Immerse the pipes in a tank containing a mixed solution of nitric acid, hydrofluoric acid, and water for pickling and passivation. The volume ratio of nitric acid to hydrofluoric acid is 10%–13% and 5%–7%, respectively. Rinse thoroughly after removal from the tank. l. Finished product inspection: Pass the room temperature tensile test (tensile strength 683 MPa, yield strength 354 MPa, elongation after fracture 48%), pass the bending test (no cracks or other defects after bending), pass the hardness test (hardness value: base material 77 HRB, heat-affected zone 80 HRB, weld 78 HRB), base material grain size 5–6, 575℃ high-temperature tensile test yield strength 143 MPa, weld ferrite (before post-weld heat treatment) FN: 7.3, meeting performance requirements. The room temperature tensile test, bending test, and hardness test are performed according to standard ASTM A370; the base material grain size is performed according to ASTM E112; the high-temperature tensile test is performed according to standard ASTM E21; and the weld ferrite is performed according to standard ISO 8249.

[0047] Comparative Example 1

[0048] The main difference between Comparative Example 1 and Example 1 is that the heat treatment holding time is not within the range of "pipe wall thickness mm * (1 ~ 2) min", while other operations are the same.

[0049] Welded pipe material TP347H, product specifications Its manufacturing method includes the following steps:

[0050] a. Raw material requirements: Plate grain size grade 6-7;

[0051] b. Ultrasonic testing of the boards: After the boards pass the ultrasonic testing, they should be labeled and stacked in the designated location;

[0052] c. Sheet metal edge planing: Cutting speed is 7.5 m / min, and the cutting depth is controlled at 0.5 mm per pass. Type I bevel is machined; the surface roughness of the planed edge is Ra 3.2 μm.

[0053] d. Sheet forming: The bending forming process is adopted. The bent tubes are not allowed to have obvious creases after visual inspection. The distance between the openings is controlled between 60 and 100 mm.

[0054] e. Shaping and spot welding: The formed open pipe is spot welded in a seam closing machine. The spot welding adopts manual argon arc welding process, the welding current is 100-120A, the weld length is 5-10mm, and the distance between each weld is 195-205mm.

[0055] f. Pipe Welding: ① Plasma welding + TIG welding process is adopted. ② For the root pass plasma welding, a back shielding gas is required, and the oxygen content on the back side must not exceed 500 ppm. ③ In plasma welding, the plasma gas is 93% Ar + 7% H2, with a gas flow rate of 5 L / min; the gun shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; and the back shielding gas is 99.99% Ar, with a gas flow rate of 25 L / min. In TIG welding, the gun shielding gas is 93% Ar + 7% H2, with a gas flow rate of 16 L / min; and the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min. ④ The heat input for plasma welding is 1.2 KJ / mm, and the heat input for TIG welding is 1.1 KJ / mm. Heat input (KJ / mm) = welding current (A) * welding voltage (V) / welding speed (mm / min) * 0.06. ⑤ The interpass temperature during welding should not exceed 70℃;

[0056] g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner to reduce deformation such as tube collapse caused by its own weight. The heat treatment temperature is 1100℃ and the holding time is 20min.

[0057] h. Straightening: During the straightening process, pay close attention to the surface quality of the pipe to prevent dents. After straightening, the straightness should be 1.0 mm / m.

[0058] i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray.

[0059] j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm;

[0060] k. Pickling and passivation: The pipe is immersed in a tank containing a mixed solution of nitric acid, hydrofluoric acid, and water for pickling and passivation. The volume percentages of nitric acid and hydrofluoric acid are 10%–13% and 5%–7%, respectively. After removal from the tank, the pipe is rinsed clean. l. Finished product inspection: The pipe passes the room temperature tensile test (tensile strength 563 MPa, yield strength 244 MPa, elongation after fracture 57%), the bending test (no cracks or other defects after bending), the hardness test (hardness value: base material 73 HRB, heat-affected zone 74 HRB, weld 74 HRB), the base material grain size is 3.5–5.5, the yield strength of the 575℃ high temperature tensile test is 127 MPa, and the weld ferrite (before post-weld heat treatment) FN: 5.7. The performance does not meet the high-temperature operating requirements of molten salt pipes in solar thermal power generation. The room temperature tensile test, bending test, and hardness test are performed according to ASTM A370, the grain size of the base material is performed according to ASTM E112, the high temperature tensile test is performed according to ASTM E21, and the weld ferrite is performed according to ISO 8249.

[0061] If the heat preservation time of Comparative Example 1 is 5 minutes, which is lower than the lower limit, the tube may fail the room temperature tensile test and hardness test, and thus fail to meet the production process requirements.

[0062] Comparative Example 2

[0063] The difference between Comparative Example 2 and Example 1 is that the grain size of the plate is not within the "6-8.5" range. The welded pipe material is TP347H, and the product specifications are... Its manufacturing method includes the following steps:

[0064] a. Raw material requirements: Plate grain size grade 5-6;

[0065] b. Ultrasonic testing of the boards: After the boards pass the ultrasonic testing, they should be labeled and stacked in the designated location;

[0066] c. Sheet metal edge planing: Cutting speed is 7.5 m / min, and the cutting depth is controlled at 0.5 mm per pass. Type I bevel is machined; the surface roughness of the planed edge is Ra 3.2 μm.

[0067] d. Sheet forming: The bending forming process is adopted. The bent tubes are not allowed to have obvious creases after visual inspection. The distance between the openings is controlled between 60 and 100 mm.

[0068] e. Shaping and spot welding: The formed open pipe is spot welded in a seam closing machine. The spot welding adopts manual argon arc welding process, the welding current is 100-120A, the weld length is 5-10mm, and the distance between each weld is 195-205mm.

[0069] f. Pipe Welding: ① Plasma welding + TIG welding process is adopted. ② For the root pass plasma welding, a back shielding gas is required, and the oxygen content on the back side must not exceed 500 ppm. ③ In plasma welding, the plasma gas is 93% Ar + 7% H2, with a gas flow rate of 5 L / min; the gun shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; and the back shielding gas is 99.99% Ar, with a gas flow rate of 25 L / min. In TIG welding, the gun shielding gas is 93% Ar + 7% H2, with a gas flow rate of 16 L / min; and the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min. ④ The heat input for plasma welding is 1.2 KJ / mm, and the heat input for TIG welding is 1.1 KJ / mm. Heat input (KJ / mm) = welding current (A) * welding voltage (V) / welding speed (mm / min) * 0.06. ⑤ The interpass temperature during welding should not exceed 70℃;

[0070] g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner, which reduces or avoids deformation such as tube collapse caused by its own weight. The heat treatment temperature is 1100℃ and the holding time is 9min; h. Straightening: During the straightening process, the surface quality of the tube is constantly monitored to prevent pitting. The straightness after straightening is 0.9mm / m.

[0071] i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray.

[0072] j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm;

[0073] k. Pickling and passivation: Immerse the tube in a tank containing a mixed solution of nitric acid, hydrofluoric acid and water for pickling and passivation. The volume percentages of nitric acid and hydrofluoric acid are 10%–13% and 5%–7%, respectively. Rinse thoroughly after removing from the tank.

[0074] 1. Finished Product Inspection: The following parameters are required: Passing the room temperature tensile test (tensile strength 661 MPa, yield strength 343 MPa, elongation after fracture 49%), passing the bending test (no cracks or other defects after bending), passing the hardness test (hardness values: base metal 81 HRB, heat-affected zone 84 HRB, weld 83 HRB), base metal grain size 3.5–4.5, yield strength at 575℃ tensile test 134 MPa, weld ferrite (before post-weld heat treatment) FN: 5.9. The room temperature tensile test, bending test, and hardness test are conducted according to ASTM A370; the base metal grain size is conducted according to ASTM E112; the high-temperature tensile test is conducted according to ASTM E21; and the weld ferrite is conducted according to ISO 8249.

[0075] Comparative Example 2: The grain size of the base material in the finished product inspection did not meet the requirements.

[0076] Comparative Example 3

[0077] Compared with Example 1, Comparative Example 3 differs in that the welding heat input is not within the range of "the heat input of plasma welding does not exceed 1.5 KJ / mm and the heat input of argon arc welding does not exceed 1.4 KJ / mm".

[0078] Welded pipe material TP347H, product specifications Its manufacturing method includes the following steps:

[0079] a. Raw material requirements: Plate grain size grade 6-7;

[0080] b. Ultrasonic testing of the boards: After the boards pass the ultrasonic testing, they should be labeled and stacked in the designated location;

[0081] c. Sheet metal edge planing: Cutting speed is 7.5 m / min, and the cutting depth is controlled at 0.5 mm per pass. Type I bevel is machined; the surface roughness of the planed edge is Ra 3.2 μm.

[0082] d. Sheet forming: The bending forming process is adopted. The bent tubes are not allowed to have obvious creases after visual inspection. The distance between the openings is controlled between 60 and 100 mm.

[0083] e. Shaping and spot welding: The formed open pipe is spot welded in a seam closing machine. The spot welding adopts manual argon arc welding process, the welding current is 100-120A, the weld length is 5-10mm, and the distance between each weld is 195-205mm.

[0084] f. Pipe Welding: ① Plasma welding + TIG welding process is adopted. ② For the root pass plasma welding, a back shielding gas is required, and the oxygen content on the back side must not exceed 500 ppm. ③ In plasma welding, the plasma gas is 93% Ar + 7% H2, with a gas flow rate of 5 L / min; the gun shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min; and the back shielding gas is 99.99% Ar, with a gas flow rate of 25 L / min. In TIG welding, the gun shielding gas is 93% Ar + 7% H2, with a gas flow rate of 16 L / min; and the tail shielding gas is 99.99% Ar, with a gas flow rate of 20 L / min. ④ The heat input for plasma welding is 1.7 KJ / mm, and the heat input for TIG welding is 1.6 KJ / mm. Heat input (KJ / mm) = welding current (A) * welding voltage (V) / welding speed (mm / min) * 0.06. ⑤ The interpass temperature during welding should not exceed 70℃;

[0085] g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner, which reduces or avoids deformation such as tube collapse caused by its own weight. The heat treatment temperature is 1100℃ and the holding time is 9min; h. Straightening: During the straightening process, the surface quality of the tube is constantly monitored to prevent pitting. The straightness after straightening is 0.9mm / m.

[0086] i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray.

[0087] j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm;

[0088] k. Pickling and passivation: Immerse the tube in a tank containing a mixed solution of nitric acid, hydrofluoric acid and water for pickling and passivation. The volume percentages of nitric acid and hydrofluoric acid are 10%–13% and 5%–7%, respectively. Rinse thoroughly after removing from the tank.

[0089] 1. Finished Product Inspection: The following parameters are required: Passing the room temperature tensile test (tensile strength 607 MPa, yield strength 319 MPa, elongation after fracture 50%), passing the bending test (no cracks or other defects after bending), passing the hardness test (hardness values: base metal 79 HRB, heat-affected zone 81 HRB, weld 81 HRB), base metal grain size 4.5–6, yield strength at 575℃ tensile test 122 MPa, weld ferrite (before post-weld heat treatment) FN: 11.4. The high-temperature tensile test and weld ferrite do not meet the requirements. The room temperature tensile test, bending test, and hardness test are performed according to ASTM A370; the base metal grain size is performed according to ASTM E112; the high-temperature tensile test is performed according to ASTM E21; and the weld ferrite is performed according to ISO 8249.

[0090] Comparative Example 3: The yield strength and weld ferrite of the finished product tested at 575℃ did not meet the requirements, and the weld defects were more numerous than in the Example 3 when X-ray inspection was performed on the pipe weld.

[0091] Further research on the parameters in the pipe welding process showed that if the heat input of plasma welding alone does not meet the range requirements (e.g., heat input of plasma welding is 1.7 KJ / mm) or if the heat input of argon arc welding alone does not meet the requirements (e.g., heat input of argon arc welding is 1.6 KJ / mm), the finished product cannot meet the requirements of the high temperature tensile test. The test results are similar to those of Comparative Example 3.

Claims

1. A manufacturing process for austenitic stainless steel welded pipes used for high-temperature molten salt transport in solar thermal power generation, characterized in that... Includes the following steps: a. Raw material requirements: Stainless steel sheet with a grain size of 6~8.5; Stainless steel sheet grade TP347H; b. Ultrasonic testing of the board material: The board material is tested using ultrasonic waves; c. Sheet metal edge planing: The cutting speed for edge planing is 5~8m / min, and the cutting amount is controlled to not exceed 0.5mm in a single pass; the surface roughness of the planed edge is required to be no greater than Ra6.3μm; d. Sheet forming: The bending forming process is adopted, and the distance at the opening is controlled within 50~100mm; e. Shaping and spot welding: The formed open pipe is spot welded in a seam sealing machine. The spot welding adopts manual argon arc welding process, with a weld length of 5~10mm and a distance of 195~205mm between each weld. f. Pipe welding: For pipe thicknesses between 2mm and 12mm, plasma welding + TIG welding is used; for pipe thicknesses between 12mm and 28mm, plasma welding + submerged arc welding + TIG welding is used; for pipe thicknesses greater than 28mm, plasma welding + submerged arc welding is used. The heat input for plasma welding should not exceed 1.5KJ / mm, the heat input for TIG welding should not exceed 1.4KJ / mm, and the heat input for submerged arc welding should not exceed 2.4KJ / mm. The ferrite number (FN) of the weld after welding should be 3~10. Plasma welding is used for the root pass in all pipe welding processes. A back shielding gas is required for the root pass plasma welding, and the oxygen content on the back pass should not exceed 500ppm. The interpass temperature should not exceed 120℃. g. Solution heat treatment: Heat treatment is carried out in a rotary solution furnace. The tube advances in a rotating manner. The heat treatment temperature is 1080℃~1130℃. The holding time is min = tube wall thickness * (1~2). The tube wall thickness is in mm. h. Straightening: After straightening, the straightness should not exceed 1mm / m; i. Water pressure and non-destructive testing: Each pipe is subjected to a water pressure test, and the welds of the pipes are inspected by X-ray. j. Pipe end beveling: Beveling both ends of the pipe on a beveling machine with a beveling angle of 37.5°±2.5° and a blunt edge of 1.6mm±0.8mm; k. Pickling and passivation: Immerse the tube in a tank containing a mixed solution of nitric acid, hydrofluoric acid and water for pickling and passivation. The volume percentages of nitric acid and hydrofluoric acid are 10%~13% and 5%~7%, respectively. Rinse thoroughly after removing from the tank. l. Finished product inspection.

2. The manufacturing process of the austenitic stainless steel welded pipe for high-temperature molten salt transportation in solar thermal power generation according to claim 1, characterized in that, In step c, the board edge planing process, when the board thickness is no more than 9mm, the boards are stacked and pressed, but the total thickness after stacking does not exceed 9mm; different types of bevels are processed according to different board thicknesses: for board thickness ≤ 9mm, an I-type bevel is used; for 9mm < board thickness ≤ 28mm, a Y-type bevel is used, with a blunt edge of 4-6mm and a bevel angle of 65-70°; for board thickness > 28mm, an X-type bevel is used, with a blunt edge of 3-5mm and a bevel angle of 60-65°.

3. The manufacturing process of the austenitic stainless steel welded pipe for high-temperature molten salt transportation in solar thermal power generation according to claim 1, characterized in that, In the pipe welding process of step f, during plasma welding, the ion gas used is 93%Ar + 7%H2, with a gas flow rate of 3~8L / min; the shielding gas used is 99.99%Ar, with a gas flow rate of 10~25L / min; the tail shielding gas used is 99.99%Ar, with a gas flow rate of 15~22L / min; and the back shielding gas used is 99.99%Ar, with a gas flow rate of 20~30L / min. During argon arc welding, the shielding gas used is 93%Ar + 7%H2, with a gas flow rate of 10~25L / min; and the tail shielding gas used is 99.99%Ar, with a gas flow rate of 15~22L / min.

4. The austenitic stainless steel welded pipe for high-temperature molten salt transport in solar thermal power generation, manufactured according to any one of claims 1-3, is characterized in that... The base material of the welded pipe for high-temperature molten salt transportation in solar thermal power generation has a grain size of 4 to 7. The yield strength in the high-temperature tensile test at 575℃ is not less than 131 MPa. The tensile strength in the room temperature tensile test is ≥515 MPa, the yield strength is ≥205 MPa, the elongation after fracture is ≥40%, the bending test is qualified, and the hardness value is ≤92 HRB.

Citation Information

Patent Citations

  • Preparation process of stainless steel welded pipe for maritime work oil-gas transmission

    CN112077538A

  • Manufacturing method of austenitic stainless steel pipe for conveying LNG

    CN113510398A

  • Austenitic stainless steel welding method

    CN109175621A

  • Machining process of hydrogen-containing high-pressure large-diameter thick-wall stainless steel pipe fitting

    CN112281084A

  • Stainless steel welded pipe heat treatment equipment

    CN113337696A